Glass substrate forming mold and glass substrate forming method
By designing glass substrate forming molds suitable for high temperatures, the energy waste and safety hazards in the glass substrate forming process in the prior art are solved, and the automation molding and detection results of high-performance glass substrates are achieved. It is suitable for high-performance glass substrates Research and development of performance glass substrates.
Patent Information
- Application Number
- CN202411079655.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-07
AI Technical Summary
When preparing high-performance glass substrates, it is difficult to control the composition of different materials and the molding of molten glass liquid, which can easily lead to safety hazards such as energy waste and glass block explosion. It is difficult to directly apply to the production line in laboratory tests, which affects production efficiency and Consistency of product performance.
A glass substrate forming mold is designed, including a mold base, a shaping device, a pressing device and a heating device. It can automatically mold glass substrates of different thicknesses at high temperatures, and use preheating, weighing and melting, applying ammonium iodide solution, and pressing. and annealing treatment to ensure the formation safety and detection accuracy of the glass substrate.
It realizes the safe forming of glass substrates of different thicknesses at high temperatures, ensuring the uniformity and accuracy of the performance detection results of glass substrates after molding, reducing the risk of energy waste and accidents, and is suitable for the research and development of high-performance glass substrate materials.
Smart Images

Figure CN118954908A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a glass substrate forming method, a forming mould and application, and belongs to the technical field of detection. Background Art
[0002] New glass has played an increasingly significant role in the development of the glass industry. In recent years, with the vigorous development of the domestic and foreign liquid crystal panel industry, domestic liquid crystal panel display technology has also developed rapidly, especially high-generation liquid crystal panel display technology. From the perspective of the existing liquid crystal panel industry, whether it is TFT-LCD or OLED, glass substrate is one of the important and key materials required for its production, and it is also a basic component of the liquid crystal panel. However, facing the demand for high-generation glass substrates in today's society, the performance requirements of glass substrates are also getting higher and higher. The problem that follows is how to control the composition of different material squares to make corresponding glass substrates, and then detect their performance changes, so that they can finally be put into production. Often this process can only be carried out in the laboratory for small tests, so that unpredictable consequences such as energy waste caused by production line experiments can be avoided. Despite this, how to make the final molten glass liquid form an ideal glass substrate through laboratory material adjustment is a major problem. At present, it is often used to form blocks through ordinary molds, and then thin, cut and polish the glass frit through cutting and grinding and polishing devices. In this way, one is to waste energy and time, and the other is to be unable to determine that the glass frit will not have stress unevenness and bursting during the sample preparation process, which brings dangers.
[0003] In order to solve such problems, the present invention designs a glass substrate forming method, a forming mold and an application. The forming mold is simple to operate and can be formed into glass substrates of different thicknesses. At the same time, the forming mold of the present invention can also adapt to molten glass liquids of different viscosities for forming. It can be automatically formed at a relatively high temperature without causing the glass blocks to explode, and is relatively safe. At the same time, the formed glass substrate can also ensure the uniformity and accuracy of the test results, which is of great help to the research and development of high-performance glass substrate materials. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a glass substrate forming mold and a glass substrate forming method, which can adapt to molten glass liquids with different viscosities for forming, automatically form at a relatively high temperature, and will not cause the glass block to explode.
[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0006] The present application provides a glass substrate forming mold, characterized by comprising:
[0007] A mold base, wherein a shaping device is provided on the mold base;
[0008] A support rod, comprising a telescopic rod and a cross rod, wherein the telescopic rod is vertically mounted on one side of the mold base, and the cross rod is horizontally mounted on one end of the telescopic rod away from the mold base;
[0009] The upper pressing device is installed on the cross bar at a position away from one end of the telescopic rod, and the upper pressing device is located directly above the shaping device and is directly projected onto the shaping device.
[0010] Optionally, in some embodiments of the present application, the pressing device includes:
[0011] A pressing head, the pressing head is installed on one side of the upper pressing device facing the shaping device;
[0012] A counterweight block, detachably mounted in the upper pressure device;
[0013] A heating device is located in the upper pressing device, and the heating device heats the pressing head.
[0014] Optionally, in some embodiments of the present application, the shaping device includes a shaping groove, and the position of the shaping groove corresponds to the position of the pressure head.
[0015] Optionally, in some embodiments of the present application, a heating element is further provided on the mold base, and the heating element is provided corresponding to the molding groove.
[0016] Optionally, in some embodiments of the present application, the telescopic rod includes an electric telescopic member.
[0017] Optionally, in some embodiments of the present application, a glass substrate forming method is further provided, which is implemented by using a glass substrate forming mold as described above, and the glass substrate forming method includes:
[0018] Step 1: preheating the glass substrate forming mold;
[0019] Step 2: weighing and melting the glass component raw materials;
[0020] Step 3: Apply ammonium iodide solution in the shaping tank;
[0021] Step 4: Pour the molten raw material into the shaping tank, press the molten raw material through the upper pressing device, and increase the pressure to a preset pressure;
[0022] Step 5: After the pressing is completed, the glass is annealed and tested to complete the manufacturing.
[0023] Optionally, in some embodiments of the present application, the preset pressure includes 5 bar, 10 bar and 15 bar.
[0024] Optionally, in some embodiments of the present application, the detected items include: transmittance, annealing point, strain point, and softening point.
[0025] The molding die of the present invention has a wide application range and strong operability.
[0026] The advantage is that a silicon carbon rod heating device is installed in the mold base, which can provide baking for the mold shaping device;
[0027] The advantage is that the mold base includes pressure control and temperature control parts, as well as control switches and emergency stop devices;
[0028] The advantage is that the pressure control part can ensure the downward pressure of the pressure head;
[0029] The advantage is that the temperature control part can ensure the temperature of the glass liquid under load;
[0030] The advantage is that ammonium iodide is applied to the groove of the mold forming device before the high-temperature molten glass liquid is formed, which facilitates the separation of the formed glass substrate from the mold;
[0031] The advantage is that it is equipped with an emergency stop device, which is convenient for uncontrollable accidents and can ensure safety in time;
[0032] The advantage is that the upper pressing device includes a resistance wire heating device, a built-in counterweight, and a pressure head. The built-in counterweight can automatically balance the weight according to the set pressure, which is convenient for forming glass of different thicknesses without manual pressure control;
[0033] The advantage is that the resistance wire heating device included in the upper pressure device can keep the upper pressure head at a certain temperature, so that it is easy to cause explosion when the cold state meets the hot state;
[0034] The advantage is that the designed electric telescopic parts can be automatically pressed and formed at high temperature, with a pressing rate of 1.0 to 2.5 mm / min and a holding time of 2 to 5 minutes;
[0035] The advantage is that the mold base is built with refractory zirconium material, silicon carbon rod heating element, and external stainless steel plugging and fixing, which can ensure temperature concentration and is not easy to dissipate heat, and the preferred temperature range is 600℃~1000℃;
[0036] The advantage is that after repeated experiments and calculations on the molding mold, it was found that the amount of molten glass m, density ρ, pressing thickness d, and pressing pressure p are in a certain relationship, that is, p=0.55*m / (ρ*d).
[0037] Compared with the prior art, the beneficial effects of the present invention are:
[0038] The present invention designs a glass substrate forming method and a forming mold. The forming mold is easy to operate and can be formed into glass substrates of different thicknesses. At the same time, the forming mold of the present invention can also adapt to molten glass liquids of different viscosities for forming. It is automatically formed at a relatively high temperature and will not cause the glass block to explode. It is relatively safe. At the same time, the formed glass substrate can also ensure the uniformity and accuracy of the detection result, which is of great help to the research and development of high-performance glass substrate materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0040] Figure 1 A schematic diagram of the overall structure of a glass substrate forming mold provided in an embodiment of the present application;
[0041] Figure 2 A schematic diagram of the side structure of a glass substrate forming mold provided in an embodiment of the present application;
[0042] Figure 3 This is a schematic diagram of the overall process of the glass substrate forming method provided in an embodiment of the present application.
[0043] Description of reference numerals:
[0044] 100, mold base; 110, shaping device; 111, shaping groove; 120, heating element; 200, support rod; 210, telescopic rod; 220, cross bar; 300, upper pressing device; 310, pressing head; 320, counterweight block; 330, heating device. DETAILED DESCRIPTION
[0045] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the protection scope of the present application. It is understood that the drawings are only provided for reference and illustration, and are not used to limit the present application. The connection relationship shown in the drawings is only for the convenience of clear description and does not limit the connection method.
[0046] In an embodiment of the present application, a glass substrate forming abrasive tool is provided, such as Figure 1-2 As shown, the glass substrate forming mold mainly includes a mold base 100 , a support rod 200 and an upper pressing device 300 .
[0047] Specifically:
[0048] The mold base 100 is provided with a shaping device 110, which includes a shaping groove 111, which is located at the top of the mold base 100, and a heating element 120 is provided at the bottom of the shaping groove 111, which is provided corresponding to the position of the shaping groove 111. A support rod 200 is provided at one side of the mold base 100, and the support rod 200 includes a telescopic rod 210 and a cross rod 220, and the telescopic rod 210 is an electric telescopic component, and the electric telescopic component can drive the movement of the upper pressing device 300 to automatically press and form the glass raw materials at high temperature, with a descending pressing rate of 1.0 to 2.5 mm / min and a holding time of 2 to 5 minutes;
[0049] The cross bar 220 is arranged at one end of the telescopic rod 210, specifically, the cross bar 220 is horizontally installed on the end of the telescopic rod 210 away from the mold base 100, and an upper pressing device 300 is arranged at the end of the cross bar 220, and the upper pressing device 300 is installed on the cross bar 220 at one end away from the telescopic rod 210, and the upper pressing device 300 is located directly above the shaping device 110 and is directly projected onto the shaping device 110;
[0050] The upper pressing device 300 includes a pressing head 310, a counterweight block 320 and a heating device 330. Figure 2 As shown, the pressing head 310 is installed on one side of the upper pressing device 300 facing the shaping device 110 ; the counterweight block 320 is detachably installed in the upper pressing device 300 ; the heating device 330 is located in the upper pressing device 300 , and the heating device 330 heats the pressing head 310 .
[0051] The position of the shaping groove 111 corresponds to the position of the pressing head 310 .
[0052] Through the mold, an embodiment of the present application provides a glass substrate forming method, which mainly includes:
[0053] Step 1: preheating the mold base 100 in the glass substrate forming mold;
[0054] Step 2: weighing and melting the glass component raw materials;
[0055] Step 3: Apply ammonium iodide solution in the shaping tank 111;
[0056] Step 4: Pour the molten raw material into the shaping groove 111, press the molten raw material through the upper pressing device 300, and increase the pressure to a preset pressure;
[0057] Step 5: After the pressing is completed, the glass is annealed and tested to complete the manufacturing.
[0058] In order to verify the applicability of the molding mold of the present invention and the effectiveness and accuracy of the method of use, low-viscosity and high-viscosity materials are molded into glass substrates of different thicknesses, and then the performance is tested. In step 2, the embodiment of the present invention uniformly adopts the same process to melt the materials, that is, a platinum-rhodium crucible and a high-temperature silicon-molybdenum rod lifting furnace are used for melting, wherein the high-temperature silicon-molybdenum rod lifting furnace uses silicon-molybdenum rods as heating elements, and the specific melting procedure adopts:
[0059] ①Rise the temperature from room temperature to 1000℃ at 10℃ / min;
[0060] ②Heat from 1000℃ to 1560℃ at a rate of 10℃ / min, and keep at 1560℃ for 2h;
[0061] ③Heat from 1560℃ to 1600℃ at a rate of 10℃ / min, and keep at 1600℃ for 1h;
[0062] ④Heat from 1600℃ to 1630℃ at a rate of 10℃ / min, and keep at 1630℃ for 1.5h.
[0063] Then the physical and chemical properties of the formed glass substrates were tested and compared. The specific comparison process is as follows:
[0064] Example 1
[0065] The glass substrate is formed by using low viscosity material component sodium-lime-silicon glass, and the mold of the present invention is used to form glass substrates of 0.5 mm and 1.0 mm, and the performance of glass substrates of corresponding thickness is tested. The specific steps are as follows:
[0066] Table 1 Composition of low viscosity sodium-calcium-silicon glass frit
[0067] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO MgO <![CDATA[Na2O]]> and amount Mass percentage / % 72.5 3.5 10.8 1.1 12.1 100% Raw material name Quartz sand Alumina Calcium carbonate Magnesium Oxide Sodium oxide
[0068] Weigh the raw materials of each group according to the mass percentage of the raw materials in Table 1 above, and weigh a total of 600g. After mixing evenly, put them in a platinum-rhodium crucible, place them in a silicon-molybdenum rod lifting furnace, and melt them;
[0069] According to the instructions Figure 1 Assemble, inspect and connect all structures, and set the temperature to 1000℃ for preheating;
[0070] After the fourth stage of the program is completed, the platinum-rhodium crucible containing the molten glass liquid is immediately taken out, and the molten glass liquid is poured into the shaping device 110 on the mold base 100 in the forming mold, specifically into the shaping groove 111, and the pressure setting button is clicked to set the pressing pressure to 5 bar, and the down / up boat switch is clicked to press the 0.5 mm glass substrate;
[0071] When the actual pressure value displayed on the pressure display window is equal to the set pressure value, start to maintain the pressure for 2 to 5 minutes;
[0072] After the pressure is maintained, click the down / up boat-shaped switch, and the pressure head moves up to zero position to complete the pressing;
[0073] The pressed glass substrate is removed and placed in a high-temperature resistance furnace pre-set at 500°C for annealing to eliminate stress;
[0074] Repeat the above steps to press the 1.0 mm glass substrate and perform annealing to eliminate stress;
[0075] After removing the stress, the glass substrates of 0.5mm and 1.0mm were taken out for physical and chemical performance testing. Each glass substrate of each thickness was tested in 3 groups, namely, the transmittance (550nm), annealing point, strain point, softening point and other items were tested. The test results are shown in Table 2 below:
[0076]
[0077] Comparative data of Example 1 show that, after melting the same material, glass substrates of different thicknesses are pressed and formed using a mold, except for the transmittance which is affected by the thickness itself, the other thermal properties are basically stable.
[0078] Example 2
[0079] The glass substrate is formed by using borosilicate glass as a high viscosity material component, and the mold of the present invention is used to form glass substrates of 0.5 mm and 1.0 mm, and the performance of glass substrates of corresponding thickness is tested. The specific steps are as follows:
[0080] Table 3 High viscosity borosilicate glass frit composition
[0081]
[0082] 1) Weigh the raw materials of each group according to the mass percentage of the raw materials in Table 3 above, and weigh a total of 600 g. After mixing evenly, put them in a platinum-rhodium crucible, place them in a silicon-molybdenum rod lifting furnace, and melt them;
[0083] 2) Follow the instructions Figure 1 Assemble, inspect and connect all structures, and set the temperature to 1000℃ for preheating;
[0084] 3) After the fourth stage of the procedure is completed, the platinum-rhodium crucible containing the molten glass liquid is immediately taken out, and the molten glass liquid is poured into the shaping device 110 on the mold base 100 in the forming mold, specifically into the shaping groove 111, and the pressure setting button is clicked to set the pressing pressure to 10 bar, and the down / up boat switch is clicked to press the 0.5 mm glass substrate;
[0085] 4) When the actual pressure value displayed on the pressure display window is equal to the set pressure value, start to maintain the pressure for 2 to 5 minutes;
[0086] 5) After the pressure is maintained, click the down / up boat-shaped switch, and the pressure head moves up to zero position to complete the pressing;
[0087] 6) After the pressed glass substrate is removed, it is placed in a high-temperature resistance furnace pre-set at 700°C for annealing to eliminate stress;
[0088] 7) Repeat the above steps to press a 1.0 mm glass substrate and perform annealing to eliminate stress;
[0089] 8) After the stress was relieved, the glass substrates of 0.5 mm and 1.0 mm were taken out for physical and chemical performance testing. Three groups of tests were conducted for each thickness of the glass substrate, namely, transmittance (550 nm), annealing point, strain point, softening point and other items were tested. The test results are shown in Table 4 below:
[0090]
[0091]
[0092] Comparative data of Example 2: After melting the same material, glass substrates of different thicknesses are pressed and formed using a mold. Except for the transmittance which is affected by the thickness itself, the other thermal properties are basically stable.
[0093] Example 3
[0094] The material that has been used and produced by the production line is weighed and melted, and the mold of the present invention is used to form and press the glass substrate. The physical and chemical properties of the glass substrate finally formed by pressing are analyzed and compared with the performance of the glass substrate produced by the production line. The specific steps are as follows:
[0095] Table 5 Production line glass frit composition
[0096]
[0097] 1) Weigh the raw materials of each group according to the mass percentage of the raw materials in Table 1 above, and weigh a total of 600 g. After mixing evenly, put them in a platinum-rhodium crucible, place them in a silicon-molybdenum rod lifting furnace, and melt them;
[0098] 2) Follow the instructions Figure 1 Assemble, inspect and connect all structures, and set the temperature to 1000℃ for preheating;
[0099] 3) After the fourth stage of the procedure is completed, the platinum-rhodium crucible containing the molten glass liquid is immediately taken out, and the molten glass liquid is poured into the shaping device 110 on the mold base 100 in the forming mold, specifically into the shaping groove 111, and the pressure setting button is clicked to set the pressing pressure to 15 bar, and the down / up boat switch is clicked to press the 0.5 mm glass substrate;
[0100] 4) When the actual pressure value displayed on the pressure display window is equal to the set pressure value, start to maintain the pressure for 2 to 5 minutes;
[0101] 5) After the pressure is maintained, click the down / up boat-shaped switch, and the pressure head moves up to zero position to complete the pressing;
[0102] 6) After the pressed glass substrate is removed, it is placed in a high-temperature resistance furnace pre-set at 700°C for annealing to eliminate stress;
[0103] 7) Take out the 0.5mm glass substrate after stress relief, and take a 300*300mm glass substrate produced by the production line, and perform physical and chemical performance tests respectively. Corresponding to the three groups of tests, namely, the transmittance (550nm), annealing point, strain point, softening point and other items are tested respectively. The test results are shown in Table 6 below:
[0104]
[0105] The comparative data of Example 3 show that the physical and chemical properties of the glass substrate formed by melting the same material and using a mold to press the glass substrate are basically consistent with those of the glass substrate produced by the production line.
[0106] Through the verification of the present invention in the above different embodiments, the molding mold of the present invention has a wide range of applications, which is sufficient to prove that the present invention meets the actual use requirements. Moreover, through the operation process of the embodiment, it is not difficult to find that the operation process is simple, the molding thickness range is relatively wide, and the performance detection of the glass substrate after molding is also relatively stable, which can adapt to the continuous renewal pursuit of high-performance glass substrates in today's society.
[0107] The above embodiments are only used to illustrate the technical method of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical method of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical method of the present invention.
Claims
1. A glass substrate forming mold, characterized in that: include: A mold base, wherein a shaping device is provided on the mold base; A support rod, comprising a telescopic rod and a cross rod, wherein the telescopic rod is vertically mounted on one side of the mold base, and the cross rod is horizontally mounted on one end of the telescopic rod away from the mold base; The upper pressing device is installed on the cross bar at a position away from one end of the telescopic rod, and the upper pressing device is located just above the shaping device and is projected directly onto the shaping device.
2. A glass substrate forming mold according to claim 1, characterized in that: The pressing device includes: A pressing head, the pressing head is mounted on a side of the upper pressing device facing the shaping device; A counterweight block is detachably mounted in the upper pressing device; A heating device is located in the upper pressing device, and the heating device heats the pressing head.
3. A glass substrate forming mold according to claim 2, characterized in that: The shaping device includes a shaping groove, and the position of the shaping groove corresponds to the position of the pressure head.
4. A glass substrate forming mold according to claim 3, characterized in that: The mold base is also provided with a heating element, and the heating element is arranged corresponding to the shaping groove.
5. The glass substrate forming mold according to claim 1, wherein: The telescopic rod includes an electric telescopic part.
6. A glass substrate forming method, implemented by the glass substrate forming mold according to claim 4, characterized in that: The glass substrate forming method comprises: Step 1: Preheating the mold base in the glass substrate forming mold; Step 2: Weigh and melt the glass component raw materials; Step 3: Apply ammonium iodide solution in the shaping tank; Step 4: Pour the molten raw material into the shaping tank, press the molten raw material through the upper pressing device, and increase the pressure to the preset pressure; Step 5: After pressing, the glass is annealed and tested to complete the manufacturing process.
7. The glass substrate forming method according to claim 6, wherein: The preset pressures include 5 bar, 10 bar and 15 bar.
8. The glass substrate forming method according to claim 6, wherein: The test items include: transmittance, annealing point, strain point, and softening point.
Citation Information
Patent Citations
Preparation method for ferromolybdenum sample melting glass body
CN102401756A
Method for accurately detecting components of raw glass sheets
CN104280415A
OLED glass substrate composition and preparation method thereof
CN116102254A
Glass ceramic containing petalite crystal phase, glass ceramic product and preparation method
CN117923800A
Mold press molding apparatus and method for production of glass optical element
JP2005239435A