Mineral processing technology of multi-metal magnetite

By premagnetic separation and mixed flotation after separation of grinding, the problems of low grade efficiency and over-grinding of multimetal magnetite grinding are solved, efficient copper recovery and magnetite grading are achieved, and the overall ore dressing process is improved. Stability and metal recovery.

CN118950238APending Publication Date: 2024-11-15UNIV OF SCI & TECH BEIJING
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411153461.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the grinding grading process of polymetal magnetite, the grading efficiency and serious over-grinding phenomenon are low, resulting in low magnetite grading efficiency, affecting the stability of the subsequent process and metal recovery rate.

Method used

The combination of premagnetic separation-separated grinding-mixed flotation technology is adopted to obtain non-magnetic and magnetic products for grinding separately through premagnetic separation, and mixed flotation is carried out under the optimal process conditions, using butyl yellow medicine and 2# Oil acts as a collector to optimize the separation process between magnetite and copper ore.

Benefits of technology

Improve the grinding efficiency of magnetite and copper ore, reduce the over-grinding of non-magnetic minerals, solve the 'density effect' problem in magnetite grading, improve the copper recovery rate to 89.54%, and enhance copper and iron The separation and enrichment effect of minerals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950238A_ABST
    Figure CN118950238A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-metal magnetite beneficiation process which comprises the following steps: (1) pre-magnetic separation: screening and crushing ores, adding the ores into a magnetic separator, and carrying out pre-magnetic separation under the excitation current of 0.2-0.3 A to obtain a non-magnetic product and a magnetic product; (2) separate ore grinding is conducted, specifically, the non-magnetic product and the magnetic product are subjected to ore grinding respectively till the content of the non-magnetic product and the magnetic product with the fineness of 200 meshes is 60%-80%, and a non-magnetic ore grinding product and a magnetic ore grinding product are obtained; and (3) bulk flotation is conducted, specifically, the magnetic ore grinding product and the non-magnetic ore grinding product are mixed according to the mass ratio of (2.5-3.5): 1, flotation and magnetic separation are conducted, and copper concentrate and iron concentrate are obtained. Aiming at a certain multi-metal magnetite in Anhui Province, the invention provides a pre-magnetic separation-separated ore grinding-bulk flotation combined process, so that rough concentrate with the copper recovery rate of 89.54% can be obtained, and the problem of'density effect 'of magnetite classification can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a beneficiation process of polymetallic magnetite, belonging to the technical field of mineral beneficiation. Background Art

[0002] China is rich in iron ore resources, but rich iron ore resources are relatively rare, and most of them exist in the form of complex polymetallic ores, accompanied by a variety of valuable metal elements such as copper, cobalt, zinc, gold and silver. Moreover, the main recovery target minerals are usually fine-grained impregnation-type embedded, and there are many types of ores, which makes sorting more difficult. In recent years, during the deep mining process of a polymetallic iron ore resource in Anhui, the properties of the ore have changed significantly, and the content of magnetic minerals has increased. The ore is mainly composed of magnetite, and useful minerals also include chalcopyrite, pyrite, a small amount of cobalt minerals and precious metal minerals. The gangue minerals are mostly pyroxene, dolomite and olivine. For this type of ore, the existing technology usually uses a combined process of magnetic separation, flotation and gravity separation for treatment.

[0003] Grinding reduces the particle size of ore and is the basis for the separation of different minerals. The selection of grinding methods is inseparable from detailed and rich mineralogical properties. The mature development of process mineralogy parameter analysis equipment such as scanning electron microscope-energy spectrum (SEM-EDS) and process mineral parameter automatic analysis system (MLA) has greatly facilitated the determination of process parameters, including the selection of grinding parameters, and provided reliable theoretical support for the formulation of mineral processing procedures in beneficiation plants. For example, Patra and other researchers observed the embedded particle size of iron ore through a microscope and found that within the particle size range of -150+75μm, the dissociation degree was 84.59%, so -150μm was used as the ultimate goal of grinding. However, different types of minerals will show different grinding behaviors due to differences in content and physical properties such as hardness and brittleness. Krolop studied the performance of different types of iron oxide ore types in grinding and concluded that the degree of dissociation of ore mainly composed of magnetite is greatly affected by silicate minerals during grinding, and the difference in the dissociation degree of iron oxide minerals depends on the embedded particle size of the mineral rather than the content of gangue minerals.

[0004] In the process of classifying grinding products of qualified particle size, hydrocyclones are usually used as classification equipment. According to the differences in the size, shape and density of ore particles, the coarse particles with large centrifugal force move toward the wall in the centrifugal field of the high-speed spiral, while the fine particles are dominated by resistance and enter the inner vortex. The fine particles with high density will also move downward along the wall of the cyclone, and return to the mill to continue grinding with the coarse particles with unqualified particle size in the closed-circuit grinding process, forming the "density effect" of the grinding and classification process. The result is low classification efficiency of the hydrocyclone and serious over-grinding. Therefore, it is necessary to optimize the traditional grinding and classification process to adapt to the changes in ore properties (the "density effect" aggravated by the increase in magnetite content). The goal of optimization is to reduce the continued grinding of fine particles under the condition of meeting the dissociation degree of the target mineral and ensure the smooth progress of the subsequent process.

[0005] At present, a lot of research has been done on the optimization of iron ore beneficiation process, but it mainly focuses on the selection of grinding, grading and beneficiation equipment and the modification of hydrocyclone structure. However, there are few reports on the research on improving the process flow for the root cause of the change in ore properties. For example, in order to solve the problem of poor magnetite conjoined bodies mixed into magnetic products or the inability to enrich the fine magnetite particles that have achieved monomer dissociation due to insufficient magnetite dissociation in the grinding process, Guo et al. developed a three-product magnetic separator with centrifugal force, mechanical dispersion force and fluid resistance for the pre-separation of free magnetite and pre-discarding of tailings. Frausto uses a fine screen instead of a hydrocyclone to ensure that the grinding product is graded according to particle shape and size, thereby separating the ideal target size and minimizing the "density effect" of qualified particle sizes in the grading stage. Although the improvement of equipment will have an immediate relief effect, it fails to solve the problem of mixing different minerals in the grinding and grading process. In addition, some studies have shown that through pre-selection, a part of the target minerals can be preferentially enriched in low-grade ores and most of the gangue minerals can be discarded. This approach not only reduces the processing volume of selected ore and reduces the processing cost of ore, but also improves the quality of the product. Summary of the invention

[0006] In view of the above-mentioned prior art, the present invention provides a beneficiation process for polymetallic magnetite: a combined process of pre-magnetic separation-separate grinding-mixed flotation.

[0007] The present invention is achieved through the following technical solutions:

[0008] A multi-metal magnetite beneficiation process comprises the following steps:

[0009] (1) Pre-magnetic separation: Screen and crush the ore, add appropriate amount of water to stir into slurry, add it to the magnetic separator, adjust the excitation current to 0.2A-0.3A (preferably 0.25A), perform pre-magnetic separation until non-magnetic minerals are produced, and obtain non-magnetic products and magnetic products;

[0010] (2) Grinding separately: The non-magnetic product and the magnetic product obtained above are added to a ball mill respectively, and a proper amount of water and lime are added to grind the ore until the fineness of -200 mesh content is 60% to 80% (preferably 65%), thereby obtaining a non-magnetic grinding product and a magnetic grinding product respectively;

[0011] (3) Mixed flotation: The magnetic grinding product and the non-magnetic grinding product obtained above are mixed in a mass ratio of (2.5-3.5):1 (preferably 3:1), and conventional flotation and magnetic separation are performed to obtain copper concentrate and iron concentrate.

[0012] Furthermore, the TFe grade in the raw ore of the polymetallic magnetite is relatively high, reaching 50.28%, and the contents of other valuable metals such as copper and cobalt are 0.54% and 0.0213% respectively, in addition to 0.0418% titanium; the metal minerals in the ore are mainly magnetite, with a content of 79.94%. The metal sulfides are mainly chalcopyrite and pyrite, of which the content of chalcopyrite is 0.68% and the content of pyrite is 1.80%.

[0013] Furthermore, in the step (2), a hydrocyclone is used to classify the product after grinding, and coarse particles with unqualified particle sizes are returned to the ball mill for further grinding in the closed-circuit grinding process.

[0014] Furthermore, in the step (2), the lime is added in an amount of 2-8 kg / t, preferably 4 kg / t.

[0015] Furthermore, in the step (3), flotation includes roughing and scavenging, and butyl xanthate and 2# oil are added in the order of collector first and frother in roughing and scavenging to obtain rough concentrate, middlings and tailings. Furthermore, in roughing, the addition ratio of butyl xanthate is 40-80 g / t, preferably 60 g / t, and the addition ratio of 2# oil is 10-30 g / t, preferably 20 g / t; in scavenging, the addition ratio of butyl xanthate is 20-60 g / t, preferably 40 g / t, and the addition ratio of 2# oil is 5-15 g / t, preferably 10 g / t.

[0016] The present invention aims at the problems of low classification efficiency, serious over-grinding and reduced metal recovery rate in the grinding and classification process of a polymetallic magnetite in Anhui Province. Starting from the mineralogical properties of the selected ore, the present invention uses an X-ray diffractometer (XRD), a scanning electron microscope energy spectrum (SEM-EDS) and an automatic analysis system for process mineral parameters to study the mineral composition, intercalation relationship, intercalation particle size and dissociation degree of the ore, especially the intercalation relationship of magnetite, chalcopyrite, cobalt minerals and precious metal minerals to reveal the reasons for such changes. Subsequently, a single factor experiment is conducted to study the influence of magnetic field intensity and grinding process parameters on the enrichment of magnetite and chalcopyrite. On this basis, the present invention proposes a combined process of pre-magnetic separation-separate grinding-mixed flotation, which reduces the over-grinding of non-magnetic minerals while improving the grinding efficiency of magnetite and copper ore through more targeted grinding means. Under the optimal process conditions (excitation current 0.25A, grinding fineness -200 mesh content of 65%, butyl xanthate as collector for mixed roughing), a coarse concentrate with a copper recovery rate of 89.54% can be obtained, and the problem of "density effect" in magnetite classification can be solved (the present invention adopts a separate grinding method to separate the two mineral particles with large density differences for grinding and classification, and uses an independent hydrocyclone to classify the two products, thereby avoiding the mixing of fine particles with high density and coarse particles with low density). The research results of the present invention have certain guiding significance for the separation of high-grade polymetallic iron ore, solving the "density effect" of grinding and classification, and strengthening the separation and enrichment of copper and iron minerals.

[0017] Various terms and phrases used herein have the general meanings that are well known to those skilled in the art. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 : Experimental flow chart of pre-magnetic separation, grinding and screening, where A: direct grinding of raw ore; B: grinding and screening of non-magnetic products after pre-magnetic separation of raw ore; C: grinding and screening of magnetic products after pre-magnetic separation of raw ore.

[0019] Figure 2 : Experimental flow chart of flotation.

[0020] Figure 3 : Schematic diagram of XRD results of the original ore.

[0021] Figure 4 : Schematic diagram of BPMA results of the original ore.

[0022] Figure 5 : BSE mineral coloring images of the original ore BPMA analysis, where (a), (b), (d), and (e) are the mineral coloring images of the original ore BSE images; (c) is the pyrite particle sorting; (f) is the chalcopyrite particle sorting.

[0023] Figure 6: Schematic diagram of the cumulative particle size distribution curves of magnetite, pyrite and chalcopyrite in the original ore.

[0024] Figure 7 :The intercalation relationship between the main metal sulfide ores and other minerals, among which, (a) chalcopyrite and olivine are interrelated; (b) chalcopyrite and pyrite are interrelated; (c) pyrite and calcite are interrelated; (d) pyrite and magnetite are interrelated; (e) pyrite and ankerite and pyrite are interrelated; (f) native gold and pyrite are interrelated. Ccp: chalcopyrite; Ol: olivine; Py: pyrite; Crl: pyrite; Cal: calcite; Mag: magnetite; Sig: pyrite; Ank: ankerite; Ng: native gold.

[0025] Figure 8 : Schematic diagram of the monomer dissociation degree and intergrowth of magnetite, pyrite and chalcopyrite in the original ore.

[0026] Fig. 9 : Schematic diagram of the relationship between the excitation current and magnetic product indicators.

[0027] Fig.10 : The relationship between the grinding yield of ore, magnetic product and non-magnetic product-200 mesh and grinding time.

[0028] Fig.11 :Experimental process flow chart of grinding-flotation.

[0029] Fig.12 : Schematic diagram of product indicators of grinding-flotation.

[0030] Fig.13 :Experimental process flow chart of pre-magnetization - grinding - separate flotation.

[0031] Fig.14 : Schematic diagram of the flotation results of non-magnetic products from pre-magnetization - grinding - separate flotation.

[0032] Fig.15 : Schematic diagram of the flotation results of magnetic products of pre-magnetization - grinding - separate flotation.

[0033] Fig.16 : Distribution diagram of the degree of dissociation of chalcopyrite in flotation tailings with a fineness of 75% non-magnetic product.

[0034] Fig.17 : Particle ordering diagram of chalcopyrite and pyrite in the flotation tailings of non-magnetic products with a fineness of 75%, wherein (a) is the particle ordering diagram of chalcopyrite; (b) is the particle ordering diagram of pyrite.

[0035] Fig.18 : Schematic diagram of XRD phase analysis results.

[0036] Fig.19 :Experimental process flow chart of pre-magnetic separation - grinding - mixed flotation.

[0037] Fig. 20 : Schematic diagram of the experimental results of pre-magnetic separation - grinding - mixed flotation.

[0038] Fig.21 : Process flow chart of three mineral processing schemes, among which, (a) Scheme I: grinding-flotation; (b) Scheme II: pre-magnetic separation-grinding-separate flotation; (c) Scheme III: pre-magnetic separation-grinding-mixed flotation. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with the embodiments. However, the scope of the present invention is not limited to the following embodiments. It will be appreciated by those skilled in the art that various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention.

[0040] The instruments, reagents, and materials involved in the following examples, unless otherwise specified, are all conventional instruments, reagents, and materials available in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following examples, unless otherwise specified, are all conventional experimental methods and detection methods available in the prior art.

[0041] Study on the beneficiation technology of experimental polymetallic magnetite

[0042] 1. Materials and Methods

[0043] 1.1 Experimental samples and preparation

[0044] The research object is the polymetallic magnetite in the deep mining area of ​​Anhui Taiping Mining. The ore is used as the experimental sample after screening, crushing and mixing. The reagents used in the experiment include butyl xanthate (industrial grade), 2# oil (industrial grade), and lime (CaO, industrial grade). The experimental samples and reagents were provided by Anhui Taiping Mining Co., Ltd.

[0045] 1.2 Experimental section

[0046] 1.2.1 Pre-magnetic separation

[0047] In the pre-magnetic separation experiment, 500g of sample was taken each time, and before the experiment, an appropriate amount of water was added to stir it into a uniform slurry, and then added to the magnetic separator ( 400×300 weak magnetic separator, Wuhan Rock Powder Equipment Manufacturing Co., Ltd.), adjust the magnetic separator excitation current to 0.1A, 0.2A, 0.3A, 0.4A and 0.5A for experiments respectively, and the magnetic separation is considered to be completed when no magnetic minerals are produced in the magnetic product tank. Figure 1 shown.

[0048] 1.2.2 Grinding and Screening

[0049] In each grinding experiment, 500 g of sample was taken and 500 mL of water was added to the mill (XMQ250×90 conical ball mill, Wuhan Mining Machinery Co., Ltd.) at S / L = 1:1 for 1, 2, 3, 4 and 5 minutes. After grinding, the ground product was transferred to the vibrating screen ( 200 wet standard vibrating screen, Wuhan Rock Powder Equipment Manufacturing Co., Ltd.) was used for screening analysis. When there were no obvious mineral particles in the clear water under the sieve, it was considered that the screening end point was reached. Figure 1 shown.

[0050] 1.2.3 Flotation experiment

[0051] In each flotation experiment, 500g of sample was weighed and added to the XFD 1.5L flotation cell for roughing and scavenging to obtain coarse concentrate, middlings and tailings. The experimental process is as follows: Figure 2 As shown. Before grinding, 2g of lime was added to the ball mill and ground together with the sample. During flotation, butyl xanthate (60g / t for roughing, 40g / t for scavenging) and 2# oil (20g / t for roughing, 10g / t for scavenging) were added in the order of collector first and frother. Roughing and scavenging were performed to obtain rough concentrate, middlings and tailings. After the experiment, the experimental product was filtered, dried and ground, and then its copper grade was tested.

[0052] 1.3 Analysis methods

[0053] The elemental composition of the experimental samples was studied by X-ray fluorescence spectrometry (XRF), and the mineral composition, content, and distribution relationship of the samples were studied by X-ray diffractometer, scanning electron microscope and energy spectrum. The distribution particle size and characteristics of the main target minerals in the ore have an important influence on the determination of grinding fineness and the design of the process flow. Therefore, the process mineralogy parameter automatic analysis system BPMA (BGRIMM Process Mineralogy Analyzing System) was used to analyze the distribution particle size and dissociation degree of magnetite, pyrite and chalcopyrite in the raw ore. The copper grade of the flotation concentrate, middlings and tailings was determined by titration.

[0054] The concentrate yield and copper metal recovery rate are calculated according to formula (1) and formula (2) respectively.

[0055]

[0056]

[0057] Wherein, γ is the rough concentrate yield (%), m1 is the rough concentrate mass (g), m is the sample mass (g), ε is the flotation recovery (%), β is the metal grade in the concentrate (%), and α is the metal grade in the sample (%).

[0058] 2. Results and Discussion

[0059] 2.1 Ore properties

[0060] 2.1.1 Chemical multi-element

[0061] The TFe grade in the raw ore is relatively high, reaching 50.28%. The contents of other valuable metals such as copper and cobalt are 0.54% and 0.0213% respectively. In addition, it also contains 0.0418% titanium. The detailed elemental composition data are shown in Table 1. The gangue minerals are mainly calcium magnesium silicate minerals, mainly MgO, SiO2 and CaO. Other oxide types are shown in Table 2. Compared with the previous shallow ores, the Fe metal content is significantly increased (TFe of shallow ores is about 35%). Therefore, the matching degree between the existing mineral processing technology and the ore properties is reduced, and the product indicators of the mineral processing plant fluctuate significantly. For example, the grinding process and magnetic separation process have a great influence on the classification and recovery of magnetite.

[0062] Table 1 XRF analysis results of raw ore (single element)

[0063]

[0064] *g / t.

[0065] Table 2 XRF analysis results of raw ore (oxides)

[0066]

[0067] 2.1.2 Mineral composition

[0068] Figure 3 , Figure 4 The main mineral types of the original ore analyzed by XRD and BPMA are respectively. The metal minerals in the ore are mainly magnetite, with a content of 79.94%. The metal sulfides are mainly chalcopyrite and pyrite, of which the content of chalcopyrite is 0.68% and the content of pyrite is 1.80%. The gangue minerals are mostly pyroxene and dolomite, and other gangue minerals include garnet, olivine, amphibole, mica, calcite, quartz, etc. Its main components are magnesium, iron and aluminum silicates, carbonates and silicon dioxide. Figure 5 This is the BSE mineral coloring diagram of the original ore BPMA analysis, Figure 5 It can be seen that, in general, the magnetite particles in the original ore are relatively large, and most of the particles are intertwined or wrapped with other minerals. Further analysis found that Figure 5(b) Medium-large particles of magnetite encapsulate pyroxene and olivine particles; Figure 5 In (c), adjacent intergrowths of magnetite particles and calcite can also be observed. Figure 5 (c) and (f) show that the mineral particles of pyrite and chalcopyrite are intergrown with magnetite in small amounts. In addition, large particles of pyrite and chalcopyrite show a close symbiotic relationship between the two. Therefore, in order to ensure the product quality of magnetically separated iron ore concentrate, it is necessary to ensure a high degree of dissociation of magnetite.

[0069] Tables 3 and 4 are the chemical phase analysis of iron and copper in the raw ore samples, respectively. As shown in Table 3, iron is mainly found in magnetic iron, with a distribution rate of 96.44%, followed by non-magnetic iron minerals such as pyrite, hematite and siderite. The results of the phase analysis are consistent with the analysis results of XRD and BPMA, and magnetite is the main recovered iron mineral. As shown in Table 4, for copper minerals, copper minerals are mainly primary copper sulfide, accounting for 94.03%. Based on the above mineralogical properties, the processing technology of this polymetallic ore can adopt a beneficiation method of first flotation and then magnetic separation. On the one hand, flotation can easily separate sulfide ores including chalcopyrite, pyrite and a small amount of pyrrhotite that may exist. On the other hand, the particle size requirement of flotation can ensure the dissociation degree of magnetite, which is conducive to improving the product quality of magnetic iron concentrate.

[0070] Table 3 Analysis of iron phases in raw ore

[0071]

[0072] Table 4 Phase analysis of raw copper ore

[0073]

[0074] 2.1.3 Embedding granularity

[0075] Figure 6 is the cumulative particle size distribution curve of magnetite, pyrite and chalcopyrite. Figure 6 It can be seen that magnetite and pyrite in the original ore have similar particle size distribution characteristics, with coarse particles and low particle size distribution curves; the embedded particle size of chalcopyrite is fine, distributed below 208μm, and the cumulative particle size distribution curve is high. When the particle size is +74μm, the cumulative distribution of magnetite reaches 59.86%, pyrite is 71.12%, and chalcopyrite is only 29.43%. In terms of the embedded particle size of the mineral, when the grinding fineness is -74μm, about 70% of the magnetite is in a monomer dissociated state, and the monomer dissociation degree of chalcopyrite is higher, at 80%. In order to dissociate more than 75% of the chalcopyrite, the ore needs to be ground to a particle size of -38μm.

[0076] 2.1.4 Embedding relationship

[0077] For magnetite, the mineral content accounts for a large proportion, and after crushing and grinding, there are more magnetite particles that are dissociated as monomers. A small amount of particles associated with sulfide minerals are less likely to be mixed into the foam product during the flotation process, and the magnetite itself has a large specific gravity and is easy to fall off during the slurry flow and foam floating process. Therefore, it is necessary to focus on the relationship between the main recovered metal sulfide ores and a small amount of precious metals, including the embedded particle size, the occurrence of minerals and the embedded relationship. These factors determine the choice of grinding system and mineral processing process.

[0078] Figure 7 It is the intergrowth relationship between the main metal sulfide ore and other minerals. Under the scanning electron microscope, it was found that chalcopyrite mainly forms intergrowth with gangue minerals. Figure 7 (a) It can be seen that in the intergrowth formed with olivine, the larger chalcopyrite particles mainly surround the olivine in the form of shell-type or encapsulation-type intergrowth. Figure 7 (b) It can be seen that particles with smaller particle sizes are usually adjacent to each other, such as the adjacent intergrowth of chalcopyrite and pyrite. The BPMA mineral automatic analysis system also identified cobalt sulfide ores, such as carrollite and siegenite. Figure 7 (c), (d), and (e) show that the mineral particles of pyroxene and pyroxene are relatively small, less than 20 μm. They usually form adjacent and inclusion-type intergrowths with other minerals, such as adjacent intergrowths of pyroxene and calcite, and inclusions formed with magnetite. As far as the flotation of pyroxene and pyroxene is concerned, their floatability is similar to that of sulfide ores. Under sufficient dissociation degree, xanthate collectors have a good collecting effect. However, the embedded particle size of cobalt minerals is too fine, all distributed below 20 μm, and is wrapped by other minerals. Therefore, the recovery of cobalt has higher requirements for grinding. Some mineral particles with larger brightness were also found under the scanning electron microscope, such as Figure 7 (f) shows the mineral particles of natural gold, with a particle size of 70 μm. EDS analysis shows that the mass fractions of gold and silver are 84.90% and 15.10%, respectively. In terms of the intergrowth state of natural gold, its dissociation degree is relatively high, and only a small amount of pyrite exists at the edge of the particles. Therefore, it can be inferred that the natural gold particles are embedded in the pyrite particles in the original ore, and the particles are stripped from the pyrite due to crushing and grinding. It can be seen that gold minerals and sulfide ores have a close symbiotic relationship, and the recovery of such fine embedded minerals can be enhanced by increasing the dissociation degree of their load minerals.

[0079] 2.1.5 Degree of dissociation

[0080] Table 5 shows the degree of intergrowth of magnetite, pyrite and chalcopyrite in the original ore. As can be seen from Table 5, the degree of monomer dissociation of magnetite, pyrite and chalcopyrite in the original ore is not high, 10.36% for magnetite, 9.19% for pyrite and 15.59% for chalcopyrite. A large number of intergrowths are formed with other minerals, especially three intergrowths, with multiple intergrowths of magnetite and pyrite exceeding 70% and multiple intergrowths of chalcopyrite exceeding 60%. Figure 8 It is the association of magnetite, pyrite and chalcopyrite with other minerals. Figure 8 It can be seen that magnetite is associated with olivine and pyroxene in large quantities, with a total amount of 33.01%. Pyrite is associated with magnetite, dolomite, pyroxene and olivine in large quantities, and the degree of association with chalcopyrite is 5.25%. Chalcopyrite is mostly associated with magnetite and dolomite, with the degrees of association being 17.75% and 12.74% respectively. For the flotation of chalcopyrite and pyrite, if a higher recovery rate is to be achieved, a large range of mineral dissociation must be achieved in order to fully interact with the collector molecules. In addition, the association of magnetite and sulfide ores will also cause the sulfur content of iron concentrate to be too high, affecting product indicators. Therefore, the optimization and transformation of the grinding process is of great significance to the flotation of sulfide minerals and the production of high-quality iron concentrate.

[0081] Table 5 The degree of intergrowth of magnetite, pyrite and chalcopyrite in the original ore

[0082]

[0083] 2.2 Pre-flotation treatment

[0084] 2.2.1 Pre-magnetic separation

[0085] Since the magnetite content of medium-deep ores is significantly increased, and the current magnetic separation process parameters are targeted at shallow ores, the magnetic field strength of the magnetic separator cannot separate most of the magnetic minerals. Therefore, it is necessary to explore the appropriate magnetic field strength of the magnetic separator. In the experiment, the magnetic field strength is adjusted by changing the excitation current, so the excitation current is used instead of the magnetic field strength to explore the relationship between the excitation current of the magnetic separator and the magnetic product indicators.

[0086] Fig. 9 is the relationship between the excitation current and the iron and copper content of the magnetic product and the iron recovery rate. Fig. 9It can be seen that when the excitation current changes from 0.1 to 0.5A, the iron metal grade in the magnetic product decreases slightly with the increase of the excitation current. When the excitation current is 0.1A, the iron grade is 62.33%, and when the current increases to 0.5A, the iron grade only decreases by 1.5%. The iron recovery rate increases significantly with the increase of the excitation current. When the current increases from 0.1A to 0.5A, the iron recovery rate increases from 63.03% to 96.62%. The excitation current has little effect on the change of the iron grade of the magnetic product concentrate, indicating that the dissociation degree of magnetite particles in the original ore is high, and there are fewer mineral particles associated with other minerals. During the magnetic separation process, there are fewer other gangue minerals mixed with magnetite in the magnetic product, which is consistent with the process mineralogical properties of the original ore. Increasing the excitation current increases the attraction of magnetic minerals, and the magnetic force on the large-size magnetite particles increases, gradually getting rid of their own gravity and water flow resistance and moving toward the magnetic pole, and more magnetite particles are separated. For copper minerals, 17.75% of the copper minerals in the original ore are associated with magnetite. Therefore, when magnetite is enriched in the magnetic product, the copper minerals associated with it enter the magnetic product together. The copper recovery rate increases with the increase of the excitation current. When the excitation current is 0.5A, the copper recovery rate of the magnetic product reaches 54.33%. Considering the iron recovery rate and the separation effect of copper minerals, the optimal excitation current of the magnetic separator is between 0.2A and 0.3A. When the excitation current is 0.25A, the yield of the magnetic product reaches 75%, of which the magnetic product contains 0.27% copper and the non-magnetic product contains 1.23% copper.

[0087] 2.2.2 Grinding fineness - time

[0088] Fig.10 This is the relationship between the grinding time and the grinding -200 mesh yield of the original ore, magnetic product and non-magnetic product. Fig.10 It can be seen that non-magnetic products are easier to grind, and the -200 mesh particle size produced in the same grinding time is the highest, followed by the original ore, and magnetic products are more difficult to grind. When the grinding time is 4 minutes, the -200 mesh particle size yield of non-magnetic products reaches 79.84%, and the -200 mesh particle size yield of magnetic products is only 72.50%. This is due to the differences in mineral composition and ore properties of different samples. The main component of the magnetic product is magnetite, which has a hardness of more than 5.5, while the hardness of non-magnetic minerals with dolomite and other gangue minerals as the main components is relatively small, about 4. Judging from the logarithmic fitting results of the grinding curve, most of the experimental data points fall on the curve, indicating that the fitting correlation is good, and the correlation coefficients are all greater than 0.99.

[0089] 2.3 Flotation experiment

[0090] 2.3.1 Scheme I: Grinding-Flotation

[0091] Fig.11This is the experimental process flow of direct grinding and flotation of raw ore. Fig.12 It is the product index of grinding-flotation. Fig.12 It can be seen that the copper grade of the rough concentrate and the middling ore increases first and then decreases with the change trend of the grinding fineness (-200 mesh particle content), while the copper recovery rate increases with the increase of grinding fineness. When the -200 mesh content is 65%, the dissociation degree of copper minerals is insufficient, and the copper minerals captured by the collector are less. The copper grades of the rough concentrate and the middling ore are 12.84% and 2.22% respectively, and the copper recovery rate is 88.35% at this time. Continue to increase the grinding time, the mineral particles are ground finer, the wrapped copper mineral particles are exposed, and more copper is recovered. When the grinding fineness is 65%, the copper grade of the rough concentrate and the middling ore is the highest, which is 13.21% and 3.85% respectively. When the grinding fineness is greater than 65%, the copper grade of the rough concentrate and the middling ore decreases significantly, and the copper grade drops to 6.77% and 0.88% respectively when the -200 mesh content is 75%. This is mainly attributed to the indiscriminate grinding of the mill. From the grinding fineness-time relationship curve, it can be seen that magnetic minerals and non-magnetic minerals can be ground to different degrees. In the grinding process, gangue mineral particles are ground faster than magnetite particles. In the experimental group with a larger grinding fineness, the gangue mineral content in the fine particle size is higher, and the amount of entrained and mixed foam products is more, which has an adverse effect on the flotation index, and this effect will become more and more obvious as the particle size of the gangue mineral becomes finer. In addition, for the recovery rate of copper, the change of grinding fineness has little effect on it. When the grinding fineness increases by 5%, the copper recovery rate only increases by about 1%. However, the higher the grinding fineness, the longer the grinding time. It takes 32 seconds to increase the grinding fineness from 65% to 70%, and it takes 47 seconds to increase from 75% to 80%. The energy consumption generated in actual production will be higher. Therefore, considering the comprehensive grinding energy consumption and product indicators, the flotation fineness is preferably -200 mesh, accounting for 65%. At this time, the copper grades of coarse concentrate and medium ore are 13.21% and 3.85% respectively, and the copper recovery rate is 88.36%.

[0092] 2.3.2 Scheme II: Pre-magnetic separation - grinding - separate flotation

[0093] Fig.13 This is the experimental process of raw ore pre-magnetic separation - grinding - separate flotation. Fig.14 , Fig.15 They are the flotation results of non-magnetic products and magnetic products respectively. Fig.13 For the experimental process and conditions, the raw ore is pre-magnetically separated to obtain magnetic products and non-magnetic products, which are then ground according to the grinding fineness-time relationship curve in Section 2.2.2, and the obtained grinding products are then flotated. The same reagent system is used as in the grinding-flotation process. Fig.14 and Fig.15It can be seen that the roughing product indicators of non-magnetic products and magnetic products show the same trend, and the grades of concentrates and middlings decrease with the increase of grinding fineness. It is worth mentioning that when the grinding fineness is 65%, the copper grade of non-magnetic product flotation concentrate is 8.79%, and the copper grade of magnetic product flotation concentrate is 9.38%. The copper grade in non-magnetic products is much higher than that in magnetic products, the former is 1.22% and the latter is 0.28%. From the copper grade of the flotation tailings of the two, the non-magnetic product is 0.22%, which is much higher than the 0.047% of the magnetic product.

[0094] Fig.16 This is the distribution diagram of the dissociation degree of chalcopyrite in the flotation tailings of non-magnetic products with a fineness of 75%. Fig.16 It can be seen that in the flotation tailings with a grinding fineness of 75%, there are still 23.99% of the copper mineral particles that are dissociated into monomers, and 68.03% of the copper mineral particles have a dissociation degree greater than 80%. Fig.17 The particle sorting diagram of chalcopyrite and pyrite in the flotation tailings of non-magnetic products with a fineness of 75%. From (a), the monomer dissociated chalcopyrite particles can be clearly observed. It can be seen that the copper loss in the tailings is not caused by insufficient dissociation.

[0095] Fig.18 The XRD phase analysis results of the original ore and the 75% fineness magnetic separation tailings flotation tailings. Fig.18 It can be seen that after pre-magnetic separation, gangue minerals such as dolomite, calcite and kaolinite are enriched in large quantities. Dolomite increased from 4.8% to 30.4%, and calcite increased from 3.7% to 16.6%. These changes lead to increased slurry viscosity, the mixing of foam products to reduce concentrate indicators, and the coating on the surface of copper minerals to hinder the reaction between copper minerals and collectors, seriously affecting the recovery of copper minerals. In addition, research reports show that in the flotation of sulfide ores, carbonate gangue minerals such as calcite and dolomite will release a large amount of Ca in the slurry. 2+ and Mg 2+ , thus forming colloidal precipitates that hinder the flotation of sulfide ores.

[0096] 2.3.3 Scheme III: Pre-magnetic separation - grinding - mixed flotation

[0097] In order to avoid the adverse effects of over-grinding of non-magnetic minerals and excessive concentration of gangue minerals on copper ore flotation, the ore beneficiation method of pre-magnetic separation of raw ore - separate grinding - proportional mixing and re-floatation is adopted. Fig.19 The experimental process flow of this mineral processing method is as follows: Fig. 20 is the experimental result. Fig.19As shown, after pre-magnetic separation, the raw ore is ground according to the grinding fineness-time relationship curve in Section 2.2.2; then the magnetic product and the non-magnetic product are mixed evenly at a mass ratio of 3:1 (determined based on the 75% yield of magnetic minerals in the pre-magnetic separation experiment in Section 2.2.1) as flotation feed. Fig. 20 It can be seen that the change of copper grade in concentrate and middling is similar to the first two processes. The copper grade increases with the increase of grinding fineness, and the copper grade reaches a peak of 6.64% when the grinding fineness is around 65%. At this time, the copper recovery rate reaches 89.54%. In addition, the change of grinding fineness has little effect on the recovery rate of copper. Even at a grinding fineness of 60%, the recovery rate of copper can reach 87.68%, which is not much different from the recovery rate of 90.17% at a fineness of 80%. In addition, compared with the flotation process of magnetic products and non-magnetic products, due to the reduction of the proportion of silicate and carbonate gangue minerals in the slurry, the adverse effect of fine gangue minerals on the flotation of copper minerals is reduced, which greatly reduces the loss of copper minerals in tailings. At a fineness of 65%, the copper grade of tailings is 0.057%. Compared with the direct grinding and flotation process of the original ore, while ensuring the grinding of magnetic minerals, the amount of over-grinding of non-magnetic minerals is reduced, which not only ensures the dissociation of copper minerals but also reduces the adverse effects of fine gangue minerals on flotation, and the copper recovery rate is increased by 2.3%.

[0098] 2.4 Process applicability

[0099] As far as the current production process is concerned, the ore processed by the beneficiation plant is in a transition period from shallow ore to medium and deep ore, and the changes in the properties of the ore during this change process are mainly concentrated in the obvious increase in the content of magnetite, and the total iron grade has increased from 36.19% to 50.28%. The biggest trouble caused by this change in ore properties to the production process is the prominent "density effect" problem of magnetite in the grinding and grading process. That is, the magnetite particles of qualified particle size in the grinding product cannot be separated during the grading process, but are returned to the grinding process, resulting in serious over-grinding of magnetite particles, which in turn causes a series of problems in the subsequent flotation process and dehydration process. Therefore, on the basis of the above three schemes, with Scheme III as a reference, the copper metal content of Schemes I and II is calculated, and the impact of the improvement of the grinding process on the flotation of copper ore is discussed. The calculation results are shown in Table 6. The process flow of the three beneficiation schemes is shown in Table 6. Fig.21As shown in Table 6 (flotation includes conventional roughing, scavenging and concentrating, etc., and the final product of flotation is copper concentrate; magnetic separation also includes conventional roughing, scavenging and concentrating, etc., and the final product is iron concentrate). As shown in Table 6, Scheme I is to directly grind the raw ore, with the shortest grinding time of 10.92 minutes and a copper metal recovery rate of 88.35%. However, this process will also cause the problem of low magnetite classification efficiency when applied to the selection of medium and deep ores in the future, or even more serious. Schemes II and III pre-magnetically select the raw ore, and then grind the magnetic product and non-magnetic product separately, with the same total grinding time of 11.53 minutes. The difference is that the magnetic product and non-magnetic product of Scheme II are separated to flot copper, which is obviously not feasible. The copper metal recovery rate is only 71.18% (2.3.2 Scheme II is to separate the magnetic product and non-magnetic product for copper flotation after pre-magnetic separation, and the total copper recovery rate is not discussed in this chapter; the copper recovery rate discussed in 2.4 Process Applicability is only for the copper of grinding feed, that is, the aforementioned total copper recovery rate), which is significantly lower than 89.54% of Scheme 3. Compared with Scheme I, Scheme III is used for the future separation of medium and deep ores. Since magnetic minerals and non-magnetic minerals have more targeted classification, it can not only solve the "density effect" of magnetite classification, but also is beneficial to the flotation of copper minerals, and the metal recovery rate is increased by 1.19% (89.54%-88.35%=1.19%).

[0100] Table 6 Comparison of different mineral processing schemes

[0101]

[0102]

[0103] 3. Conclusion

[0104] The main mineral component of the ore is magnetite, accounting for nearly 80%, with a total iron grade of 50.28%, a copper grade of 0.54%, and 0.0213% cobalt and 1.13g / t gold. It is a polymetallic iron-rich ore resource. The gangue minerals are mostly pyroxene and dolomite, as well as garnet, olivine and amphibole, and its main components are silicates or carbonates of magnesium, iron and aluminum.

[0105] Most of the chalcopyrite is embedded in the gangue minerals, and the embedded particle size is relatively fine. More than 75% of the chalcopyrite is distributed in the -38μm particle size. The proportion of magnetite in this particle size is 93.48%. Magnetite can be selected and chalcopyrite can be effectively separated by magnetic separation.

[0106] Cobalt minerals, gold and silver minerals are closely associated with metal sulfide ores, and the embedded particle size is relatively fine, mostly distributed below 20μm. The natural gold particles in the original ore form intergrowths with chalcopyrite, and the cobalt minerals in sulfide-copper-cobalt ore and sulfide-nickel-cobalt ore also form adjacent or encapsulated intergrowths with chalcopyrite and pyrite, which can be enriched into concentrate products with the recovery of sulfide ores.

[0107] The process of pre-magnetic separation, separate grinding and mixed flotation can effectively improve the grinding efficiency of magnetic products and reduce the over-grinding of non-magnetic products. Under the conditions of excitation current of 0.25A and grinding fineness of -200 mesh 65%, 6.64% copper concentrate can be obtained by roughing, and the total recovery rate of copper reaches 89.54%.

[0108] The above examples are provided to those skilled in the art to fully disclose and describe how to make and use the claimed embodiments, and are not intended to limit the scope of the disclosure herein. Modifications that are obvious to those skilled in the art will fall within the scope of the appended claims.

Claims

1. A polymetallic magnetite beneficiation process, characterized in that: The following steps are involved: (1) Pre-magnetic separation: Screen and crush the ore, add appropriate amount of water to stir into slurry, add it to the magnetic separator, adjust the excitation current to 0.2A ~ 0.3A, and perform pre-magnetic separation until non-magnetic minerals are produced, and obtain non-magnetic products and magnetic products; (2) Grinding separately: The non-magnetic product and the magnetic product obtained above are added to a ball mill respectively, and a proper amount of water and lime are added to grind the ore until the fineness of -200 mesh content is 60% to 80%, thereby obtaining a non-magnetic grinding product and a magnetic grinding product respectively; (3) Mixed flotation: The magnetic grinding product and the non-magnetic grinding product obtained above are mixed in a mass ratio of (2.5-3.5):1, and flotation and magnetic separation are performed to obtain copper concentrate and iron concentrate.

2. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: The original ore of the polymetallic magnetite contains 50.28% TFe, 0.54% copper, 0.0213% cobalt and 0.0418% titanium; 79.94% magnetite, 0.68% chalcopyrite and 1.80% pyrite.

3. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: In the step (1), the excitation current is 0.25A.

4. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: In the step (2), the ore is ground to a fineness of -200 mesh with a content of 65%.

5. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: In the step (3), the mass ratio of the magnetic grinding product to the non-magnetic grinding product is 3:

1.

6. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: In the step (2), a hydrocyclone is used to classify the product after grinding.

7. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: In the step (2), the lime is added in a ratio of 2 to 8 kg / t.

8. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: In the step (3), flotation includes roughing and scavenging. During roughing and scavenging, butyl xanthate and 2# oil are added in the order of collector first and frother to obtain coarse concentrate, middlings and tailings.

9. The beneficiation process of polymetallic magnetite according to claim 8, characterized in that: During the roughing, the addition ratio of butyl xanthate is 40-80 g / t, and the addition ratio of 2# oil is 10-30 g / t; during the scavenging, the addition ratio of butyl xanthate is 20-60 g / t, and the addition ratio of 2# oil is 5-15 g / t.

10. The beneficiation process of polymetallic magnetite according to claim 1, characterized in that: The excitation current is 0.25A, the grinding fineness is -200 mesh content is 65%, the mass ratio of magnetic grinding products to non-magnetic grinding products is 3:1; the addition ratio of lime is 4kg / t; flotation includes roughing and scavenging, in roughing, the addition ratio of butyl xanthate is 60g / t, and the addition ratio of 2# oil is 20g / t; in scavenging, the addition ratio of butyl xanthate is 40g / t, and the addition ratio of 2# oil is 10g / t.

Citation Information

Patent Citations

  • Complete flotation mineral separation process for polymetallic siderite

    CN101274306A

  • Beneficiation method for copper-nickel sulfide ore containing pyrrhotite

    CN106583022A

  • Beneficiation method for diversified raw ore

    CN108906312A

  • Beneficiation process of skarn type magnetite containing copper and gold

    CN112588433A

  • Mixed iron ore beneficiation method

    WO2024082323A1