Lithium-aluminum-silicon glass and preparation method thereof

By adjusting the oxide components of lithium aluminum silicon glass and using a two-step chemical strengthening method, a thicker compression stress layer was formed, which solved the problem of insufficient damage resistance of existing lithium aluminum silicon glass, and significantly improved its mechanical strength and Drop-resistant performance, suitable for high-demand display protection.

CN118954947AActive Publication Date: 2024-11-15CAIHONG GRP SHAOYANG SPECIAL GLASS CO LTD +1

Patent Information

Application Number
CN202411160635.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The mechanical strength and drop resistance of existing lithium-aluminum silicon glasses cannot meet the growing consumer requirements for damaging performance.

Method used

By adjusting the oxide component ratio, a lithium aluminum silicon glass was prepared, including 49-67% SiO2, 12-27% Al2O3, 2-5.5% Li2O, etc., and a two-step chemical strengthening method was used to utilize NaNO3 The mixed molten salt with KNO3 is ion exchanged to form a thicker compressive stress layer, improving the mechanical properties and drop resistance of the glass.

Benefits of technology

The surface compression stress CS≥800MPa and compression stress layer DOL≥100μm of lithium aluminum silicon glass is realized, which improves the drop resistance of the glass and can reach a directional drop height of 1500mm on 180 mesh sandpaper, which is suitable for high-demand display protection. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954947A_ABST
    Figure CN118954947A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of glass manufacturing, in particular to lithium aluminum silicon glass and a preparation method thereof.The lithium aluminum silicon glass is prepared from, by mass, 49 wt%-67 wt% of SiO2, 12 wt%-27 wt% of Al2O3, 0 wt%-3.5 wt% of B2O3, 2 wt%-5.5 wt% of Li2O, 0.5 wt%-13.5 wt% of Na2O, 0 wt%-3.5 wt% of K2O, 0 wt%-4.5 wt% of MgO, 0 wt%-3.5 wt% of ZnO, 0 wt%-2 wt% of CaO, 0 wt%-2 wt% of SrO, 1.5 wt%-14 wt% of P2O5, 0 wt%-1 wt% of ZrO2, 0 wt%-9 wt% of Y2O3 and 0 wt%-0.5 wt% of SnO; rO is the sum of the mass percent of MgO, ZnO, CaO and SrO in the glass composition, and the RO is 0-4.5%. Ion exchange is promoted by adjusting the components of the lithium aluminum silicon glass, and a thicker composite compressive stress layer is formed on the surface of the glass, so that the strength of the glass is improved, and the surface compressive stress, the bending resistance, the falling resistance and the like are improved. The problems that lithium aluminum silicon glass in the prior art is low in mechanical strength and falling resistance and cannot meet the requirement of consumers for damage resistance of a display screen are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass manufacturing, and in particular to lithium aluminosilicate glass and a preparation method thereof. Background Art

[0002] With the development of new display technologies, such as thinner and lighter, more diverse application scenarios, larger smart touch screens, and 5G, consumers have higher requirements for the anti-destructive performance of display screens, such as impact resistance, drop resistance, and scratch resistance. At present, the high-strength glass systems mainly include soda-lime-silica glass, high-aluminum glass, and lithium aluminosilicate glass. Compared with traditional soda-lime-silica glass and high-aluminum glass, lithium aluminosilicate glass has the characteristics of dense network structure, high elastic modulus, and suitability for two-step chemical tempering. It is regarded as the third generation of high-strength glass substrate and has attracted much attention in recent years. In view of the particularity of the Li2O component to the structure and properties of glass, aluminosilicate glass containing Li2O is usually called lithium aluminosilicate glass. The functions of Li2O in aluminosilicate glass are mainly manifested in two aspects: one is to provide a small radius Li for two-step chemical tempering enhancement. + , in order to achieve the simultaneous increase of surface compressive stress (CS) and stress layer depth (DOL), ensuring that the glass has good mechanical properties; secondly, to reduce the high-temperature viscosity of the glass and promote the full melting of high-content Al2O3. Lithium aluminum silicate glass is generally prepared by float or overflow method to produce large-sized glass sheets with different series of thicknesses, and then through ion exchange enhancement process, it can achieve high strength, high hardness and anti-drop functions. It is widely used as cover plates in the field of electronic information, transparent devices in the field of aviation, and observation windows of ships and special vehicles.

[0003] Although the existing lithium aluminum silicate glass has better mechanical strength and drop resistance than traditional glass, it still cannot meet the growing consumer demand for anti-destructiveness. Summary of the invention

[0004] In view of the problem that the mechanical strength and drop resistance of lithium aluminosilicate glass in the prior art are low and cannot meet the consumers' requirements for the anti-destruction performance of display screens, the present invention provides a lithium aluminosilicate glass and a preparation method thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a lithium aluminum silicate glass, which comprises the following raw material components in terms of the mass percentage of oxides:

[0007] 49-67wt% SiO2, 12-27wt% Al2O3, 0-3.5wt% B2O3, 2-5.5wt% Li2O, 0.5-13.5wt% Na2O, 0-3.5wt% K2O, 0-4.5wt% MgO, 0-3.5wt% ZnO, 0-2wt% CaO, 0-2wt% SrO, 1.5-14wt% P2O5, 0-1wt% ZrO2, 0-9wt% Y2O3 and 0-0.5wt% SnO; RO is the sum of the mass percentages of MgO, ZnO, CaO and SrO in the glass composition, and RO is 0-4.5%.

[0008] Furthermore, the surface compressive stress CS is ≥800 MPa, and the directional drop height is ≥800 mm on 180-grit sandpaper.

[0009] Furthermore, the compressive stress layer DOL is ≥100 μm, 0.15≤DOL / t≤0.25, wherein t is the thickness of the lithium aluminum silicate glass.

[0010] A method for preparing lithium aluminosilicate glass, comprising:

[0011] 49-67wt% SiO2, 12-27wt% Al2O3, 0-3.5wt% B2O3, 2-5.5wt% Li2O, 0.5-13.5wt% Na2O, 0-3.5wt% K2O, 0-4.5wt% MgO, 0-3.5wt% ZnO, 0-2wt% CaO, 0-2wt% SrO, 1.5-14wt% P2O5, 0-1wt% ZrO2, 0-9wt% Y2O3 and 0-0.5wt% SnO are mixed according to the mass percentage of oxides, melted, clarified, homogenized, molded and annealed to obtain a glass sample; RO is the sum of the mass percentages of MgO, ZnO, CaO and SrO in the glass composition, and RO is 0-4.5%;

[0012] Cutting and polishing the glass sample to obtain glass products;

[0013] subjecting the glass article to a first strengthening in a first mixed molten salt;

[0014] Strengthening the glass product after the first strengthening for a second time in a second mixed molten salt to complete the preparation of lithium aluminosilicate glass;

[0015] Wherein, the first mixed molten salt and the second mixed molten salt are both mixed molten salts of NaNO3 and KNO3.

[0016] Furthermore, in the first mixed molten salt, NaNO3 is 36-100wt%, and the rest is KNO3.

[0017] Furthermore, in the second mixed molten salt, KNO3 is 95-100wt%, and the rest is NaNO3.

[0018] Furthermore, the temperature of the first strengthening is 380° C. to 470° C., and the time is 90 to 360 minutes.

[0019] Furthermore, the temperature of the second strengthening is 380° C. to 460° C., and the time is 15 to 180 minutes.

[0020] Furthermore, the thickness of the glass product is ≥0.4 mm and ≤2 mm.

[0021] A lithium aluminosilicate glass is prepared by the above method.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The lithium aluminosilicate glass of the present invention comprises the following raw material components in terms of the mass percentage of oxides:

[0024] 49-67wt% SiO2, 12-27wt% Al2O3, 0-3.5wt% B2O3, 2-5.5wt% Li2O, 0.5-13.5wt% Na2O, 0-3.5wt% K2O, 0-4.5wt% MgO, 0-3.5wt% ZnO, 0-2wt% CaO, 0-2wt% SrO, 1.5-14wt% P2O5, 0-1wt% ZrO2, 0-9wt% Y2O3 and 0-0.5wt% SnO; wherein RO is the sum of the mass percentages of MgO, ZnO, CaO and SrO in the glass composition, and RO is 0-4.5%. Among them, SiO2 network former oxide is the main component of glass. The basic structural unit is silicon-oxygen tetrahedron [SiO4], which is connected in a vertex manner. It is the main network structure of the glass and gives the glass a certain intrinsic strength. When its content is relatively high, the high degree of network connection will increase the viscosity of the glass and increase the difficulty of melting. At the same time, the proportion of silicon-oxygen skeleton structure is relatively high, and the network gap is relatively small, which is not conducive to ion exchange during chemical strengthening and affects the efficiency of chemical strengthening. Therefore, the range of SiO2 content in the present invention needs to be controlled within 49-67wt%; Al2O3 is a glass network intermediate. When the content of alkali metals and alkaline earth metals in the glass is relatively high, Al 3+It tends to become glass aluminum oxide tetrahedron [AlO4], replacing part of [SiO4] to form a network structure, participate in the network composition, and improve the intrinsic strength of the material; in addition, the volume of [AlO4] is greater than the volume of [SiO4], so when the Al2O3 content is high, it is conducive to ion exchange. However, if the Al2O3 content is too high, on the one hand, the high-temperature viscosity of the glass will also increase significantly, making the glass difficult to melt. On the other hand, as one of the main components of lithium aluminum silicate glass, the increase in aluminum content will also increase the crystallization tendency of the glass. Therefore, the range of Al2O3 content in the present invention needs to be controlled within 12 to 27wt%. Li2O, as a flux, can significantly reduce the high-temperature viscosity at high temperatures and improve the solubility and formability of the glass. At the same time, it is an important component of lithium aluminum silicate glass and one of the ion exchange components. When the Li2O content is high, it not only increases the cost of glass manufacturing, but also significantly increases the thermal expansion coefficient of the glass, and because Li + The accumulation of Na2O increases the tendency of glass crystallization, making the glass prone to devitrification. Therefore, the content of Li2O in the present invention needs to be controlled within the range of 2 to 5.5wt%. Na2O is an oxide outside the glass network, which can provide "free oxygen" to destroy the network structure of the glass, thereby reducing the viscosity and melting temperature of lithium aluminum silicate glass. In addition, Na2O is an important element for ion exchange in chemical strengthening. When the content of Na2O is too high, the thermal expansion coefficient will increase, the chemical stability will be reduced, and Na2O is easy to volatilize, resulting in uneven glass composition. When the content of Na2O is too low, it is not conducive to the melting and molding of the glass, as well as Na + With K + The ion exchange thus cannot achieve the purpose of enhancing the mechanical strength of the glass. Comprehensively considered, the range of the Na2O content of the present invention needs to be controlled within 0.5-13.5wt%. K2O and Na2O are both alkali metal oxides and have similar functions in the glass structure. In addition, there is a "mixed alkali effect" between K2O and Na2O, which has a certain effect on improving a series of properties of the glass. K2O also has a certain effect on lowering the liquidus temperature of the glass. Therefore, the content of K2O in the present invention is in the range of 0-3.5wt%. B2O3 is a glass network former. It exists as a triangle [BO3] during high-temperature melting, which reduces the high-temperature viscosity of the glass. At low temperatures, it can capture free oxygen to form a tetrahedron [BO4], making the structure tend to be compact, improving the chemical stability and thermal stability of the glass, and improving the mechanical strength of the glass. When the amount of B2O3 introduced is too high, the Young's modulus and acid resistance of the glass decrease. In addition, B2O3 can form a dense network structure, affecting ion migration, thereby significantly reducing the ion exchange capacity of the glass. Therefore, the content of B2O3 in the present invention needs to be controlled within the range of 0-3.5wt%. MgO is an oxide outside the glass network, which helps to improve the glass meltability, reduce the high temperature viscosity of the glass, and promote the melting and clarification of the glass. However, since its ionic radius is close to that of alkali metal ions and has a larger charge, MgO2+ The ionic potential energy is also large, so in the chemical strengthening process, Mg 2+ It will hinder the ion exchange of Li-Na and Na-K. Therefore, the range of MgO content in the present invention needs to be controlled within 0-4.5wt%. The effect of ZnO is similar to that of MgO. In the process of chemical strengthening, it also has a significant hindering effect on ion exchange. Therefore, the range of ZnO content in the present invention needs to be controlled within 0-3.5wt%. CaO, as a network exo-oxide, can improve the chemical stability of glass and reduce high-temperature viscosity, as well as improve ion exchange capacity and improve Young's modulus of glass. However, if the CaO content is too high, the glass material will become shorter and the brittleness will increase. Therefore, the range of CaO content in the present invention needs to be controlled within 0-2wt%. SrO belongs to the network exo-oxide, which has the effect of improving the chemical stability of glass, accelerating glass melting, and lowering the liquidus temperature. The introduction of SrO in glass in an appropriate amount will improve the mechanical properties of glass, such as hardness and anti-fracture. However, when the SrO content is too high, the clarification effect will be worse and the glass density will increase. Therefore, the range of SrO content in the present invention is controlled within 0-2wt%. Y2O3 belongs to rare earth metal oxides, intermediate oxides, and the introduction of an appropriate amount of Y2O3 can improve the toughness of glass, increase the Young's modulus and hardness of glass. However, the introduction of Y2O3 will increase the crystallization tendency of lithium aluminum silicon glass system and reduce the manufacturability of glass. The content of Y2O3 in the present invention needs to be controlled within the range of 0-9wt%, more preferably 0-3wt%. ZrO2 can improve the fracture toughness value of glass, but when the content is too high, it will increase the crystallization tendency of glass. Therefore, the content of ZrO2 in the present invention needs to be controlled within the range of 0-1wt%. P2O5 belongs to glass network former oxides, which are interconnected into a network with [PO4] tetrahedrons and have a layered structure, which is beneficial to ion exchange in chemical strengthening and has damage resistance. However, a large content of P2O5 is not conducive to the chemical stability of the glass surface and increases the tendency of glass devitrification. Taking all factors into consideration, the content of P2O5 in the present invention needs to be controlled within the range of 1.5-14wt%. In addition to the above-mentioned oxides, the glass of the present invention contains a chemical clarifier, in which the SnO concentration is controlled at about 0-0.5wt%. The present invention obtains lithium aluminum silicate glass with excellent comprehensive performance through a specific combination of components, improves the chemical strengthening effect of the glass, and better serves as a glass cover to protect smart terminal products. Among them, RO is the sum of the mass percentages of MgO, ZnO, CaO and SrO in the glass composition, and satisfies MgO+ZnO+CaO+SrO is 0-4.5%. By optimizing the components of lithium aluminum silicate glass, the glass is chemically strengthened, and the stability and other properties of the glass are not affected. Under the condition, the components of the lithium aluminum silicate glass are adjusted to promote ion exchange, and a thicker composite compressive stress layer is formed on the surface of the glass, thereby improving the strength of the glass, improving the surface compressive stress, anti-bending performance and anti-drop performance.

[0025] The present invention also provides a method for preparing lithium aluminosilicate glass, which comprises mixing raw material components, melting, clarifying, homogenizing, molding, annealing, cutting, and polishing to obtain a glass product; then, the glass product is strengthened twice in a first mixed molten salt in sequence to complete the preparation of the lithium aluminosilicate glass. The present invention uses a mixed molten salt of NaNO3 and KNO3 to perform two-step chemical strengthening on the lithium aluminosilicate glass, which utilizes small ions in the glass to exchange ions with large ions in the salt bath to generate compressive stress (CS) and a compressive stress layer (DOL) on the glass surface. That is, Li in the glass + and Na + With Na in salt bath + and K + Li-Na, Na-K and a small amount of Li-K exchange are carried out to form a compressive stress layer on the glass surface, thereby increasing the mechanical strength and impact resistance of the glass. Although the traditional one-step chemical strengthening method can obtain a higher CS, the DOL is shallow, resulting in poor impact resistance of the glass. The DOL can be increased by prolonging the ion exchange time, but at the same time, the CS is rapidly reduced due to stress relaxation, making it difficult to reach the ideal value. The two-step chemical strengthening method of the present invention can increase the DOL value of the glass surface, and keep the maximum CS value near the glass surface, so that the glass's anti-fall and anti-drop performance is greatly improved. The first chemical strengthening makes the Na in the molten salt + (r=0.098nm) and Li in glass + (r=0.078nm) to exchange and obtain extremely deep DOL; the second strengthening, K in the molten salt + (r = 0.133nm) The Na that entered the glass during the first chemical strengthening + By exchanging them, a higher CS is obtained, thereby further improving the mechanical properties and drop resistance of lithium aluminosilicate glass.

[0026] The present invention also provides a lithium aluminum silicate glass prepared by the above preparation method, which has a larger surface compressive stress and a deeper compressive stress layer, and thus has better mechanical properties and drop resistance. According to testing, the glass can drop 1500mm in a directional manner on 180-mesh sandpaper. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a schematic flow chart of a method for preparing lithium aluminosilicate glass. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0029] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0030] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0031] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0032] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0033] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0034] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0035] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0036] The present invention discloses a method for chemically strengthening lithium aluminosilicate glass, which comprises the following raw material components in terms of mass percentage of oxides:

[0037] 49-67wt% SiO2, 12-27wt% Al2O3, 0-3.5wt% B2O3, 2-5.5wt% Li2O, 0.5-13.5wt% Na2O, 0-3.5wt% K2O, 0-4.5wt% MgO, 0-3.5wt% ZnO, 0-2wt% CaO, 0-2wt% SrO, 1.5-14wt% P2O5, 0-1wt% ZrO2, 0-9wt% Y2O3 and 0-0.5wt% SnO; wherein RO is the sum of the mass percentages of MgO, ZnO, CaO and SrO in the glass composition, and RO is 0-4.5%.

[0038] After testing, the surface compressive stress CS is ≥800MPa, the compressive stress layer DOL is ≥100μm, 0.15≤DOL / t≤0.25, where t is the thickness of lithium aluminum silicate glass.

[0039] See also Figure 1 The present invention provides a method for preparing lithium aluminosilicate glass, comprising:

[0040] S1: According to the mass percentage of oxides, 49-67wt% SiO2, 12-27wt% Al2O3, 0-3.5wt% B2O3, 2-5.5wt% Li2O, 0.5-13.5wt% Na2O, 0-3.5wt% K2O, 0-4.5wt% MgO, 0-3.5wt% ZnO, 0-2wt% CaO, 0-2wt% SrO, 1.5-14wt% P2O5, 0-1wt% ZrO2, 0-9wt% Y2O3 and 0-0.5wt% SnO are mixed, melted, clarified, homogenized, molded, annealed, and a glass sample is obtained;

[0041] S2: cutting and polishing the glass sample to obtain a glass product; the thickness of the glass product is ≥0.4 mm and ≤2 mm;

[0042] S3: subjecting the glass product to a first strengthening in the first mixed molten salt; the first strengthening temperature is 380° C. to 470° C., and the time is 90 to 360 min;

[0043] S4: Strengthening the glass product after the first strengthening for a second time in a second mixed molten salt to complete the preparation of lithium aluminosilicate glass; the temperature of the second strengthening is 380° C. to 460° C., and the time is 15 to 180 minutes;

[0044] Among them, the first mixed molten salt and the second mixed molten salt are both mixed molten salts of NaNO3 and KNO3; in the first mixed molten salt, NaNO3 is 36-100wt% and the rest is KNO3, and in the second mixed molten salt, KNO3 is 95-100wt% and the rest is NaNO3.

[0045] In order to further verify the beneficial effects of the present invention, 36 embodiments are provided, and the lithium aluminum silicate glass prepared by the 36 embodiments is further verified. The strengthened glass products prepared by the 36 embodiments are sequentially subjected to sandpaper drop by using a simulated whole machine drop tester, using a 180g steel plate, 180 mesh sandpaper, directional drop, and a starting height of 400mm. If the sample does not break, it is raised 100mm each time for a limit test. The content of each component in the embodiment and the corresponding test results are shown in the following table:

[0046]

[0047]

[0048]

[0049]

[0050]

[0051]

[0052]

[0053]

[0054] It can be seen that after secondary strengthening, the lithium aluminum silicate glass prepared by this method has a compressive stress CS ≥ 800MPa on the surface, a compressive stress layer DOL ≥ 100μm, and has a high drop resistance ≥ 800mm, which is better suitable for various display protective glasses.

[0055] The present invention provides a lithium aluminum silicate glass, which is prepared by the above method. The glass has a larger surface compressive stress and a deeper compressive stress layer, and thus has more excellent mechanical properties and drop resistance. According to testing, the glass can drop 1500 mm in a directional manner on 180-mesh sandpaper.

[0056] In summary, the present invention provides a lithium aluminosilicate glass and a preparation method thereof, wherein the components of the lithium aluminosilicate glass are adjusted so that the glass is chemically strengthened, and under the condition that the stability and other properties of the glass are not affected, the components of the lithium aluminosilicate glass are adjusted to promote ion exchange, and a thicker composite compressive stress layer is formed on the surface of the glass, thereby improving the strength of the glass, improving the surface compressive stress, bending resistance, and drop resistance, etc. Through secondary strengthening, small ions in the glass are used to exchange ions with large ions in the salt bath to generate compressive stress (CS) and a compressive stress layer (DOL) on the surface of the glass, further improving the mechanical properties and drop resistance of the lithium aluminosilicate glass.

[0057] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.

Claims

1. A lithium aluminosilicate glass, characterized in that: Calculated by mass percentage of oxides, the raw material components include the following: 49-67wt% SiO2, 12-27wt% Al2O3, 0-3.5wt% B2O3, 2-5.5wt% Li2O, 0.5-13.5wt% Na2O, 0-3.5wt% K2O, 0-4.5wt% MgO, 0-3.5wt% ZnO, 0-2wt% CaO, 0-2wt% SrO, 1.5-14wt% P2O5, 0-1wt% ZrO2, 0-9wt% Y2O3 and 0-0.5wt% SnO; RO is the sum of the mass percentages of MgO, ZnO, CaO and SrO in the glass composition, and RO is 0-4.5%.

2. The lithium aluminosilicate glass according to claim 1, characterized in that: Its surface compressive stress CS ≥ 800MPa, and its directional drop height on 180-mesh sandpaper is ≥ 800mm.

3. The lithium aluminosilicate glass according to claim 1, characterized in that: The compressive stress layer DOL is ≥100 μm, 0.15≤DOL / t≤0.25, wherein t is the thickness of the lithium aluminum silicate glass.

4. A method for preparing lithium aluminosilicate glass, characterized in that: include: 49-67wt% SiO2, 12-27wt% Al2O3, 0-3.5wt% B2O3, 2-5.5wt% Li2O, 0.5-13.5wt% Na2O, 0-3.5wt% K2O, 0-4.5wt% MgO, 0-3.5wt% ZnO, 0-2wt% CaO, 0-2wt% SrO, 1.5-14wt% P2O5, 0-1wt% ZrO2, 0-9wt% Y2O3 and 0-0.5wt% SnO are mixed according to the mass percentage of oxides, melted, clarified, homogenized, molded and annealed to obtain a glass sample; RO is the sum of the mass percentages of MgO, ZnO, CaO and SrO in the glass composition, and RO is 0-4.5%; Cutting and polishing the glass sample to obtain glass products; subjecting the glass article to a first strengthening in a first mixed molten salt; Strengthening the glass product after the first strengthening for a second time in a second mixed molten salt to complete the preparation of lithium aluminosilicate glass; Wherein, the first mixed molten salt and the second mixed molten salt are both mixed molten salts of NaNO3 and KNO3.

5. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: In the first mixed molten salt, NaNO3 accounts for 36 to 100 wt%, and the remainder is KNO3.

6. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: In the second mixed molten salt, KNO3 accounts for 95-100wt% and the remainder is NaNO3.

7. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: The temperature of the first strengthening is 380° C. to 470° C., and the time is 90 to 360 minutes.

8. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: The temperature of the second strengthening is 380° C. to 460° C., and the time is 15 to 180 minutes.

9. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: The thickness of the glass product is ≥0.4 mm and ≤2 mm.

10. A lithium aluminosilicate glass, characterized in that: The method is prepared by any one of claims 4 to 9.

Citation Information

Patent Citations

  • Glass composition, aluminosilicate glass and preparation method of aluminosilicate glass

    CN108793734A

  • Lithium aluminosilicate glass and preparation method thereof

    CN108863050A

  • Chemically strengthened glass and method for producing same

    CN113302167A

  • Chemically strengthened glass article and method for producing same

    CN114929641A

Cited By

  • Composition for anti-crack glass, anti-crack glass as well as preparation method and application of anti-crack glass

    CN119797755A

  • Glass, preparation method and application

    CN119822634A

  • Calcium lithium aluminum silicate glass and preparation method thereof

    CN120136425A

  • Glass product and preparation method thereof, chemically strengthened glass and preparation method thereof, display screen and electronic equipment

    CN121063821A

  • Glass article and method of making, chemically strengthened glass and method of making, display screen, electronic device

    CN121063821B