NiCa-based bifunctional material, preparation method and application thereof, and integrated method for directly capturing carbon dioxide in air and preparing methane through in-situ conversion

The preparation of methane is achieved through the NiCa-based bifunctional material at room temperature with high efficiency of direct air carbon dioxide and in-situ conversion, which solves the problem of low capture efficiency for extremely low concentrations of CO2 in the prior art, and has low material cost and excellent cyclic stability and efficient conversion performance.

CN118949999AActive Publication Date: 2024-11-15SHANGHAI JIAOTONG UNIV

Patent Information

Application Number
CN202411009817.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing integrated technology for direct air carbon dioxide capture and in-situ conversion to prepare methane has low capture efficiency for extremely low concentrations of CO2 at room temperature, and is relatively expensive, making it difficult to achieve efficient CO2 conversion and methane production.

Method used

Using NiCa-based bifunctional materials, the chemical composition includes calcium hydroxide and nickel element. Through heat treatment, drying, calcining and reduction treatment in the preparation method, NiCa-based bifunctional materials with high CO2 adsorption and methane conversion are prepared, and Methane was prepared at room temperature by humid air trapping and conversion of hydrogen-containing atmosphere.

Benefits of technology

It has achieved efficient capture and efficient conversion of extremely low concentrations of CO2. The CO2 adsorption amount reaches 8.96mmol/g, the conversion rate is as high as 95.97%, the methane output is as high as 8.60mmol/g, and the material cost is low, the cycle stability is good, which is suitable for industrialization. Production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949999A_ABST
    Figure CN118949999A_ABST
Patent Text Reader

Abstract

The invention provides a NiCa-based bifunctional material, a preparation method and application thereof, and an integrated method for direct air carbon dioxide capture and in-situ conversion preparation of methane, and relates to the technical field of carbon capture. The invention provides a NiCa-based bifunctional material which comprises the following chemical components: calcium hydroxide and nickel elementary substance, and the mass content of the nickel elementary substance is 5-20%. According to the invention, calcium hydroxide is used as a CO2 adsorbent, nickel is used as a catalyst, and the adsorption capacity of CO2 with extremely low concentration is far greater than that of existing K-based and Na-based adsorbents. The NiCa-based bifunctional material provided by the invention has the adsorption capacity of up to 8.96 mmol / g for 400 ppm CO2 at room temperature, the yield of CH4 obtained by in-situ conversion is up to 8.60 mmol / g, the efficient capture of extremely low concentration CO2 can be realized, the yield and selectivity of CH4 obtained by in-situ conversion are high, and the performance of direct air carbon dioxide capture and in-situ conversion for methane preparation is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon capture, and in particular to a NiCa-based dual-functional material, a preparation method and application thereof, and an integrated method for direct air carbon dioxide capture and in-situ conversion to prepare methane. Background Art

[0002] Carbon capture is mainly divided into two pathways according to the source of carbon dioxide: carbon capture and storage (CCS) and direct air capture (DAC). The former is also known as "flue gas capture", which is to capture carbon from power plants and industrial waste gas, and the technology is more mature at present; the latter carbon dioxide comes from natural air and is a new generation of carbon capture technology. Traditional CCUS (Carbon Capture, Utilization and Storage) technology is divided into two stages: CO2 capture and storage or conversion utilization. In recent years, renewable electricity hydrogen production technology has developed rapidly, and the cost of hydrogen production has continued to decrease. If the energy required for CO2 desorption, purification, conversion and utilization is used, and the adsorbent is regenerated and CO2 is utilized through hydrogenation catalytic reaction without desorbing CO2, the integrated CO2 capture and conversion (ICCU) will be realized, which will have huge advantages in energy saving and consumption reduction.

[0003] At present, the research on ICCU technology is mainly aimed at the CO2 concentration of flue gas (volume concentration of about 10-20%). There are only 4 literature reports on the application of ICCU technology to DAC. The adsorption catalytic bifunctional materials used are all supported materials. The adsorption components such as potassium (K) and sodium (Na) and ruthenium (Ru) catalyst are loaded on an alumina (Al2O3) carrier. The material composition is 22.1% K2CO3 / Al2O3+4%Ru / Al2O3 (VESELOVSKAYA JV, PARUNIN PD, NETSKINA OV, et al. A Novel Process for Renewable Methane Production: Combining Direct Air Capture by K2CO3 / Alumina Sorbent with CO2Methanation over Ru / Alumina Catalyst [J]. Topics in Catalysis, 2018, 61 (15): 1528-36.), 5%Ru / 40%K2CO3 / K-β”-Al2O3 (LEE J, OTOMOJ. Low-Temperature Activated Direct Air Capture Methanation Using K-β”Alumina[J]. Industrial&Engineering Chemistry Research, 2023, 62(31):12096-108.), 0.5% Ru, 6.1% “Na2O” / Al2O3 (JEONG-POTTER C, FARRAUTO R. Feasibility Study of CombiningDirect Air Capture of CO2and Methanation at Isothermal Conditions with DualFunction Materials[J].Applied Catalysis B:Environmental,2021,282:119416.) and 1%Ru, 6.1% "Na2O" / Al2O3 (JEONG-POTTER C, ABDALLAH M, SANDERSON C, et al.Dualfunction materials (Ru+Na2O / Al2O3) for direct air capture of CO2 and in situ catalytic methanation: The impact of realistic ambient conditions [J]. Applied Catalysis B: Environment and Energy, 2022, 307: 120990.). The above materials can adsorb 400ppm CO2 up to 1.3mmol / g at room temperature, and the methane production can reach 1.04mmol / g, verifying the feasibility of direct air CO2 capture and in situ conversion to produce methane integrated (DAC-ICCU) technology. However, the above materials have low CO2 capture capacity at room temperature. Even if the CO2 conversion rate is high, the CH4 yield obtained by temperature conversion is still very low. .

[0004] Chinese patent CN117046437A discloses a dual-functional material for optical drive integrated CO2 capture and fuel production, the preparation agent includes calcium nitrate tetrahydrate, nickel nitrate hexahydrate, aluminum nitrate nonahydrate, chelating agent citric acid and solvent deionized water, which is used for calcium cycle coupling methane dry reforming reaction. The dual-functional material has low cost and small carbon deposition, can convert greenhouse gas into synthesis gas, achieve negative greenhouse gas emissions, and has high CO2 conversion rate, CH4 conversion rate, CO yield and H2 yield. The conversion reaction used in the above dual-functional material is methane dry reforming, the capture process is for high-concentration CO2 in flue gas (CO2 concentration is 20%), and the temperature of the capture process and the conversion reaction process is high (both are 720°C), while the dual-functional material is difficult to capture extremely low-concentration CO2 from air at room temperature, and the CO2 capture amount is low.

[0005] Chinese patent CN117839377A discloses an integrated capture and conversion system based on carbon dioxide adsorption and catalytic dual-functional materials. The adsorption and catalytic dual-functional materials are composed of three parts: adsorbent, catalyst and carrier. The adsorbent uses alkali metals, including one or more of K2CO3, Na2CO3, and MgO. The catalyst realizes the hydrogenation conversion process, including one or more of Ru, Ni, Co, and Pt. The carrier includes one or more of Al2O3, SiO2, and CeO2. The adsorbent and the catalyst are evenly dispersed on a carrier with a set specific surface area and pore structure to strengthen the contact and mass transfer process with the gas flow. However, the capture amount of CO2 by the above-mentioned adsorption and catalytic dual-functional materials is below 1mmol / g, and the capture amount of CO2 is low. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a NiCa-based bifunctional material and its preparation method and application, and an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane. The NiCa-based bifunctional material provided by the present invention is used in DAC-ICCU, which can achieve efficient capture of extremely low concentration CO2, high CO2 adsorption capacity, and high CH4 production.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The invention provides a NiCa-based dual-function material, the chemical composition of which comprises calcium hydroxide and nickel element; the mass content of the nickel element in the NiCa-based dual-function material is 5-20%.

[0009] Preferably, the NiCa-based bifunctional material further comprises a doped metal element, and the doped metal element comprises one or more of Mg, Ce and Zr;

[0010] The molar ratio of calcium to doped metal elements in the NiCa-based bifunctional material is 5 to 15:1.

[0011] The present invention provides a method for preparing the NiCa-based dual-functional material described in the above technical solution, comprising the following steps:

[0012] mixing a calcium precursor, a nickel precursor, citric acid and water to obtain a mixed solution;

[0013] heat-treating the mixed solution to obtain a sol;

[0014] The sol is dried and then calcined to obtain a NiCa-based calcined material;

[0015] The NiCa-based calcined material is subjected to reduction treatment to obtain the NiCa-based dual-functional material.

[0016] Preferably, when the NiCa-based bifunctional material further includes a doped metal oxide, the mixed solution further includes a doped metal precursor; the doped metal precursor includes one or more of a magnesium precursor, a cerium precursor and a zirconium precursor;

[0017] In the mixed solution, the molar ratio of metal ions to water is 1:30-80, and the molar ratio of metal ions to citric acid is 1:0.8-1.2.

[0018] Preferably, the heat treatment temperature is 80-90°C.

[0019] Preferably, the calcination temperature is 500-650° C., and the holding time is 3-5 hours.

[0020] Preferably, the temperature of the reduction treatment is 450-550° C., and the holding time is 0.5-2 h; the reducing agent used in the reduction treatment includes a hydrogen-containing atmosphere, and the volume fraction of hydrogen in the hydrogen-containing atmosphere is 10-100%.

[0021] The present invention also provides the use of the NiCa-based bifunctional material described in the above technical solution or the NiCa-based bifunctional material prepared by the preparation method described in the above technical solution in CO2 capture and / or CO2 conversion into methane.

[0022] The present invention also provides an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane, comprising the following steps:

[0023] Moist air is introduced into the NiCa-based bifunctional material for direct air CO2 capture, and then a hydrogen-containing atmosphere is introduced for in-situ methanation to obtain methane; the NiCa-based bifunctional material is the NiCa-based bifunctional material described in the above technical scheme or the NiCa-based bifunctional material obtained by the preparation method described in the above technical scheme.

[0024] Preferably, the temperature of the direct air CO2 capture is room temperature;

[0025] The volume fraction of hydrogen in the hydrogen-containing atmosphere is 10 to 100%;

[0026] The temperature of the in-situ methanation is 400-600°C.

[0027] The present invention provides a NiCa-based bifunctional material, the chemical composition of which includes calcium hydroxide and nickel; the mass content of nickel in the NiCa-based bifunctional material is 5-20%. The present invention uses Ca(OH)2 as an adsorbent for CO2 and Ni as a catalyst. The adsorption amount of extremely low concentration CO2 in humid air at room temperature is much greater than that of existing K-based and Na-based adsorbents, and the material has good cyclic stability and fast adsorption rate. As shown in the test results of the embodiment, the NiCa-based bifunctional material provided by the present invention can quickly adsorb extremely low concentration (400ppm) CO2 in humid air at room temperature, the adsorption amount of CO2 is as high as 8.96mmol / g, the CO2 conversion rate is as high as 95.97%, the yield of CH4 obtained by in-situ conversion is as high as 8.60mmol / g, the CH4 selectivity is as high as 100%, no CO is generated, and extremely low concentration CO2 can be efficiently captured. The yield of in-situ converted CH4 is high, the CH4 selectivity is high, and the performance of direct air carbon dioxide capture and in-situ conversion to prepare methane is excellent. Moreover, the present invention does not use precious metals, and the cost of the NiCa-based bifunctional material is low.

[0028] The present invention plays a role in inhibiting the agglomeration and deactivation of NiCa-based bifunctional materials by doping Mg, Ce and Zr elements as promoters, and further improves the recycling stability of NiCa-based bifunctional materials. As shown in the test results of the embodiment, the cycle performance of the bifunctional materials can be improved by doping MgO, CeO2 or ZrO2 in the NiCa bifunctional materials. Compared with the NiCa bifunctional materials, the CO2 adsorption capacity of the doped NiCa-based bifunctional materials is slightly reduced due to the reduction of the effective content of Ca, but the CO2 adsorption capacity of the three NiCa bifunctional materials (NiCaMg, NiCaCe, NiCaZr) is higher than 7.4mmol / g, and the CO2 conversion rate is higher than 95.4%, and the CH4 selectivity is maintained at 100%, so the bifunctional materials doped with metal oxides still have excellent performance. In five cycles, the CO2 adsorption amount decreased from 7.42mmol / g to 7.29mmol / g, and the CO2 conversion rate decreased from 97.11% to 94.39%. The performance attenuation was small, indicating that NiCaZr has significantly improved its cycle stability through ZrO2 doping.

[0029] The preparation method of the NiCa-based dual-functional material provided by the present invention has simple process, simple operation, wide source of raw materials, low cost, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of the device used for the integration of reduction treatment, direct air CO2 capture and in-situ conversion of methane;

[0031] Figure 2 XRD patterns of the NiCa-based calcined material (NiCaZr-calcined), the NiCa-based bifunctional material (NiCaZr-pretreated) and after CO2 adsorption (NiCaZr-CO2) prepared in Example 4;

[0032] Figure 3 These are the real-time variation curves of the gas component concentration and temperature at the reactor outlet during DAC (a~d) and in-situ methanation (e~h), where the black curve in a~d is the CO2 concentration at the reactor outlet, and the gray dotted line is the CO2 inlet concentration. DETAILED DESCRIPTION

[0033] The invention provides a NiCa-based dual-function material, the chemical composition of which comprises calcium hydroxide and nickel element; the mass content of the nickel element in the NiCa-based dual-function material is 5-20%.

[0034] In the present invention, the NiCa-based bifunctional material preferably further includes a doped metal element, and the doped metal element preferably includes one or more of Mg, Ce and Zr. When the doped metal element is a mixture of two or more, the present invention has no special restrictions on the usage ratio of different doped metal elements, and any ratio is acceptable. In the present invention, the doped metal element preferably exists in the form of a doped metal oxide. In the present invention, the doped metal element oxide preferably includes one or more of MgO, CeO2 and ZrO2.

[0035] In the present invention, the molar ratio of calcium to the doping metal element (denoted as M) in the NiCa-based bifunctional material is preferably 5 to 15:1, more preferably 6 to 12:1, and further preferably 8 to 10:1.

[0036] In the present invention, the mass content of nickel in the NiCa-based bifunctional material is preferably 5-20%, more preferably 8-12%, and further preferably 10%.

[0037] The present invention also provides a method for preparing the NiCa-based dual-functional material according to the above technical solution, comprising the following steps:

[0038] mixing a calcium precursor, a nickel precursor, citric acid and water to obtain a mixed solution;

[0039] heat-treating the mixed solution to obtain a sol;

[0040] The sol is dried and then calcined to obtain a NiCa-based calcined material;

[0041] The NiCa-based calcined material is subjected to reduction treatment to obtain the NiCa-based dual-functional material.

[0042] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0043] The invention mixes a calcium precursor, a nickel precursor, citric acid and water to obtain a mixed solution.

[0044] In the present invention, the calcium precursor preferably includes one or more of calcium nitrate, calcium oxalate and calcium acetate.

[0045] In the present invention, the nickel precursor preferably includes one or more of nickel nitrate and / or nickel acetate.

[0046] In the present invention, when the NiCa-based bifunctional material further includes a doped metal oxide, the mixed solution further includes a doped metal precursor, and the mixed solution is preferably obtained by mixing a calcium precursor, a nickel precursor, a doped metal precursor, citric acid and water. In the present invention, the doped metal precursor preferably includes one or more of a magnesium precursor, a cerium precursor and a zirconium precursor; the nickel precursor preferably includes one or more of magnesium nitrate, magnesium oxalate and magnesium acetate; the cerium precursor preferably includes cerium nitrate and / or cerium acetate; the zirconium precursor preferably includes one or more of zirconium nitrate, zirconium oxalate and zirconium acetate.

[0047] The present invention has no special limitation on the mixing, and the raw materials can be dissolved in water, such as stirring and mixing; the mixing temperature is preferably room temperature.

[0048] In the present invention, the molar ratio of metal ions to water in the mixed solution is preferably 1:30-80, more preferably 1:35-60, and further preferably 1:40-50; the molar ratio of metal ions to citric acid in the mixed solution is preferably 1:0.8-1.2, more preferably 1:0.9-1.1, and further preferably 1:1.

[0049] After obtaining the mixed solution, the present invention performs heat treatment on the mixed solution to obtain a sol.

[0050] In the present invention, the temperature of the heat treatment is preferably 80-90°C, more preferably 80-85°C; the heat treatment is preferably carried out under stirring conditions, and the present invention has no special limitation on the stirring time, as long as a transparent sol is obtained.

[0051] After obtaining the sol, the present invention calcines the sol after drying to obtain a NiCa-based calcined material.

[0052] In the present invention, the drying temperature is preferably 110-130° C., more preferably 120° C.; the drying time is preferably 8-16 h, more preferably 10-12 h; and the drying is preferably carried out in an oven.

[0053] In the present invention, the calcination temperature is preferably 500-650°C, more preferably 530-620°C, and further preferably 550-600°C; the calcination holding time is preferably 3-5h, more preferably 3.5-4.5h, and further preferably 4h; the heating rate from room temperature to the calcination temperature is preferably 2.5-10°C / min, more preferably 5-8°C / min.

[0054] After obtaining the NiCa-based calcined material, the present invention performs a reduction treatment on the NiCa-based calcined material to obtain the NiCa-based dual-functional material.

[0055] In the present invention, the temperature of the reduction treatment is preferably 450-550°C, more preferably 480-520°C, and further preferably 500°C; the holding time of the reduction treatment is preferably 0.5-2h, and more preferably 1-1.5h; the time for the temperature to rise from room temperature to the temperature of the pretreatment is preferably 25-45min, more preferably 30-40min, and further preferably 30-35min; the pressure of the reduction treatment is preferably normal pressure; the reducing agent used in the reduction treatment preferably includes a hydrogen-containing atmosphere; the hydrogen-containing atmosphere preferably includes hydrogen-nitrogen; the volume fraction of hydrogen in the hydrogen-containing atmosphere is preferably 10-100%, more preferably 30-80%, and further preferably 40-50%; the flow rate of the hydrogen-containing atmosphere is preferably 300-500mL / min, more preferably 350-450mL / min, and further preferably 400mL / min.

[0056] In the present invention, the pretreatment preferably includes: heating, introducing a hydrogen-containing atmosphere, and purging and activating. In the present invention, during the reduction treatment, NiO is reduced to Ni, and CaCO3 eventually generates Ca(OH)2.

[0057] After completing the pretreatment, the present invention preferably further comprises introducing nitrogen into the system obtained by the pretreatment to purge until no hydrogen is detected in the outflow gas flow, thereby obtaining the NiCa-based bifunctional material; the nitrogen introduction flow rate is preferably 300 to 500 mL / min, more preferably 350 to 450 mL / min, and further preferably 400 mL / min.

[0058] When the reducing agent is a hydrogen-containing atmosphere, after completing the pretreatment, the present invention preferably further comprises introducing nitrogen into the system obtained by the pretreatment to purge until no hydrogen is detected in the outflowing gas flow, thereby obtaining the NiCa-based bifunctional material; the nitrogen introduction flow rate is preferably 300 to 500 mL / min, more preferably 350 to 450 mL / min, and further preferably 400 mL / min.

[0059] The present invention also provides the use of the NiCa-based bifunctional material described in the above technical solution or the NiCa-based bifunctional material prepared by the preparation method described in the above technical solution in CO2 capture and / or CO2 conversion to methane. In the present invention, the concentration of CO2 in the CO2 capture and CO2 conversion to methane is independently preferably ≥400ppm.

[0060] The present invention also provides an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane, comprising the following steps:

[0061] Moist air is introduced into the NiCa-based bifunctional material for direct air CO2 capture, and then a hydrogen-containing atmosphere is introduced for in-situ methanation to obtain methane; the NiCa-based bifunctional material is the NiCa-based bifunctional material described in the above technical scheme or the NiCa-based bifunctional material obtained by the preparation method described in the above technical scheme.

[0062] In an embodiment of the present invention, the humid air is preferably simulated humid air, and the simulated humid air preferably includes CO2, O2, N2 and water; the concentration of CO2 in the simulated humid air is preferably 400ppm, and the volume fraction of oxygen is preferably 21%. In the present invention, the relative humidity of the air is preferably 30-90%, and specifically preferably 30%, 50%, 70% or 90%.

[0063] In the present invention, the temperature of the direct air CO2 capture is preferably room temperature (15-40°C); the air flow rate is preferably 300-500mL / min, more preferably 350-450mL / min, and further preferably 400mL / min; during the direct air CO2 capture process, Ca(OH)2 captures CO2 to generate CaCO3, and the air supply is stopped when the NiCa-based bifunctional material reaches adsorption saturation.

[0064] In the present invention, the temperature of the in-situ methanation is preferably 400-600°C, more preferably 450-550°C, and further preferably 450-500°C; the flow rate of the hydrogen-containing atmosphere is preferably 100-300mL / min, more preferably 150-250mL / min, and further preferably 200mL / min; the volume fraction of hydrogen in the hydrogen-containing atmosphere is preferably 10-100%, more preferably 30-80%, and further preferably 40-50%; the present invention has no special limitation on the time of the in-situ methanation, and the in-situ methanation is stopped when the CH4 concentration in the outflowing gas flow is lower than 0.01vol%; the pressure of the in-situ methanation is preferably normal pressure; in the in-situ methanation process, the adsorbed CO2 reacts with H2 under the action of the catalyst Ni to obtain the target product CH4, and the adsorbent is regenerated into Ca(OH)2.

[0065] In the present invention, the reduction treatment, direct air carbon dioxide capture and in-situ conversion of methane are preferably integrated in Figure 1 The device shown is carried out as follows Figure 1A detailed description is given. A NiCa-based calcined material is filled into a quartz tube reactor, both ends of the NiCa-based calcined material are fixed with quartz wool, and a thermocouple is inserted into the NiCa-based calcined material to measure the temperature; the quartz tube reactor is placed in a tube furnace, and a variable temperature mode is achieved by setting the temperature of the tube furnace (room temperature (15-40°C) in the direct air CO2 capture stage, and 400-600°C in the in-situ methane conversion stage); in the direct air CO2 capture process, the flow rates of two air streams are controlled to simulate the relative humidity level of the air (30%, 50%, 70% and 90%), one air stream passes through a scrubber bottle filled with water, and the other does not pass through the scrubber bottle; two non-dispersive infrared analyzers are used to monitor the gas composition in real time; one is used to monitor the extremely low CO2 concentration in the DAC step, and the other is used to monitor the concentrations of CO2, CH4 and CO in the in-situ methanation.

[0066] In the present invention, the integrated method of direct air carbon dioxide capture and in-situ conversion to prepare methane includes two main stages: direct air CO2 capture and in-situ methanation. The specific experimental operation process includes: introducing simulated air at room temperature and setting relative humidity to simulate the air in a real environment. In this process, Ca(OH)2 captures CO2 to generate CaCO3, and ventilation is stopped after the NiCa-based bifunctional material reaches adsorption saturation; pure N2 is introduced for purging; the reactor is heated and a second hydrogen-containing atmosphere is introduced. In this process, the adsorbed CO2 reacts with H2 under the action of the catalyst Ni to obtain the target product CH4, and the adsorbent is regenerated into Ca(OH)2, and ventilation is continued until the CH4 concentration in the reactor outlet gas flow is lower than 0.01wt%; pure N2 is introduced for purging until no H2 is detected in the outlet gas flow; the above operations are all performed under normal pressure.

[0067] In order to further illustrate the present invention, a NiCa-based bifunctional material provided by the present invention, a preparation method and application thereof, and an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0068] Example 1

[0069] Preparation by sol-gel method: add calcium nitrate and citric acid to deionized water, stir at room temperature until completely dissolved and evenly dispersed to obtain a mixed solution, continue stirring at 80°C to generate a transparent sol, place it in a 120°C oven for drying for 12 hours to obtain an expanded solid; place the expanded solid in a muffle furnace, heat it to 550°C at a heating rate of 5°C / min, and then calcine it for 4 hours to obtain a NiCa-based calcined material (abbreviated as NiCa-calcined). Among them, Ni mass / (Ni mass+Ca(OH)2 mass)×100%=10%, the total amount of deionized water and metal ions (Ca2+ +Ni 2+ )=40:1, and the molar ratio of citric acid to the total amount of metal ions=1:1.

[0070] Example 2

[0071] Prepared by sol-gel method: add calcium nitrate, magnesium nitrate and citric acid to deionized water, stir at room temperature until all dissolved and evenly dispersed to obtain a mixed solution, continue stirring at 80°C to generate a transparent sol, place it in a 120°C oven for drying for 12 hours to obtain an expanded solid; place the expanded solid in a muffle furnace, heat it to 550°C at a heating rate of 5°C / min, and then calcine it for 4 hours to obtain a NiCa-based calcined material (abbreviated as NiCaMg-calcined). Among them, Ni mass / (Ni mass+Ca(OH)2 mass+MgO mass)×100%=10%, H2O in the mixed solution: (Ca 2+ +Ni 2+ +Mg 2+ ) molar ratio = 40:1, the molar ratio of citric acid to the total amount of metal ions = 1:1.

[0072] Example 3

[0073] Prepared by sol-gel method: add calcium nitrate, cerium nitrate and citric acid to deionized water, stir at room temperature until completely dissolved and evenly dispersed to obtain a mixed solution, continue stirring at 80°C to generate a transparent sol, place it in a 120°C oven for drying for 12 hours to obtain an expanded solid; place the expanded solid in a muffle furnace, heat it to 550°C at a heating rate of 5°C / min, and then calcine it for 4 hours to obtain a NiCa-based calcined material (abbreviated as NiCaCe-calcined). Among them, Ni mass / (Ni mass+Ca(OH)2 mass+CeO2 mass)×100%=10%, H2O in the mixed solution: (Ca 2+ +Ni 2+ +Ce 4+ ) molar ratio = 40:1, the molar ratio of citric acid to the total amount of metal ions = 1:1.

[0074] Example 4

[0075] Prepared by sol-gel method: add calcium nitrate, zirconium nitrate and citric acid to deionized water, stir at room temperature until all dissolved and evenly dispersed to obtain a mixed solution, continue stirring at 80°C to generate a transparent sol, place it in a 120°C oven for drying for 12 hours to obtain an expanded solid; place the expanded solid in a muffle furnace, heat it to 550°C at a heating rate of 5°C / min, and then calcine it for 4 hours to obtain a NiCa-based calcined material (abbreviated as NiCaZr-calcined). Among them, Ni mass / (Ni mass+Ca(OH)2 mass+ZrO2 mass)×100%=10%, H2O in the mixed solution:(Ca 2+ +Ni 2+ +Zr 4+ ) molar ratio = 40:1, the molar ratio of citric acid to the total amount of metal ions = 1:1.

[0076] Example 5

[0077] use Figure 1 The device is to carry out reduction treatment, direct air CO2 capture and in-situ methane conversion integration on the NiCa-based calcined materials prepared in Examples 1 to 4, respectively; fill the NiCa-based calcined materials into a quartz tube reactor, fix both ends of the material with quartz wool, and insert a thermocouple into the material to measure the temperature; place the quartz tube reactor in a tubular furnace, and realize a variable temperature mode by setting the temperature of the tubular furnace (25°C in the direct air CO2 capture stage and 450°C in the in-situ methane conversion stage); in the direct air CO2 capture process, the relative humidity level of the air (dry, 30%, 50%, 70% and 90%) is simulated by controlling the flow rate of two simulated air streams, one of which passes through a scrubber bottle and the other does not pass through the scrubber bottle; use two non-dispersive infrared analyzers to monitor the gas composition in real time; one is used to monitor the extremely low CO2 concentration in the DAC step, and the other is used to monitor the concentrations of CO2, CH4 and CO in the in-situ methanation. Simulated air composition: 400ppmCO2+21vol%O2+N2.

[0078] The specific experimental operation process includes:

[0079] Step 1) Reduction treatment: heating to 500° C. for 30 min, introducing 40 vol% H2-N2 at a flow rate of 400 mL / min, purging and activating for 1 h, to obtain the NiCa-based bifunctional material; the NiCa-based bifunctional materials obtained by reduction treatment of the NiCa-based calcined materials prepared in Examples 1 to 4 are sequentially recorded as NiCa, NiCaMg, NiCaCe and NiCaZr;

[0080] Step 2) pure N2 was introduced at a flow rate of 400 mL / min until no H2 was detected in the outflow gas flow;

[0081] Step 3) DAC: introducing simulated air at room temperature, setting the relative humidity (90%), and stopping ventilation after the NiCa-based bifunctional material reaches adsorption saturation;

[0082] Step 4) introducing pure N2 at a flow rate of 400 mL / min for purging;

[0083] Step 5) In-situ methanation: The reactor is heated to 450°C, 40 vol% H2-N2 is introduced at a flow rate of 200 mL / min, and the adsorbed CO2 reacts with H2 under the action of catalyst Ni to obtain the target product CH4, and the adsorbent is regenerated into Ca(OH)2. Aeration is continued until the CH4 concentration in the reactor outlet gas flow is less than 0.01 wt%.

[0084] Step 6) Purging with pure N2 at a flow rate of 400 mL / min until no H2 is detected in the outflowing gas stream;

[0085] Step 7) Repeat steps 1) to 6) to carry out a cycle performance test, wherein steps 1) to 6) are all carried out under normal pressure.

[0086] The NiCa-based bifunctional materials obtained by reduction treatment of the NiCa-based calcined materials prepared in Examples 1 to 4 are respectively denoted as NiCa, NiCaMg, NiCaCe and NiCaZr.

[0087] Figure 2 From the XRD patterns of the NiCa-based calcined material (NiCaZr-calcined), NiCa-based bifunctional material (NiCaZr-pretreated) and after CO2 adsorption (NiCaZr-CO2) prepared in Example 4, it can be seen that the main components of the calcined NiCaZr are CaCO3, NiO and ZrO2. Since the content of NiO and ZrO2 is small and uniformly dispersed, no characteristic peaks are shown in the XRD results; the pretreatment step enables NiCaZr to have active ingredients for realizing air carbon capture and methanation functions - Ca(OH)2 and Ni, and the Zr species still exists in the form of oxide ZrO2; in the DAC process, Ca(OH)2 adsorbs CO2 in the air and is converted into CaCO3.

[0088] Figure 3 The real-time curves of the concentration and temperature of the gas components at the reactor outlet during DAC (a-d) and in-situ methanation (e-h) are shown in Table 1. The black curve in a-d is the CO2 concentration at the reactor outlet, and the gray dashed line is the CO2 inlet concentration. The CO2 adsorption capacity and conversion rate, CH4 production and selectivity of the NiCa-based bifunctional material were calculated by the inlet and outlet concentrations. Among them, the CO2 inlet concentration was obtained by the blank experiment (i.e., no material was added to the quartz tube reactor).

[0089] Table 1 Catalytic performance parameters of NiCa-based bifunctional materials used for the first time

[0090]

[0091]

[0092] NiCa showed excellent performance, with a CO2 adsorption of 8.96 mmol / g and a CH4 production of 8.60 mmol / g, no CO2 release during the temperature rise stage, and CH4 as the only conversion product without CO production. However, due to the sintering and agglomeration of the material, the CO2 adsorption of NiCa dropped sharply to 46% of the first cycle after five DAC and in situ methanation cycles.

[0093] The cyclic performance of the NiCa bifunctional material can be improved by doping MgO, CeO2 or ZrO2 in the bifunctional material. Compared with the NiCa bifunctional material, the CO2 adsorption capacity of the doped NiCa-based bifunctional material decreases slightly due to the decrease in the effective content of Ca, but the CO2 adsorption capacity of the three NiCa bifunctional materials (NiCaMg, NiCaCe, NiCaZr) is higher than 7.4mmol / g, and the CO2 conversion rate is higher than 95.4%, and the CH4 selectivity remains at 100%. Therefore, the bifunctional material doped with metal oxides still has excellent performance. In five cycles, the CO2 adsorption capacity decreased from 7.42mmol / g to 7.29mmol / g, and the CO2 conversion rate decreased from 97.11% to 94.39%, and the performance attenuation was small, indicating that NiCaZr has a significant improvement in cyclic stability through the doping of ZrO2.

[0094] During the methanation process, as the temperature rises, CH4 is gradually produced, and there is no CO2 release and CO generation, indicating that the NiCa-based bifunctional material provided by the present invention has high CO2 conversion rate and CH4 selectivity and has excellent catalytic conversion performance.

[0095] Comparative Example 1

[0096] The supported bifunctional material was synthesized by an impregnation method, with Al2O3 as a carrier, Ru as a catalyst, and Na2CO3 as an adsorbent. The catalyst content in the supported bifunctional material was 1wt%, and the adsorbent content was 20wt%.

[0097] The adsorbent metal precursor (Na2CO3) and Al2O3 were added to deionized water, and the obtained adsorbent metal precursor mixed solution was stirred at room temperature for 12 hours, heated to 80°C and continued to stir until the water volatilized naturally, and placed in a 120°C oven for drying for 12 hours to obtain a dry solid, which was placed in a muffle furnace and heated to 400°C at a heating rate of 5°C / min for the first calcination for 4 hours to obtain an adsorbent-carrier material. Among them, the Na2CO3 concentration in the adsorbent metal precursor mixed solution was 47.2mmol / L, and the Al2O3 concentration was 193.7mmol / L.

[0098] The catalyst metal precursor (RuCl3·H2O) was added to deionized water to obtain a catalyst precursor solution, which was stirred at room temperature for 12 hours, heated to 80°C and continued to be stirred until the water evaporated naturally, and placed in a 120°C oven for drying for 12 hours to obtain a dry solid. After grinding, the solid was placed in a muffle furnace and heated to 300°C at a heating rate of 5°C / min for a second calcination for 4 hours to obtain a supported bifunctional material (denoted as Ru / Na / Al2O3). The concentration of RuCl3·H2O in the catalyst metal precursor salt mixture was 2.9mmol / L.

[0099] Comparative Example 2

[0100] The supported bifunctional material was prepared according to the method of Example 1, which differed from Comparative Example 1 only in that the adsorbent metal precursor was K2CO3, and a supported bifunctional material (denoted as Ru / K / Al2O3) was obtained.

[0101] Comparative Example 3

[0102] A supported bifunctional material was prepared according to the method of Example 1, which differed from Comparative Example 1 only in that the adsorbent metal precursor was MgO, the first calcination temperature was 550° C., and a supported bifunctional material (denoted as Ru / Mg / Al2O3) was obtained.

[0103] Comparative Example 4

[0104] A supported bifunctional material was prepared according to the method of Example 1, the only difference from Comparative Example 1 being that the catalyst content in the supported bifunctional material was 10 wt%, the adsorbent metal precursor was CaO, the catalyst metal precursor was Ni(NO3)2·6H2O, the first calcination temperature was 550°C, and the second calcination temperature was 550°C, to obtain a supported bifunctional material (denoted as Ni / Ca / Al2O3).

[0105] Comparative Example 5

[0106] The catalytic performance of the supported bifunctional materials prepared in Comparative Examples 1 to 4 for direct air carbon dioxide capture and in-situ conversion of methane was tested according to the method of Example 5. The in-situ methanation temperature and performance parameters of the supported bifunctional materials are shown in Table 2.

[0107] Table 2 Catalytic performance parameters of supported bifunctional materials for the first use

[0108]

[0109] It can be seen from Table 2 that compared with the supported bifunctional materials prepared in Comparative Examples 1 to 4, the NiCa-based bifunctional materials prepared in the present invention are used for integrated direct air carbon dioxide capture and in-situ methane conversion, and the CO2 adsorption capacity, CO2 conversion rate and CH4 production are significantly improved, and the catalytic performance is excellent.

[0110] Comparative Example 6

[0111] The material composition of the materials of DAC-ICCU technology reported in existing literature and the reaction conditions and catalytic performance parameters of DAC-ICCU technology are shown in Table 3.

[0112] Literature [1]: VESELOVSKAYA JV, PARUNIN PD, NETSKINA OV, et al. ANovelProcess for Renewable Methane Production: Combining DirectAir Capture by K2CO3 / Alumina Sorbent with CO2Methanation over Ru / Alumina Catalyst[J]. Topics inCatalysis, 2018, 61(15):1528-36.

[0113] Literature [2]: LEE J, OTOMO J. Low-Temperature Activated Direct Air CaptureMethanation Using K-β” Alumina[J]. Industrial&Engineering Chemistry Research, 2023, 62(31):12096-108.

[0114] Literature[3]: JEONG-POTTER C, FARRAUTO R.Feasibility Study ofCombiningDirect Air Capture of CO2and Methanation at Isothermal Conditions with DualFunction Materials[J].Applied Catalysis B:Environmental,2021,282:119416.

[0115] Literature [4]: ​​JEONG-POTTER C, ABDALLAH M, SANDERSON C, et al. Dual functionmaterials (Ru+Na2O / Al2O3) for direct air capture ofCO2and in situ catalyticmethanation: The impact of realistic ambient conditions [J]. Applied CatalysisB: Environment and Energy, 2022, 307: 120990.

[0116] Table 3 Composition of K-based and Na-based adsorption materials and reaction conditions and catalytic performance parameters of DAC-ICCU technology

[0117]

[0118] As shown in Table 3, compared with the existing materials, the NiCa-based bifunctional material prepared by the present invention is used for direct air carbon dioxide capture and in-situ conversion of methane integration, and the CO2 adsorption and CH4 production are significantly improved, and the performance is excellent. Moreover, the present invention does not use precious metals, and the cost of the NiCa-based bifunctional material is low.

[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A NiCa-based bifunctional material, the chemical composition of which includes calcium hydroxide and nickel; the mass content of nickel in the NiCa-based bifunctional material is 5-20%.

2. The NiCa-based dual-functional material according to claim 1, characterized in that: The NiCa-based bifunctional material further includes a doped metal element, wherein the doped metal element includes one or more of Mg, Ce and Zr; The molar ratio of calcium to doped metal elements in the NiCa-based bifunctional material is 5 to 15:

1.

3. The method for preparing the NiCa-based dual-functional material according to claim 1 or 2, comprising the following steps: mixing a calcium precursor, a nickel precursor, citric acid and water to obtain a mixed solution; heat-treating the mixed solution to obtain a sol; The sol is dried and then calcined to obtain a NiCa-based calcined material; The NiCa-based calcined material is subjected to reduction treatment to obtain the NiCa-based dual-functional material.

4. The preparation method according to claim 3, characterized in that: When the NiCa-based bifunctional material further includes a doped metal oxide, the mixed solution further includes a doped metal precursor; the doped metal precursor includes one or more of a magnesium precursor, a cerium precursor and a zirconium precursor; In the mixed solution, the molar ratio of metal ions to water is 1:30-80, and the molar ratio of metal ions to citric acid is 1:0.8-1.

2.

5. The preparation method according to claim 3 or 4, characterized in that: The temperature of the heat treatment is 80-90°C.

6. The preparation method according to claim 3 or 4, characterized in that: The calcination temperature is 500-650° C., and the heat preservation time is 3-5 hours.

7. The preparation method according to claim 3, characterized in that: The temperature of the reduction treatment is 450-550° C., and the holding time is 0.5-2 hours. The reducing agent used in the reduction treatment includes a hydrogen-containing atmosphere, and the volume fraction of hydrogen in the hydrogen-containing atmosphere is 10-100%.

8. Use of the NiCa-based bifunctional material according to any one of claims 1 to 2 or the NiCa-based bifunctional material prepared by the preparation method according to any one of claims 3 to 7 in CO2 capture and / or CO2 conversion into methane.

9. An integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane, comprising the following steps: Moist air is introduced into the NiCa-based bifunctional material for direct air CO2 capture, and then a hydrogen-containing atmosphere is introduced for in-situ methanation to obtain methane; the NiCa-based bifunctional material is the NiCa-based bifunctional material according to any one of claims 1 to 2 or the NiCa-based bifunctional material obtained by the preparation method according to any one of claims 3 to 7.

10. The integrated method according to claim 9, characterized in that: The temperature of the direct air CO2 capture is room temperature; The volume fraction of hydrogen in the hydrogen-containing atmosphere is 10 to 100%; The temperature of the in-situ methanation is 400-600°C.

Citation Information

Patent Citations

  • Catalyst for preparing high-purity hydrogen by biomass low-temperature gasification and preparation method thereof

    CN108212165A

  • Methods for producing alkaline earth carbonates

    JP2020033263A

  • Exhaust gas purifying catalyst

    WO2012093599A1

Cited By

  • Carbon dioxide trapping in-situ conversion system

    CN119680377A

  • Difunctional composite material as well as preparation method and application thereof

    CN120437945A