Artificial inorganic large-flower white stone and preparation method thereof

By using inorganic materials such as cement and quartz sand to prepare artificial big white stone, the problems of high production costs and environmental pollution of big white stone are solved, and environmentally friendly preparation technology is realized, which improves the material performance and aesthetics, and is suitable as a substitute for natural stone. .

CN118955045APending Publication Date: 2024-11-15CHINA STATE CONSTR HAILONG TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017924.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Dahua Baishi has high production costs and high environmental pollution, and lacks environmentally friendly preparation methods.

Method used

The premix is ​​prepared by step-by-step stirring and sieving, followed by vacuum under vacuum. Pressed and molded under conditions, combined with the mold maintenance process, artificial inorganic white stone was prepared.

Benefits of technology

It reduces production costs, improves the flexural properties and compressive strength of the materials, realizes an environmentally friendly preparation process, and significantly improves the aesthetics and customizability of the patterns, is low in cost and environmentally friendly, and is suitable as a substitute for natural stone.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955045A_ABST
    Figure CN118955045A_ABST
Patent Text Reader

Abstract

The invention relates to an artificial inorganic large-flower white stone and a preparation method of the artificial inorganic large-flower white stone. The invention relates to a high-temperature-resistant colored glaze which is prepared from a mixture of the following components in parts by weight: 18-23 parts of cement, 55-63 parts of quartz sand, 1-5 parts of black mineral grains, 1-5 parts of white mirror glass, 5-10 parts of an inorganic admixture, 0.8-1.5 parts of an inorganic pigment, 0.6-1.2 parts of a water reducing agent, 3-6 parts of a toughening agent and 1-3 parts of water. The preparation method has the beneficial effects that the prepared artificial inorganic large-flower white stone has material properties superior to those of natural stone or organic artificial stone, is low in cost, environment-friendly and wide in market application range when being used as a flat replacement product of the natural stone, and can generate good social benefits and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building decoration materials, in particular to an artificial inorganic large flower white stone and a preparation method thereof. Background Art

[0002] As a high-end decorative stone, Dahua White Stone is a classic white stone variety from Italy, which is favored by designers for its unique aesthetic characteristics. Its base is usually pure white, with occasional delicate light gray mesh. This elegant gray texture gives the stone a natural sense of flow and rich visual layers, showing an artistic atmosphere that is both low-key and elegant. The Dahua White Stone slab market has developed rapidly in recent years, and has attracted close attention from investors and consumers not only in China but also around the world.

[0003] Compared with traditional artificial stone and some natural stones, inorganic artificial stone has significant advantages in many aspects: environmental protection and safety, strong durability, good stability and customization. Inorganic artificial stone is widely used in many fields such as kitchen countertops, bathroom countertops, floors, wall decoration and outdoor landscape design. It is an ideal choice for modern architectural decoration that pursues environmental protection, durability and beauty. With the continuous advancement of technology and the growing market demand for environmentally friendly materials, inorganic artificial stone is gradually becoming an important development trend in the stone industry.

[0004] At present, the application of large flower white stone is mainly in two forms: large flower white natural stone or sintered imitation large flower white ceramic tile. However, with the continuous mining of large flower white natural stone, natural stone is gradually exhausted. In addition, the mining process of natural stone has a large loss of raw materials, low efficiency and great environmental pollution. In addition, the current requirements of green environmental protection have caused the cost of natural stone to rise sharply. Imitation large flower white ceramic tiles need to be sintered. The high pollution, high emissions and high energy consumption in the sintering process are contrary to the current concept of building a resource-saving and eco-friendly society. At the same time, high temperature firing, circulating water cooling, exhaust gas and solid waste emissions all increase the cost of ceramic tiles.

[0005] In the field of inorganic artificial stone, there is no preparation method for large flower white stone. Summary of the invention

[0006] 1. Technical issues to be resolved

[0007] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides an artificial inorganic large flower white stone and a preparation method thereof, which solves the technical problems of the existing large flower white stone having high production cost, serious environmental pollution and lack of environmentally friendly preparation method.

[0008] (II) Technical solution

[0009] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0010] In the first aspect, an embodiment of the present invention provides an artificial inorganic large flower white stone, which is prepared from a mixture including the following components in parts by weight: 18-23 parts of cement, 55-63 parts of quartz sand, 1-5 parts of black mineral particles, 1-5 parts of white mirror glass, 5-10 parts of inorganic admixtures, 0.8-1.5 parts of inorganic pigments, 0.6-1.2 parts of water reducer, 3-6 parts of toughening agent and 1-3 parts of water.

[0011] The jet-black mineral particles are jet-black mineral particles, and there is no restriction on the specific mineral types; the white mirror glass particles are white, transparent or translucent glass particles.

[0012] As a preferred embodiment of the present invention, the solid content of the toughening agent in the artificial inorganic large flower white stone is 40%-50%, and the remaining components are water; in the mixture, the weight ratio of the inorganic admixture to the toughening agent is 1-1.5:1.

[0013] As a preferred embodiment of the present invention, the artificial inorganic large flower white stone, the cement is white silicate cement; the water reducer is polycarboxylic acid water reducer; the inorganic admixture includes a combination of calcium powder and white silica fume and / or kaolin; the particle size of the inorganic admixture is 320-350 mesh.

[0014] As a preferred embodiment of the present invention, the artificial inorganic large flower white stone, the inorganic pigments include titanium dioxide, iron yellow, iron red and iron black in a preset weight ratio, and the preset weight ratio is equal to the area ratio occupied by the colors of the corresponding four pigments in the large flower white stone; the inorganic admixture is calcium powder and white silica fume mixed in a weight ratio of 1:3, or calcium powder and kaolin mixed in a weight ratio of 1:3, or calcium powder, white silica fume and kaolin mixed in a weight ratio of 1:3:3.

[0015] The area ratios of the four pigment colors are obtained by surface judgment, and the specific method for area calculation refers to the prior art.

[0016] As a preferred embodiment of the present invention, the artificial inorganic white stone has a toughening agent of styrene-butadiene emulsion; the total water content of the mixture including the water content in the toughening agent accounts for 1.5%-5% of the total weight of the mixture.

[0017] As a preferred embodiment of the present invention, the artificial inorganic large flower white stone, the particle size range of quartz sand includes 4-6 mesh, 6-8 mesh, 8-16 mesh, 16-26 mesh, 26-40 mesh and 40-70 mesh, and the weight ratio of quartz sand with corresponding particle size is 5-10:6-15:10-15:5-15:6-15:8-13; the particle size range of jet black mineral particles includes 16-26 mesh and 26-40 mesh, and the weight ratio of the two particle sizes of jet black mineral particles is 4:1; the particle size range of white mirror glass includes 8-16 mesh and 16-30 mesh, and the weight ratio of the two particle sizes of white mirror glass is 1:1.

[0018] Among them, when the endpoint values ​​of the particle size interval coincide, the upper limit values ​​are not included in this interval.

[0019] In a second aspect, an embodiment of the present invention provides a method for preparing the artificial inorganic large flower white stone according to the first aspect, comprising the following steps:

[0020] S1. Preparing premixes containing different inorganic pigments respectively: according to the number of colors n of the inorganic pigments, quartz sand, inorganic admixtures, cement, water reducer, water, and toughening agent are divided into n parts, n ≥ 3; taking an inorganic pigment of one color and stirring and mixing with one part of quartz sand each time, then adding one part of inorganic admixture and one part of cement, stirring and mixing, then adding a mixed solution of one part of water reducer and one part of water, stirring and adding one part of toughening agent, stirring evenly, and preparing a premix containing the inorganic pigment of the color; preparing n kinds of premixes containing inorganic pigments of different colors respectively in the above manner;

[0021] S2, sieving to prepare a mixture: taking any one or two inorganic pigment premixes in S1 and pre-sieving them, then sequentially adding the remaining inorganic pigment premixes, black mineral particles and white mirror glass, mixing and sieving them for a second time to prepare a mixture;

[0022] S3, pressing: putting the mixed material into a mold under vacuum conditions to press and form a rough board;

[0023] S4. Curing: The rough board is subjected to mold curing and demolding curing in turn to complete the preparation of the inorganic large flower white stone.

[0024] As a preferred embodiment of the present invention, in the method for preparing the artificial inorganic large flower white stone, in S2, the screening method is vibration screening, the sieve hole diameter is 9-10mm, and the pre-screening and secondary screening are completed within 8 minutes in total.

[0025] The usage ratio of the corresponding pigments in each premix is ​​determined by the area ratio of the corresponding pigments in the Dahua white stone. The usage ratio of each material other than the pigment in the premix is ​​also consistent with the usage ratio of the pigment. For example, if the usage ratio of the two pigments in the first premix and the second premix is ​​A:B, then the ratio of each other component in the premix between the two premixes is also A:B; and so on for multiple premixes.

[0026] In addition, in step S2, vibration screening, pre-screening and secondary screening are completed within 8 minutes in total, which can ensure uniform dispersion between premixes and avoid cross-color discoloration between premixes as much as possible.

[0027] As a preferred embodiment of the present invention, in the method for preparing the artificial inorganic large flower white stone, in S3, the vacuum degree is -0.09 to -1.00MPa, the pressure holding time is 3-4min, and the pressure is 15-17MPa; the pressing vibration frequency is set to 20-25Hz, 30-35Hz and 45-50Hz respectively, and the duration corresponding to each vibration frequency is equal.

[0028] As a preferred embodiment of the present invention, in the method for preparing the artificial inorganic large flower white stone, in S4, the curing temperature is 22-25°C, and the humidity is above 95%; the curing with the mold is 1 day, and the demolding curing is 14-28 days.

[0029] (III) Beneficial effects

[0030] The beneficial effects of the present invention are as follows: an artificial inorganic large flower white stone and a preparation method thereof of the present invention use inorganic admixtures as the main filler, and utilize the good fluidity of the toughening agent to fully disperse the inorganic admixtures, so that the prepared artificial inorganic large flower white stone has significantly improved anti-bending performance. At the same time, controlling the amount of water added can not only satisfy the cement hydration effect, but also facilitate the vacuum pressing process and improve the compressive strength of the artificial stone. Based on the above, the overall material adopts inorganic materials with a wide range of sources, the production cost is reduced, and the prepared inorganic artificial stone material has significant advantages in properties. The black ore particles and the white mirror glass are matched, and the inorganic pigments in a specific proportion are mixed step by step to ensure the beauty and customizability of the inorganic large flower white stone pattern. Compared with the prior art, the present invention provides a production formula and method of large flower white stone, and the prepared artificial inorganic large flower white stone has material properties that are superior to natural stone or organic artificial stone. As a substitute for natural stone, it has low cost, environmental friendliness and a wide range of market applications, and can produce good social and economic benefits.

[0031] The inorganic admixture and the toughening agent are set in a specified ratio, which can give full play to the dispersing effect of the toughening agent, thereby improving the flexural properties of the inorganic large flower white stone and saving the amount of raw materials.

[0032] The inorganic admixture is a combination of calcium powder and white silica fume and / or metakaolin, wherein the main component of calcium powder is CaCO3. White silica fume contains a large amount of amorphous silicon dioxide. When it reacts with calcium in the system, it will produce more calcium silicate hydrate (CSH), thereby enhancing the structural strength of artificial stone, reducing porosity and improving its durability. Metakaolin is composed of Al2O3 and SiO2. When it reacts with calcium in the system, in addition to generating CSH, it will also form calcium aluminate hydrate (CAH) and calcium sulfoaluminate hydrate (CASH). These hydration products fill the pores of the material, improve the density and strength of artificial stone, and also improve its impermeability and chemical corrosion resistance, extending the service life of artificial stone. Among them, when the inorganic admixture is calcium powder, white silica fume and kaolin mixed in a weight ratio of 1:3:3, the corresponding inorganic large flower white stone has the best performance, with the maximum average flexural strength after 28 days reaching 15.8MPa, and the maximum average flexural strength after 28 days reaching 83.2MPa.

[0033] In addition, the particle size of inorganic admixture is 320-350 mesh, and the reactivity between the components is high. An appropriate amount of calcium powder is added to the cement, which helps to prevent the occurrence of alkali-aggregate reaction in the system.

[0034] Inorganic pigments include titanium dioxide, iron yellow, iron red and iron black in a preset weight ratio. These four inorganic colors are combined and adjusted in steps. The debugging result is closer to the color tone of natural white stone. At the same time, the color can be fine-tuned as needed to meet different customization needs. Inorganic colors are stable in nature and not easy to fade.

[0035] The total amount of water in the preparation component system, including the water in the toughening agent, accounts for 1.5%-5% of the total weight of the preparation component system. Strictly controlling the amount of water within this range can prevent excessive water from affecting the overall strength of the artificial stone material during the subsequent pressing process.

[0036] The quartz sand is continuously graded in the range of 40-70 mesh, and the larger quartz sand is used as aggregate. At the same time, the jet black ore particles are continuously graded in the range of 16-40 mesh, and the white mirror glass particles are continuously graded in the range of 8-30 mesh. Under the premise of meeting the strength of artificial stone materials, it presents the texture of natural large flower white stone and meets the appearance requirements.

[0037] During the mixing process, different inorganic pigments are mixed with other materials to form a premix, and then the premix is ​​quickly mixed by vibration screening to prevent excessive cross-over between colors and ensure the color of the inorganic large flower white stone. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1This is a picture of the artificial inorganic large flower white stone prepared in Example 1 of the artificial inorganic large flower white stone and its preparation method of the present invention. DETAILED DESCRIPTION

[0039] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0040] An artificial inorganic large flower white stone and a preparation method thereof proposed in an embodiment of the present invention are aimed at the technical problems that the production cost of large flower white stone is high, the environmental pollution is large, and there is still a lack of environmentally friendly preparation methods; inorganic admixtures are used as the main filler, and the good fluidity of the toughening agent is utilized to fully disperse the inorganic admixtures, and the prepared artificial inorganic large flower white stone has significantly improved anti-bending performance. At the same time, the amount of water added is controlled, which can not only meet the cement hydration effect, but also facilitate the vacuum pressing process and improve the compressive strength of the artificial stone. Based on the above, the overall material adopts inorganic materials with a wide range of sources, the production cost is reduced, and the prepared inorganic artificial stone material has significant advantages in properties. The black ore particles and white mirror glass are matched, and the inorganic pigments used in a specific proportion are mixed step by step to ensure the beauty and customizability of the inorganic large flower white stone pattern. The present invention provides a production formula and method of large flower white stone, and the prepared artificial inorganic large flower white stone has material properties that are superior to natural stone or organic artificial stone. As a substitute for natural stone, it has low cost, environmental friendliness and a wide range of market applications, and can produce good social and economic benefits.

[0041] In order to better understand the above technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a clearer and more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.

[0042] Example 1

[0043] This embodiment provides an artificial inorganic large flower white stone and a preparation method thereof, and the specific steps are as follows:

[0044] (1) According to the following formula: 23 parts by weight of cement, 60 parts by weight of quartz sand, 3 parts by weight of black mineral particles, 3 parts by weight of white mirror glass, 6 parts by weight of inorganic admixture, 1.5 parts by weight of inorganic pigment (after mixing), 1 part by weight of water reducer, 5 parts by weight of toughening agent and 1.5 parts by weight of water; wherein the weight ratio of titanium dioxide, iron yellow, iron red and iron black in the inorganic pigment is 14:3:2:1;

[0045] According to the ratio of 14:3:2:1, the other components except inorganic pigments, black mineral particles and white mirror glass are divided into 4 parts to be mixed, corresponding to the 4 pigments of titanium dioxide, iron yellow, iron red and iron black; among which, the usage ratio of the four colors is equal to the area proportion of the corresponding four colors in the large flower white stone;

[0046] The inorganic admixtures are calcium powder, white silica fume and kaolin mixed in a weight ratio of 1:3:3.

[0047] In addition, the quartz sand used has a particle size of 4-6 mesh 8 parts, 6-8 mesh 10 parts, 8-16 mesh 12 parts, 16-26 mesh 10 parts, 26-40 mesh 9 parts, and 40-70 mesh 11 parts by weight; the particle size range of the jet black ore particles is 16-26 mesh and 26-40 mesh, and the weight ratio of the two particle sizes of the jet black ore particles is 4:1; the particle size range of the white mirror glass is 8-16 mesh and 16-30 mesh, and the weight ratio of the two particle sizes of the white mirror glass is 1:1.

[0048] (2) Preparation of premix: Taking the materials to be mixed corresponding to titanium dioxide as an example, the mixing process of each premix is ​​as follows: first, stir and mix quartz sand and titanium dioxide, then add inorganic admixtures and cement and stir and mix, then add the mixed solution of water reducer and water and stir and mix, and finally add toughening agent and stir evenly to prepare a premix containing titanium dioxide inorganic pigment. The preparation method of the premix corresponding to the other three pigments is the same as that of the premix containing titanium dioxide inorganic pigment;

[0049] (3) Sieving to prepare a mixture: first, a premix containing titanium dioxide and a premix containing iron yellow are mixed and pre-screened, and then a premix containing iron red, a premix containing iron black, black ore particles and white mirror glass are added, mixed and screened for a second time to prepare a mixture; a 9.5 mm square hole sieve is selected as the sieve, and the pre-screening and the second screening are completed within 8 minutes in total;

[0050] (4) Pressing: The mixed material is pressed into a mold under vacuum conditions to prepare a rough board. The vacuum degree is -0.095 MPa, the press holding time is 3 minutes, the press pressure is 15 MPa, and the press frequency is 20 Hz vibration for 1 minute, 35 Hz vibration for 1 minute, and 50 Hz vibration for 1 minute;

[0051] (5) Curing: Curing the rough board with mold for 24 hours, and then demolding and curing for 28 days. The curing conditions are 20°C and the humidity is controlled above 95%;

[0052] (6) After the curing is completed, the product is ground and polished to a certain thickness to complete the preparation of the inorganic large flower white stone.

[0053] The performance indicators of the prepared inorganic large flower white stone are shown in Table 1.

[0054] Example 2

[0055] This embodiment provides an artificial inorganic large flower white stone and a preparation method thereof, which is different from Embodiment 1 in that the inorganic admixture is calcium powder and white silica fume mixed in a weight ratio of 1:3.

[0056] The performance indicators of the prepared inorganic large flower white stone are shown in Table 1.

[0057] Example 3

[0058] This embodiment provides an artificial inorganic large flower white stone and a preparation method thereof, which is different from the embodiment 1 in that the inorganic admixture is calcium powder and metakaolin mixed in a weight ratio of 1:3.

[0059] The performance indicators of the prepared inorganic large flower white stone are shown in Table 1.

[0060] Table 1

[0061]

[0062] Refer to Table 1 and Figure 1 , Example 1 is the best example. The surface of the prepared inorganic large flower white stone is smooth, without pores and pockmarks, with a sense of suspended particles on the surface, clear texture, and a transparent and moist surface. At the same time, the average flexural strength of the large flower white stone after 28 days is the largest, reaching 15.8MPa, and the average flexural strength after 28 days is the largest, reaching 83.2MPa.

[0063] Referring to Table 1, the appearance of the inorganic large flower white stone prepared in Example 2 is not much different from that in Example 1, but because there is no kaolin in the inorganic admixture, the average flexural strength and the average compressive strength are both lower than those in Example 1.

[0064] Referring to Table 1, the average flexural strength and average compressive strength of the inorganic large flower white stone prepared in Example 3 are both lower than those in Example 1 and Example 2.

[0065] The inorganic large flower white stone prepared in the above three groups of embodiments, without adding fiber substances, still has an average flexural strength of more than 15 MPa, and has excellent flexural performance.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An artificial inorganic large flower white stone, characterized in that: The mixture is prepared from the following components in parts by weight: 18-23 parts of cement, 55-63 parts of quartz sand, 1-5 parts of black mineral particles, 1-5 parts of white mirror glass, 5-10 parts of inorganic admixtures, 0.8-1.5 parts of inorganic pigments, 0.6-1.2 parts of water reducer, 3-6 parts of toughening agent and 1-3 parts of water.

2. The artificial inorganic large flower white stone according to claim 1, characterized in that: The solid content of the toughening agent is 40%-50%, and the remaining component is water; In the mixture, the weight ratio of the inorganic admixture to the toughening agent is 1-1.5:

1.

3. The artificial inorganic large flower white stone according to claim 1 or 2, characterized in that: The cement is white Portland cement; The water reducer is a polycarboxylate water reducer; Inorganic admixtures include calcium powder in combination with white silica fume and / or metakaolin; The particle size of the inorganic admixture is 320-350 mesh.

4. The artificial inorganic large flower white stone according to claim 3, characterized in that: The inorganic pigments include titanium dioxide, iron yellow, iron red and iron black in a preset weight ratio, wherein the preset weight ratio is equal to the area ratio of the colors of the four pigments in the large flower white stone; The inorganic admixture is calcium powder and white silica fume mixed in a weight ratio of 1:3, or calcium powder and kaolin mixed in a weight ratio of 1:3, or calcium powder, white silica fume and kaolin mixed in a weight ratio of 1:3:

3.

5. The artificial inorganic large flower white stone according to claim 2, characterized in that: The toughening agent is styrene-butadiene emulsion; The total water content in the mixture, including the water content in the toughening agent, accounts for 1.5% to 5% of the total weight of the mixture.

6. The artificial inorganic large flower white stone according to claim 1, characterized in that: The particle size ranges of quartz sand include 4-6 mesh, 6-8 mesh, 8-16 mesh, 16-26 mesh, 26-40 mesh and 40-70 mesh, and the weight ratio of quartz sand of corresponding particle sizes is 5-10:6-15:10-15:5-15:6-15:8-13; The particle size range of the black ore particles includes 16-26 mesh and 26-40 mesh, and the weight ratio of the two particle sizes of the black ore particles is 4:1; The particle size range of white mirror glass includes 8-16 mesh and 16-30 mesh, and the weight ratio of the two particle sizes of white mirror glass is 1:

1.

7. A method for preparing the artificial inorganic large flower white stone according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Preparing premixes containing different inorganic pigments respectively: According to the number of colors n of the inorganic pigment, quartz sand, inorganic admixture, cement, water reducer, water, and toughening agent are divided into n portions respectively, n ≥ 3; Each time, one color of inorganic pigment is mixed with one part of quartz sand, and then one part of inorganic admixture and one part of cement are added, and then a mixed solution of one part of water reducing agent and one part of water is added, and after stirring, one part of toughening agent is added, and stirred evenly to prepare a premix containing the inorganic pigment of the color; According to the above method, n kinds of premixes containing inorganic pigments of different colors are prepared; S2, sieving to prepare a mixture: taking any one or two inorganic pigment premixes in S1 and pre-sieving them, then sequentially adding the remaining inorganic pigment premixes, black mineral particles and white mirror glass, mixing and sieving them for a second time to prepare a mixture; S3, pressing: putting the mixed material into a mold under vacuum conditions to press and form a rough board; S4. Curing: The rough board is subjected to mold curing and demolding curing in turn to complete the preparation of the inorganic large flower white stone.

8. The method for preparing the artificial inorganic large flower white stone according to claim 7, characterized in that: In S2, the screening method is vibration screening, the sieve hole diameter is 9-10mm, and the pre-screening and secondary screening are completed within 8 minutes in total.

9. The method for preparing the artificial inorganic large flower white stone according to claim 7, characterized in that: In S3, the vacuum degree is -0.09 to -1.00 MPa, the holding time is 3-4 min, and the pressure is 15-17 MPa; The suppression vibration frequencies are set to 20-25Hz, 30-35Hz and 45-50Hz respectively, and the duration corresponding to each vibration frequency is equal.

10. The method for preparing the artificial inorganic large flower white stone according to claim 7, characterized in that: In S4, the curing temperature is 22-25°C and the humidity is above 95%; The mold is cured for 1 day, and the demoulding is cured for 14-28 days.