Method for synthesizing novel two-dimensional semiconductor alloy nanosheet

By using inorganic covalent compound CICs as reaction intermediates and combining with primary amine soft film plate auxiliary strategy, the problem of difficulty in synthesis and regulation of WZ alloy NPLs in the prior art is solved, and efficient preparation and precise regulation of various alloy NPLs are achieved. , improving the manipulation and application value of materials.

CN118954441APending Publication Date: 2024-11-15NANJING UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410874746.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently synthesize and regulate two-dimensional semiconductor alloy nanosheets, especially wurtzite (WZ) alloy NPLs, resulting in limited manipulation and application of materials.

Method used

Using a new reaction intermediate - inorganic covalent compounds (CICs), a variety of WZ alloy NPLs were successfully prepared and regulated through the auxiliary strategy of primary amine soft film plates. The high reactivity and kinetic equilibrium state of CICs were used to achieve The precise composition and regulation of alloy NPLs is carried out.

Benefits of technology

It has realized the efficient preparation and regulation of WZ alloy NPLs, broken the bottleneck of traditional technology, and successfully prepared a variety of alloy NPLs, such as ZnCdSe, ZnCdS, CdSeS, CdSTe, ZnCdSeS, etc., which have excellent universality and control, satisfying Different application requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954441A_ABST
    Figure CN118954441A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of design and synthesis of novel two-dimensional semiconductor nanomaterials, and particularly relates to a method for synthesizing a novel two-dimensional semiconductor alloy nanosheet, which is characterized in that a novel inorganic covalent compound CICs is used as a reaction intermediate, and a primary amine soft diaphragm plate auxiliary strategy is utilized to synthesize the novel two-dimensional semiconductor alloy nanosheet. A series of wurtzite type II-IV group two-dimensional semiconductor alloy nanosheets are successfully developed and prepared; the composition of the alloy nanosheet can be accurately regulated and controlled by regulating and controlling the composition and the feed ratio of the CICs, and synthesis regulation and control of binary, ternary, quaternary and other multi-element alloy nanosheets are allowed; according to the technology, a novel functionalized alloy nanosheet material library is enriched, development of the functional nanocrystalline design field is promoted, and a new technical route support is provided for the material science field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of design and synthesis of novel two-dimensional semiconductor nanomaterials, and in particular relates to a method for synthesizing novel two-dimensional semiconductor alloy nanosheets. Background Art

[0002] Colloidal semiconductor nanocrystals (NCs) have shown excellent application value in many fields due to their special properties that can be adjusted with structure and size. They have attracted extensive research attention. According to the dimension in which the excitons are confined, NCs can be divided into three categories, including zero-dimensional spherical quantum dots (QDs) with excitons confined in three dimensions, one-dimensional nanorods (NRs) / nanowires (NWs) with excitons confined in two dimensions, and two-dimensional nanosheets (NPLs) / nanosheets with excitons confined in one dimension. Compared with QDs and NRs, the electronic structure of NPLs, where excitons are confined only along the vertical direction, is similar to that of semiconductor quantum wells, and has unique optical properties, such as extremely narrow emission line width, short photoluminescence lifetime, high gain coefficient, and giant vibration intensity transition. At the same time, studies have shown that in many cases, the optoelectronic properties of NPLs are superior to those of the corresponding QDs / NRs, namely high single-photon and two-photon absorption coefficients, high directional emission, and low laser threshold, which makes them perfect candidates for applications ranging from light emission and conversion to sensing. In addition, due to their two-dimensional shape and atomically smooth surface, NPLs can be arranged into orderly stacks or laterally oriented assemblies, opening up additional dimensions for manipulating material properties that are not accessible with other types of NCs. By changing the composition and structure of NPLs and designing complex NPLs, the energy levels of materials can be effectively regulated and their optoelectronic characteristics can be adjusted. Therefore, designing and synthesizing various new NPLs materials, enhancing their related properties or giving the materials new functions to cope with different application scenarios has been the focus of functional material design and application in recent years.

[0003] In the past decade, NPLs have made extensive breakthroughs and significant progress in synthesis, growth mechanism, optical and electronic properties, and practical applications. So far, materials scientists have successfully prepared various semiconductor NPLs with different thicknesses and atomic flatness by adjusting the reaction environment, precursor type, reaction path, etc., including CdS, CdSe, CdTe, ZnS, ZnSe, and ZnTe. In addition, based on different reaction mechanisms, single crystal NPLs can be effectively separated and purified, including zinc blende (ZB) with cubic unit cells and wurtzite (WZ) with hexagonal unit cells. For ZB-NPLs, people have studied their different technical mechanisms, including the self-assembly process of initially formed small nanocrystals; the process of flat intermediates and then development through the directional attachment of 2D embryos with many single-point intermediates; the growth process of large NPLs extending outward through the continuous precursor attachments of their NPL seeds (embryos). The synthesis technology of WZ-NPLs is often assembled by the corresponding nanoclusters (MSCs) under the assistance of soft film. Based on this, people have further designed and synthesized various types of complex new NPLs, including core-crown type, core-shell type, abab heterojunction type, doping type and alloy type. Among them, alloy-type NPLs can effectively regulate the band gap of the material by changing the composition ratio of NPLs, so that its energy level changes continuously, corresponding to the continuous shift of the spectrum. This makes up for the problem of partial spectrum loss caused by the discontinuous red shift of the spectrum corresponding to the jumping growth characteristics of NPLs materials themselves. Not only that, alloy NPLs have shown excellent performance in catalytic and optoelectronic applications, which is attributed to their more active sites and more suitable energy level structure compared to other types of NPLs.

[0004] Although the existing technology has achieved remarkable results in the preparation of various binary and complex new NPLs, the efficient preparation and regulation of alloy NPLs, especially based on WZ crystal form, is still a challenge. At present, the synthesis of alloy NPLs is often limited to ZB crystal form, and the elemental composition that can be regulated is relatively single. On the one hand, this is mainly due to the single synthesis mechanism of WZ crystal form NPLs, which limits the controllability of the material. Traditional intermediate MSCs usually have a relatively stable and ordered structural arrangement, are in a thermodynamically stable state and have low reactivity, which makes it difficult to react with foreign ions or other MSCs to obtain the final alloy NPLs. Although there are technical attempts to first prepare alloy MSCs and then grow the corresponding WZ alloy NPLs. However, this strategy currently only achieves the preparation of a ZnCdSe NPL, and the lateral size of the product has exceeded the micron level. Since the preparation technology of alloy MSCs itself is not controllable, this method is not a reliable and efficient strategy.

[0005] On the other hand, the current synthesis technology of ZB alloy NPLs often directly mixes in the corresponding foreign ion source to participate in the growth. Since different ion sources have different reactivity, and the growth of nanocrystals requires the activity balance of each ion source, this greatly limits the regulation of different component alloy NPLs. Especially for WZ crystal NPLs, which have more stringent requirements on ligand environment and precursor type, the technical route of directly mixing precursors cannot effectively obtain the target product.

[0006] At present, the design and regulation technology of new complex NPLs is a problem in the development of functional nanocrystals, especially for alloy-type WZ-NPLs, which urgently need efficient and reliable synthesis methods and corresponding technical routes. The main technical bottleneck of this problem comes from the limited technical route of WZ-NPLs. Summary of the invention

[0007] The present invention solves the above-mentioned technical problems existing in the prior art, and provides a simple and efficient preparation and regulation technology route for WZ alloy NPLs based on a new type of reaction intermediate (inorganic covalent compound, CICs). CICs are a special type of reaction intermediate with excellent dispersibility, featureless optical absorption, and anions and cations are connected to each other in the form of covalent bonds. Compared with MSCs, CICs have an indefinite atomic composition and can be understood as a quasi-isomer of MSCs. Unlike MSCs, CICs are in a kinetic equilibrium state and have higher reactivity. Many studies have shown that CICs, as a new type of intermediate, can mediate the synthesis and post-synthetic transformation of various types of NCs. Based on this, the present invention successfully developed and prepared a variety of (6 types) alloy WZ-NPLs based on the new CICs as reaction intermediates and with the help of the soft film plate auxiliary strategy of primary amines. Not only that, by regulating the composition of CICs and the feed ratio, the composition of alloy NPLs can be precisely regulated. This technology not only enriches the new functional NPLs material library and promotes the development of functional nanocrystal design, but also provides new technical route support in the field of materials science.

[0008] The technical solution of the present invention is as follows:

[0009] (1) Preparation of different types of CICs

[0010] The present invention takes the widely concerned II-IV semiconductor NPLs as the starting point, and aims to prepare and synthesize WZ-type alloy NPLs with different components through the technical route mediated by CICs. First, according to different element combinations, it is necessary to determine the optimal reaction conditions, which need to meet the following points: 1. The reaction temperature meets the bonding requirements of the corresponding elements; 2. The reaction rate is appropriate at the corresponding temperature, and the material will not further nucleate and grow in a short time; 3. The appropriate reaction time ensures that the material is fully bonded and avoids further growth; 4. The appropriate reaction environment meets the ligand requirements necessary for the formation of CICs; 5. The appropriate precursor, according to different reaction pairs, selects the appropriate anion and cation precursors. According to the above reaction conditions, the corresponding CICs precursor is prepared in a specific environment. At this time, the formation of the corresponding ME covalent pair and the featureless optical absorption are confirmed by the corresponding ultraviolet spectrum and high-resolution mass spectrometry. According to the obtained CICs, based on the target alloy NPLs, the subsequent added foreign anions or other CICs are regulated. Due to the high reactivity of CICs, when foreign reactants are introduced, they immediately induce mutual reactions to obtain the corresponding alloy CICs.

[0011] (2) Preparation of alloy NPLs

[0012] According to the CICs obtained in (1), since they are isomers with MSCs and have corresponding covalent bonds, the technical goal of this invention is to introduce an amine template to assist the assembly of CICs to obtain the corresponding NPLs. The choice of primary amine determines the reaction rate of the material and affects the final morphology of the product. This is because different primary amines have different carbon chain lengths, which correspond to different boiling points and interlayer spacings of the soft template. Therefore, we choose octylamine with eight carbon chain lengths as the reaction system, which has a suitable boiling point and interlayer spacing, and is suitable for the growth requirements of various WZ-type NPLs. Next, the CICs are placed in primary amines for reaction at a suitable temperature, and with the help of the layered template of the primary amine, the CICs are assembled to obtain the corresponding alloy NPLs. Corresponding to different types of alloy NPLs, it is necessary to determine their different optimal reaction temperatures, which need to meet the following requirements: 1. It can meet the nucleation growth of CICs; 2. Appropriate reaction rate to prevent too fast or too slow reaction rate from resulting in low quality of NPLs products; 3. Prevent the generation of other layers or granular byproducts.

[0013] (3) Purification and characterization of alloy NPLs

[0014] The product after the reaction is in the form of a turbid liquid in octylamine, and the product is collected by centrifugation. In order to remove the excess unreacted precursor compounds and uncoordinated excess ligands dispersed in the system, it is further purified by adding ethanol to reprecipitate and dispersed in non-polar reagents such as toluene or n-hexane. Due to the strong template effect of octylamine, the product at this time is mostly in a bundled state, so it is necessary to add an appropriate amount of oleylamine or cadmium oleate to ultrasonically assist in dispersion to obtain a monodispersed product. The specific implementation is: after the reaction is completed, the product is collected by centrifugation (12000rpm, 2min), the product is redispersed in 1ml toluene and ultrasonically dispersed for 3min to assist dispersion, 2ml ethanol is added to shake for about 1min and placed in a centrifuge to purify the product (10000rpm, 2min), and this step is repeated 2 to 3 times and then dispersed in 1ml toluene and 50μL oleylamine is added to ultrasonically disperse for 2min. The composition of WZ alloy NPLs is confirmed by UV-visible spectroscopy, XRD, ICP-OES, Raman, TEM, etc.

[0015] A method for synthesizing wurtzite-type (WZ-type) two-dimensional semiconductor alloy nanosheets (alloy NPLs) comprises the following steps:

[0016] Step 1, preparing CICs, wherein the CICs are selected from any one or a combination of more than one of CdSe-CICs, ZnSe-CICs, ZnS-CICs, and CdSe-CICs;

[0017] Step 2: Add Cd source, Zn source, selenium source, sulfur source or tellurium source to any one of the CICs described in step 1, mix and react in primary amine to obtain WZ type alloy NPLs; or place any two or more CICs described in step 1 in primary amine for mixing and reacting to obtain WZ type alloy NPLs.

[0018] Preferably, the alloy NPLs are II-IV group semiconductor alloy NPLs.

[0019] Preferably, the preparation method of the CICs is: placing Cd salt and Zn salt in primary amine, reacting at 80-120° C. under an inert gas environment, injecting trioctylphosphine-selenium (TOP-Se), sulfur-octadecene (S-ODE) or trioctylphosphine-tellurium (TOP-Te), reacting at 100-160° C. for 5-20 minutes, and obtaining the corresponding CICs.

[0020] More preferably, the preparation method of the CdSe-CICs is as follows: Cd(OAc)2·2H2O (0.1599 g) is placed in a 50 ml three-necked bottle containing 4.6 g of oleylamine, and the mixture is stirred at room temperature for degassing for 30 min. The mixture is then heated to 80°C for degassing for 1 h, and heated to 120°C for reaction for 20 min after nitrogen is passed through the mixture. The system is cooled to 80°C, and then hot-injected into a TOP-Se solution (0.0118 g of selenium powder dissolved in 0.224 g of TOP (trioctylphosphine)), and the mixture is heated to 150°C for reaction for 20 min. The corresponding CdSe-CICs are obtained.

[0021] The preparation method of the ZnSe-CICs is as follows: Zn(OAc)2 (0.22 g) is placed in a 50 ml three-necked bottle containing 5.3 ml of oleylamine, and the mixture is stirred at room temperature for 30 min for degassing. Then the mixture is heated to 80°C for degassing / nitrogen cycle three times. The system is heated to 120°C and degassed for 1 h. The system is cooled to 80°C, and after passing into a nitrogen environment, TOP-Se solution (0.33 ml, 0.3 mmol), 52 μL of DPP and 0.5 ml of oleylamine are hot-injected, and the mixture is heated to 160°C for reaction for 15 min. The corresponding ZnSe-CICs are obtained.

[0022] The preparation method of the ZnS-CICs is as follows: dissolving ZnCl2 in a mixed solution of oleylamine and octylamine (concentration of 0.58 mM, wherein the volume ratio of oleylamine to octylamine is 2:1), first degassing at room temperature for 30 minutes and then degassing at 80°C for 1 hour. Then reacting at 120°C under nitrogen for 1 hour until the solution becomes clear and transparent to obtain an oleylamine zinc precursor. The obtained oleylamine zinc precursor (10-50 μL) is mixed with 0.2 ml of 0.1 M S-OED (sulfur flakes dissolved in OED (octadecene) solution) and reacted at 100°C for 5 minutes.

[0023] The preparation method of CdTe-CICs is as follows: similar to CdSe-CICs, oleylamine cadmium (0.59 mM) is prepared at 120° C. A certain amount (1.54 ml, 0.88 mmol) of oleylamine cadmium and TOP-Te (0.39 mL, 0.22 mmol Te) are reacted in 3 ml of oleylamine at 135° C. for 15 min to prepare CdTe-CICs.

[0024] Preferably, in step 2, primary amine Cd salt, primary amine Zn salt, trioctylphosphine-selenium (TOP-Se), sulfur-octadecene (S-ODE) or trioctylphosphine-tellurium (TOP-Te) is added to any one of the CICs described in step 1, and mixed and reacted in primary amine to obtain WZ type alloy NPLs.

[0025] Preferably, in step 2, the primary amine is n-octylamine.

[0026] Preferably, the specific steps of step 2 are: mixing CdSe-CICs and ZnSe-CICs in a molar ratio of 1:10 to 10:1, reacting in a primary amine solution at 130 to 180° C. to prepare WZ ZnCdSe NPLs.

[0027] Preferably, the specific steps of step 2 are: mixing ZnS-CICs and oleylamine cadmium in a molar ratio of 1:5 to 5:1, reacting in a primary amine solution at 130 to 180° C. to obtain WZ ZnCdS NPLs.

[0028] Preferably, the specific steps of step 2 are: mixing CdSe-CICs and S-ODE in a molar ratio of 1:3 to 3:1, reacting in a primary amine solution at 130 to 180° C. to obtain WZ CdSeS NPLs.

[0029] Preferably, the specific steps of step 2 are: mixing CdSe-CICs and TOP-Te in a molar ratio of 2:1, reacting in a primary amine solution at 130-180° C. to obtain WZ CdSeTe NPLs.

[0030] Preferably, the specific steps of step 2 are: mixing CdTe-CICs and S-ODE in a molar ratio of 1:1, reacting in a primary amine solution at 130-180° C. to obtain WZ CdSTe NPLs.

[0031] Preferably, the specific steps of step 2 are: mixing CdSe-CICs, ZnSe-CICs and S-ODE in a molar ratio of 2:4:1 to 6:3:1, reacting in a primary amine solution at 130 to 180° C. to obtain WZ ZnCdSeSNPLs.

[0032] Preferably, the reaction time of step 2 is 6 to 24 hours; more preferably, 8 to 12 hours.

[0033] Compared with the prior art, the advantages of the present invention are as follows:

[0034] The present invention is a simple and efficient synthesis and preparation technology of WZ-type NPLs, which allows the synthesis and regulation of binary, ternary, quaternary and other multi-element alloy NPLs.

[0035] The present invention breaks the technical bottleneck of existing synthesis strategies. By introducing a new and efficient active intermediate CICs to replace the traditional MSCs intermediate, the technology is applied for the first time to the design and regulation of new alloy WZ-NPLs. Through this technology, a series of new alloy NPLs, including ZnCdSe, ZnCdS, CdSeS, CdSeTe, CdSTe, and ZnCdSeS NPLs, are successfully prepared. Moreover, the technology can effectively meet the precise regulation of different elements in each alloy NPLs and has excellent universality.

[0036] The present invention is simple to operate and does not require complicated preparation and processing methods, which is conducive to large-scale application; the operating conditions required by the present invention are mild and can be met by any sealed high-temperature reaction device, such as a reaction kettle, a glass reactor, a three-necked flask, etc.; the present invention is highly controllable, and the reaction conditions can be arbitrarily adjusted according to different application scenarios and different product requirements, and the target product can be designed according to local conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 ESI-MS spectra of CdSe-CICs, ZnSe-CICs and their mixture (a). UV spectra of ZnSe-CICs and CdSe-CICs (b).

[0038] Figure 2 .TEM characterization of WZ ZnCdSe NPLs products (a). UV (b), Raman (c) and XRD (d) characterization of WZ ZnCdSe NPLs products with different ratios.

[0039] Figure 3 UV (a), Raman (b) and XRD (c) characterizations of WZ ZnCdS NPLs products with different ratios. TEM characterization of WZ ZnCdS NPLs products (d).

[0040] Figure 4 UV (a), Raman (c) and XRD (d) characterizations of WZ CdSeS NPLs products with different ratios. TEM characterization of WZ CdSeS NPLs products (b).

[0041] Figure 5 UV (a, b), Raman (c, f) of WZ CdSeTe and CdSTeNPLs products. TEM (d) and XRD (e) characterization of WZ CdSeTe NPLs.

[0042] Figure 6UV (a), Raman (b) and XRD (c) characterizations of WZ ZnCdSeS NPLs products with different ratios. TEM characterization of WZ ZnCdSeS NPLs products (d). DETAILED DESCRIPTION

[0043] Example 1: Preparation of CICs

[0044] The preparation method of CdSe-CICs is as follows: Cd(OAc)2·2H2O (0.1599 g) is placed in a 50 ml three-necked bottle containing 4.6 g of oleylamine, and the mixture is stirred at room temperature for degassing for 30 min. Then, the mixture is heated to 80°C for degassing for 1 h, and then heated to 120°C for reaction for 20 min after nitrogen is passed through the mixture. The system is cooled to 80°C, and then hot-injected into a TOP-Se solution (0.0118 g of selenium powder dissolved in 0.224 g of TOP (trioctylphosphine)), and heated to 150°C for reaction for 20 min. The corresponding CdSe-CICs are obtained.

[0045] The preparation method of ZnSe-CICs is as follows: Zn(OAc)2 (0.22 g) is placed in a 50 ml three-necked bottle with 5.3 ml of oleylamine, and the mixture is stirred at room temperature for 30 min for degassing. Then the mixture is heated to 80°C for degassing / nitrogen cycle three times. The system is heated to 120°C and degassed for 1 h. The system is cooled to 80°C, and after passing into a nitrogen environment, TOP-Se solution (0.33 ml, 0.3 mmol), 52 μL of DPP and 0.5 ml of oleylamine are hot-injected, and the mixture is heated to 160°C for 15 min for reaction. The corresponding ZnSe-CICs are obtained.

[0046] The preparation method of ZnS-CICs is as follows: dissolve ZnCl2 in a mixed solution of oleylamine and octylamine (concentration of 0.58mM, wherein the volume ratio of oleylamine to octylamine is 2:1), first degas at room temperature for 30min and then degas at 80℃ for 1h. Then react at 120℃ for 1h under nitrogen until the solution is clear and transparent to obtain an oleylamine zinc precursor. Mix the obtained oleylamine zinc precursor (10-50μL) with 0.2ml 0.1M S-OED (sulfur flakes dissolved in OED (octadecene) solution) and react at 100℃ for 5min.

[0047] The preparation method of CdTe-CICs is as follows: Similar to CdSe-CICs, oleylamine cadmium (0.59 mM) was prepared at 120°C. A certain amount (1.54 ml, 0.88 mmol) of oleylamine cadmium and TOP-Te (0.39 mL, 0.22 mmol Te) were reacted in 3 ml of oleylamine at 135°C for 15 min to prepare CdTe-CICs.

[0048] Example 2: WZ ZnCdSe NPLs

[0049] Technical route: First, we took CdSe-CICs and ZnSe-CICs and their mixtures as examples to conduct relevant characterization. Figure 1 a It can be seen that the ESI-MS spectrum shows that the two have different covalent pairs of CdSe and ZnSe, corresponding to the isotope peak distribution of different m / z in the figure. By mixing the two, it can be seen that a new isotope peak distribution appears at a high m / z position in the ESI0ME spectrum, which may be attributed to the obtained ZnCdSe-CICs. And by Figure 1 The UV in b also confirmed the CICs state at this time, and no related MSCs or other products with other optical characteristics appeared.

[0050] Then, different proportions of CdSe-CICs and ZnSe-CICs (the total volume of the two CICs is 600μL, and the volume combinations are adjusted such as: 600+0; 500+100; 400+200; 300+300; 200+400; 100+500; 0+600) were placed in 3ml of octylamine solution, sealed under nitrogen environment, and reacted at 180℃. The reaction gradually changed from the original clear and transparent light yellow solution to an orange-yellow suspension, and the degree of suspension increased as the reaction progressed and finally remained unchanged. The reaction was stopped after 10h. The product was purified and characterized accordingly.

[0051] pass Figure 2 a As can be seen from the graph, the product presents a two-dimensional morphology of flake distribution, and its size is about 75±5*20±5nm. This verifies that the corresponding two-dimensional NPLs product can be obtained through the CICs technical route. Then, we adjust the ratio of the two CICs to obtain alloy NPLs with different composition ratios. Through the UV characterization of the corresponding product ( Figure 2 b) It can be seen that as the Cd ratio increases, the product absorption gradually red-shifts from pure ZnSe NPLs to CdSe NPLs (349nm~450nm). And the double peak characteristics of the two-dimensional material characteristics can be seen in the product absorption, from which we speculate that the corresponding alloy ZnCdSeNPLs product can be obtained at this time. And we also confirmed this view through further ICP-OES data. The content of Zn+Cd in the product is just close to the Se content. Raman ( Figure 2 c) Characterization further confirmed the bonding composition of Zn-Se and Cd-Se in the product, and with the increase of Cd content, the relative proportion of LO peak attributed to Cd-Se in Raman gradually increased. Through the above results, we verified the successful preparation of alloy ZnCdSe NPLs. In addition, through XRD characterization of each sample ( Figure 2d), we can judge that they all belong to the diffraction characteristics of the WZ crystal type. With the increase of Cd ratio, its diffraction peak gradually blue-shifts, indicating the increase of lattice spacing. This is mainly attributed to the different atomic sizes of ZnSe and CdSe corresponding to different lattice parameters, and the corresponding alloy ZnCdSe is just distributed between the two. And from the XRD diffraction image, it can be seen that only the continuous displacement of diffraction occurs in the products of different ratios, and no new diffraction peaks appear or disappear, which also confirms the homogeneous composition of the alloy material rather than the nucleation and growth of each separately.

[0052] Example 3: WZ ZnCdS NPLs

[0053] Technical route: Add different amounts of oleylamine cadmium (0.58mM) precursor to the obtained ZnS-CICs (the total volume of the added oleylamine cadmium and the corresponding volume of oleylamine zinc in ZnS-CICs is 60μL, and the Cd:Zn ratio distribution is 1:0, 5:1, 2:1, 1:1, 1:2, 1:5, 0:1), place it at 130℃ for 10h to obtain a milky turbid liquid, which is then purified and characterized.

[0054] Based on the above different volume Zn / Cd feed ratios, products with different absorption states can be obtained. Figure 3 As shown in a, the product absorption continuously red-shifts with the increase of Cd content and is distributed between 289 and 375 nm. According to the Raman spectrum of the corresponding sample ( Figure 3 b) can further confirm the bonding composition of Cd-S and Zn-S. XRD ( Figure 3 c) provides evidence for its WZ crystal state. TEM characterization of the product also further verified its two-dimensional flake distribution, which showed a small size distribution of about 25*3nm due to the composition of the S element. The above results confirm that this technical route successfully obtained the WZ ZnCdS NPLs product.

[0055] Example 4: WZ CdSeS NPLs

[0056] Technical route: Based on the previous two examples, we have successfully prepared the double cationic alloy WZ-NPLs. Next, we will prepare the double anionic alloy WZ CdSeS NPLs based on this strategy. 0.24ml CdSe-CICs was placed in octylamine, and different amounts (100, 300, 500, 700μL) of S-ODE (0.1M) were added, and placed in a 135℃ environment for 10h to obtain a yellow suspension. After subsequent purification, the relevant product characterization was carried out.

[0057] Figure 4The UV-visible spectrum of a is visible. By changing the amount of S-ODE added, the spectrum also undergoes a continuous red shift from 375 to 450nm. Based on the trend of UV changes, we speculate that this technology can also prepare double anion alloy NPLs. By TEM ( Figure 4 b) Characterization confirmed the two-dimensional flake morphology of the product, about 15*4nm. Further Raman ( Figure 4 c) and XRD( Figure 4 d) Characterization also confirmed its Cd-Se and Cd-S bonding composition, as well as its WZ crystal characteristics. The above results fully demonstrate that our CICs-mediated technology route is highly applicable to both dicationic and dianionic alloys WZ-NPLs.

[0058] Example 5: WZ CdSeTe, CdSTe NPLs

[0059] In addition, since Te-based materials often have very strict requirements on reaction conditions and the reaction process is difficult to control, alloy Te-NPLs are still a huge challenge and there is no suitable and effective technical means. In this project, we successfully achieved the efficient preparation of Te-based alloy NPLs through the CICs-mediated technical route.

[0060] Technical route: For CdSeTe, we introduced TOP-Te (10μL, 0.1M) as Te source into 0.2ml CdSe-CICs, and placed it in pure octylamine at 150℃ for 10h to obtain an orange-yellow turbid liquid, which was purified and analyzed for products. Similarly, for CdSeTe NPLs, 0.2ml CdTe-CICs was mixed with 50μL S-ODE (0.1M) and placed in 3ml octylamine at 140℃ for 10h to obtain a milky yellow turbid liquid. After purification, the corresponding product analysis was performed.

[0061] pass Figure 5 As shown in Fig. 5a and 5b, the absorption of the corresponding alloy NPLs is between that of CdSe and CdTe, and between that of CdS and CdTe. Through the UV spectrum, we preliminarily speculate that the alloy NPLs are obtained. Taking CdSeTe as an example, further TEM characterization ( Figure 5 d) The two-dimensional flake morphology of the product was also verified. Further Raman and XRD characterizations also verified the alloy bonding composition of the two NPLs and the corresponding WZ diffraction characteristics. This shows that our CICs-mediated technology route has excellent universality.

[0062] Example 6: WZ ZnCdSeS NPLs

[0063] Based on the above results, we have successfully prepared various WZ-based alloy NPLs through the CICs-mediated technology route and achieved efficient regulation of its components. Furthermore, we have further expanded this strategy and designed and constructed quaternary alloy ZnCdSeS NPLs.

[0064] Technical route: After mixing 150μL CdSe-CICs and 200μL ZnSe-CICs, an external sulfur source S-ODE (0.1M, 50, 100, 150, 200μL) was added, and the mixture was placed in octylamine at 160°C for 10h to obtain an orange suspension. After post-treatment and purification, the product was analyzed and characterized.

[0065] pass Figure 6 a The UV-visible spectra of the products with different ratios show that the product absorption is distributed between ZnS and CdSe. Since the band gaps between different materials are quite different, the span of the absorption spectrum moving with the change of element ratio is relatively large. On the other hand, due to the complex composition of the quaternary alloy material itself and the relatively large lattice mismatch rate between the materials, the peak quality of the UV spectrum of this material is poorer than that of the ternary and binary materials. By TEM ( Figure 6 d) Its flake-like morphology can be seen, but due to its complex composition of multiple elements and the difference in growth rates of different elements, the product morphology is less regular. Raman ( Figure 6 b) and XRD( Figure 6 c) The quaternary bonding composition and WZ crystal characteristics of the product were confirmed. This verifies the excellent ability of our proposed CICs-mediated technology route to efficiently prepare and regulate various WZ alloy NPLs.

[0066] It should be noted that the above embodiments are merely preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Equivalent replacements or substitutions made on the basis of the above embodiments all fall within the protection scope of the present invention.

Claims

1. A method for synthesizing WZ-type two-dimensional semiconductor alloy NPLs, characterized in that: The following steps are involved: Step 1, preparing CICs, wherein the CICs are selected from any one or a combination of more than one of CdSe-CICs, ZnSe-CICs, ZnS-CICs, and CdSe-CICs; Step 2, adding a Cd source, a Zn source, a selenium source, a sulfur source or a tellurium source to any one of the CICs described in step 1, mixing and reacting in a primary amine to obtain the WZ-type two-dimensional semiconductor alloy NPLs; Or any two or more CICs described in step 1 are placed in a primary amine for mixed reaction to obtain the WZ-type two-dimensional semiconductor alloy NPLs.

2. The method according to claim 1, characterized in that The preparation method of the CICs is as follows: placing Cd salt and Zn salt in primary amine, reacting at 80-120° C. in an inert gas environment, injecting trioctylphosphine-selenium, sulfur-octadecene or trioctylphosphine-tellurium, reacting at 100-160° C. for 5-20 minutes, and obtaining the corresponding CICs.

3. The method according to claim 1 or 2, characterized in that In the step 2, primary amine Cd salt, primary amine Zn salt, trioctylphosphine-selenium, sulfur-octadecene or trioctylphosphine-tellurium are added to any one of the CICs described in the step 1, and mixed and reacted in the primary amine to obtain WZ type alloy NPLs.

4. The method according to claim 1, characterized in that In the step 2, the primary amine is n-octylamine.

5. The method according to claim 1 or 4, characterized in that The specific steps of step 2 are: The mixture is mixed with ZnSe-CICs in a molar ratio of 1:10 to 10:1, and reacted in a primary amine solution at 130 to 180° C. to obtain WZ ZnCdSe NPLs.

6. The method according to claim 1 or 4, characterized in that: The specific steps of step 2 are: mixing ZnS-CICs and oleylamine cadmium in a molar ratio of 1:5 to 5:1, reacting in a primary amine solution at 130 to 180° C. to obtain WZ ZnCdS NPLs.

7. The method according to claim 1 or 4, characterized in that The specific steps of step 2 are: The mixture is mixed with S-ODE in a molar ratio of 1:3 to 3:1, and reacted in a primary amine solution at 130 to 180° C. to obtain WZ CdSeS NPLs.

8. The method according to claim 1 or 4, characterized in that: The specific steps of step 2 are: The mixture was mixed with TOP-Te in a molar ratio of 2:1, and reacted in a primary amine solution at 130-180°C to obtain WZ CdSeTe NPLs.

9. The method according to claim 1 or 4, characterized in that: The specific steps of step 2 are: mixing CdTe-CICs and S-ODE in a molar ratio of 1:1, reacting in a primary amine solution at 130-180° C. to obtain WZCdSTe NPLs.

10. The method according to claim 1 or 4, characterized in that: The specific steps of step 2 are: CdSe-CICs, ZnSe-CICs and S-ODE are mixed in a molar ratio of 2:4:1 to 6:3:1, and reacted in a primary amine solution at 130 to 180° C. to obtain WZ ZnCdSeS NPLs.

Citation Information

Patent Citations

  • Preparation method of full-inorganic colloid nanocrystal with high fluorescence yield

    CN114350364A

  • Photosensitive, inorganic ligand-capped inorganic nanocrystals

    US20220011664A1