Method for removing alkyne from C3 fraction through selective hydrogenation
The Pd-Pb-P-C single-atom catalyst was prepared by using phosphorus-doped carbon material support and photoreduction method in the selection hydrogenation catalyst of three-fold carbon fractions, and the problems of uneven dispersion of catalyst active components and insufficient coking resistance were solved, achieving high efficiency hydrogenation reaction and safe catalyst operation.
Patent Information
- Application Number
- CN202310532750.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-15
AI Technical Summary
The existing three-fraction selective hydrogenation catalysts have uneven dispersion of active components, insufficient catalyst selectivity and coking resistance during the preparation process, resulting in low hydrogenation reaction efficiency and high safety risks of the device.
Using phosphorus-doped carbon material as a support, the Pd and Pb active components are in atomic dispersion state through photoreduction, forming a Pd-Pb-P-C single atom catalyst, which is used for the selective hydrogenation reaction of three carbon fractions to improve the catalyst Hydrogenation activity and selectivity and reduce the chance of polymerization coking.
The hydrogenation activity, selectivity and anti-coking properties of the catalyst are improved, ensuring efficient operation of the catalyst. Even if the hydrogenation material contains more distillates, the activity and selectivity of the catalyst remain good, reducing the safety risks of the device.
Smart Images

Figure CN118955236A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for selectively hydrogenating a C3 fraction to remove acetylene, belonging to the technical field of catalytic hydrogenation. Background Art
[0002] After the liquid hydrocarbon raw materials such as naphtha are steam cracked and separated, the propylene content in the C3 fraction is generally 70-90% (mol), the propane content is 5-10% (mol), and the propyne (MA) + propadiene (PD) content is 1.5-8.0% (mo1). In the propylene polymerization reaction, MAPD will reduce the activity of the polypropylene catalyst and affect the quality of the polymerization-grade propylene product. In order to remove MAPD from the C3 fraction, the current industry uses catalytic selective hydrogenation and solvent absorption to remove MAPD. Since the catalytic hydrogenation process is simple and has no environmental pollution, the application of catalytic hydrogenation is becoming more and more common. The usual process conditions for the hydrogenation reaction of the C3 fraction are: reactor inlet temperature 20-50°C, reaction pressure 2.2-3.0MPa, liquid phase volume space velocity 15-120h -1 , hydrogen / MAPD (molar ratio) = 1~3.
[0003] In the process flow of pre-hydrogenation of carbon three fractions, that is, the process flow of pre-depropanization and pre-hydrogenation, the cracked gas is washed with oil, water and alkali, and then first passes through the pre-depropanizer. The fractions at the top of the tower include carbon one and hydrogen, carbon two fraction and carbon three fraction. The bottom of the tower is the heavy carbon three fraction. The fraction at the top of the tower enters the carbon two fraction hydrogenation reactor. The carbon two fraction hydrogenation reactor of this process generally adopts a three-stage reactor. The first and second stage reactors are mainly used for the removal of acetylene, and the third stage reactor is used for the removal of propyne and propadiene. Generally, a gas phase hydrogenation process is adopted, and the removal rate of propyne and propadiene is above 50%. After this process, the reaction materials are separated from the carbon three fraction and the carbon one and carbon two fractions. The separated carbon three fraction enters the carbon three fraction hydrogenation reactor after cooling for liquid phase hydrogenation. Since most of the propyne and propadiene have been converted, the hydrogenation load is relatively low, and there are higher requirements for the selectivity of the catalyst. In the existing process, the activity of the catalyst is good in the early stage of catalyst operation. However, when the selectivity of the catalyst is not ideal, due to the excessive rise in reaction temperature and excessive local reaction, it is easy to cause temperature runaway, seriously affecting the safe operation of the device.
[0004] Traditional C3 hydrogenation catalysts generally use Al2O3 as a carrier, Pd as an active component, and Ag as a co-active component. The specific surface area of this catalyst is 15 to 100 m 2 / g. The catalyst is prepared by an impregnation method. During the impregnation and drying process of the catalyst, the surface tension of the impregnation liquid and the solvation effect are particularly obvious, and the metal active component precursor is deposited on the carrier surface in the form of aggregates. In addition, the distribution state between Pd and Ag is not ideal, the catalyst activity is not easy to control, and the selectivity of the catalyst is mainly controlled by the catalyst pore size and the dispersion state of the active component. Since the dispersion of the active component is affected by the number of carrier surface groups and the solvation effect during the catalyst preparation process, the randomness of the dispersion of the catalyst active component is large, and the preparation repeatability is poor, so the effect of the catalytic reaction is not ideal.
[0005] CN102206132A discloses a method for selective hydrogenation of C3 fractions, wherein the catalyst used in the method has Pd as the main active component, alumina as the carrier, and an auxiliary active component Ag. By adsorbing a specific polymer compound on the carrier, a polymer compound coating layer is formed on the carrier surface with a certain thickness, and a compound with a functional group reacts with the polymer compound to make it have a functional group that can be complexed with the active component, and the active component undergoes a complexation reaction on the functional group on the carrier surface to ensure that the active component is orderly and highly dispersed. However, the method has the following disadvantages: the carrier adsorbs a specific polymer compound by chemically adsorbing the hydroxyl group of alumina with the polymer, and the amount of the polymer compound adsorbed by the carrier is limited by the number of hydroxyl groups of alumina; the complexation between the functionalized polymer and Pd is not strong, and sometimes the active component loading amount does not meet the requirements, and some active components remain in the impregnation solution, resulting in an increase in the catalyst cost; the method for preparing a C3 hydrogenation catalyst also has the disadvantage of a complex process flow.
[0006] CN102218323A discloses a hydrogenation catalyst for unsaturated hydrocarbons. The active component of the catalyst is a mixture of 5-15% nickel oxide and 1-10% other metal oxides, the other metal oxides can be one or more of molybdenum oxide, cobalt oxide and iron oxide, and also includes 1-10% of an additive. The catalyst is mainly used to hydrogenate ethylene, propylene, butene and the like in the tail gas of coal-to-oil industry into saturated hydrocarbons, and has good deep hydrogenation capacity. However, the catalyst is mainly used for the full hydrogenation of ethylene, propylene, butene and the like in various industrial tail gases rich in CO and hydrogen, and is not suitable for the selective hydrogenation of alkynes and dienes.
[0007] CN1972885A discloses a selective hydrogenation catalyst for acetylene and diolefins in a light olefin raw material. The catalyst comprises a first component selected from copper, gold, and silver and a second component selected from nickel, platinum, palladium, iron, cobalt, ruthenium, and rhodium, and also comprises at least one inorganic salt and oxide selected from zirconium, lanthanide elements, and alkaline earth metal mixtures, and an inorganic carrier. The catalyst forms a fluorite structure after calcination, use, or regeneration. The catalyst is helped to increase the selectivity of the catalyst and the activity and selectivity after regeneration by adding a third oxide and using modified aluminum oxide or silicon oxide as a carrier. However, the catalyst is still based on copper, gold, silver, palladium, etc. as active components, and nickel, platinum, palladium, iron, cobalt, ruthenium, rhodium, etc. as auxiliary active components, and the regeneration performance of the catalyst is improved by modifying the oxide of the carrier.
[0008] In 2011, Academician Zhang Tao and others from Dalian Institute of Chemical Physics reported Pt1 / FeOx single-atom catalysts, which showed excellent CO oxidation activity and stability, and proposed the new concept of "single-atom catalysis", creating a new field of single-atom catalysis, and related research has attracted much attention. Single-atom catalysts have the following advantages: (1) They integrate the advantages of homogeneous catalysis and heterogeneous catalysis, showing high catalytic activity and high selectivity; (2) They have a simple structure and are ideal catalysts for studying the mechanism of catalytic reactions; (3) Single-atom catalysts show the maximum atomic utilization rate, which has an immediate effect on reducing the cost of precious metal catalysts. At present, single-atom catalysts have shown good development momentum in the fields of oxidation reactions, hydrogenation reactions, water-gas shift, photocatalytic hydrogen production, and electrocatalysis.
[0009] CN106654300A discloses a method for preparing a monodisperse metal atom / graphene composite material by electrochemically swelling graphite, and provides a new method for efficiently preparing a monodisperse metal atom / graphene composite catalyst with controllable types and quantities of metal atoms by electrochemical liquid phase swelling of graphite-based raw materials. The method is an electrochemical stripping method for preparing a monodisperse metal atom / graphene composite material from graphite in one step under milder conditions, and mainly comprises the following steps: (1) making an electrode from a graphite-based raw material; (2) electrolyzing the prepared electrode in an electrolytic cell, separating solid from liquid, and recycling the electrolyte; (3) further stripping the separated solid to obtain a crude monodisperse metal atom / graphene composite material; (4) separating and purifying the crude monodisperse metal atom / graphene composite material to obtain a monodisperse metal atom / graphene composite material; (5) heat treating the composite material obtained in step (4) and / or the composite material uniformly mixed with a non-gaseous nitrogen source under the protection of an inert atmosphere or / and an ammonia atmosphere, and cooling to obtain a monodisperse metal atom / graphene composite catalyst. In this material, the metal is dispersed in the form of single atoms in / on the skeleton of graphene. The type and composition of the central metal atom can be adjusted as needed, and can be divided into mononuclear or binuclear, and the binuclear metal component can be monometallic or bimetallic. The preparation process of this material is simple, efficient, low in energy consumption, and can be mass-produced. However, the document does not describe the content of the metal active component and its metal state. It only prepares a single-atom catalyst, and does not evaluate the catalyst performance for a certain system.
[0010] CN109126857A discloses a metal single atom catalyst based on a carbon nano cage carrier and a preparation method thereof. The metal single atom catalyst based on a carbon nano cage carrier comprises a carbon nano cage carrier and a metal single atom embedded in a microporous channel of a cage wall of the carbon nano cage carrier; the metal single atom is Pt, Pd, Ru, Ir, Ag or Au; the carbon nano cage carrier is a doped carbon nano cage, the loading amount of the metal single atom is below 8wt%, the doped carbon nano cage is a single element doped carbon nano cage or a co-doped carbon nano cage, the single element doped carbon nano cage is an N doped, B doped, S doped or P doped carbon nano cage, the doping amount of P in the P doped carbon nano cage is below 8at%, and the cage wall micropore diameter of the carbon nano cage carrier is 0.4-1.5nm. The preparation method of the metal single atom catalyst comprises: immersing the doped carbon nano cage in a metal precursor solution, and sequentially separating and heat treating to obtain a metal single atom catalyst based on a carbon nano cage carrier; the metal precursor is a water-soluble metal ion compound corresponding to Pt, Pd, Ru, Ir, Ag or Au, the heat treatment temperature is 40-600°C, the heat treatment time is 0.5-24h, the immersion temperature is 0-100°C, and the immersion time is 0.5-50h. The loading amount of the Pd metal single atom in the catalyst is below 8wt%, which has a wide range, a large amount and a high cost.
[0011] CN112808288A discloses a nitrogen-phosphorus or nitrogen-phosphorus-sulfur co-doped carbon-loaded metal single atom catalyst and its microwave-assisted preparation method. The catalyst comprises a carrier and an active component metal loaded on the carrier; the carrier is a nitrogen-phosphorus or nitrogen-phosphorus-sulfur co-doped carbon material, the metal comprises any one of palladium, ruthenium, rhodium, iridium, platinum, iron, cobalt, and nickel, and the metal loading amount in the catalyst is 0.1% to 5% by mass percentage. The preparation method of the catalyst comprises the following steps: (1) phytic acid and any one or a mixture of two or more nitrogen-containing and sulfur-containing organic molecules such as thiourea, urea, melamine, dicyandiamide, cyanuric acid, aniline, and pyrrole are mixed in a certain mass ratio, and placed in a microwave oven for microwave heating, and the obtained black product is a nitrogen-phosphorus or nitrogen-phosphorus-sulfur doped carbon carrier; (2) a certain amount of metal precursor solution is mixed with the carrier and reducing agent in the above step (1), stirred, washed, and dried to obtain the nitrogen-phosphorus or nitrogen-phosphorus-sulfur doped carbon material loaded with metal single atoms catalytic material.
[0012] CN111389437A discloses a molybdenum carbide supported single atom hydrogenation catalyst, a preparation method thereof and its application in the semi-hydrogenation of alkynes. The hydrogenation catalyst comprises: a carrier, the carrier comprises MoC; and a metal single atom, the metal single atom is supported on the carrier, and the metal single atom is chemically bonded to the molybdenum atom in the MoC; wherein the metal single atom comprises at least one of single atom nickel, single atom cobalt and single atom copper.
[0013] CN108250024A discloses a method for hydrogenating a carbon three fraction. The method uses a Fe-Mn catalyst to selectively hydrogenate the carbon three fraction as a hydrogenation raw material after hydrogenation, and converts propyne (MA) and propadiene (PD) in the material into propylene. The carrier of the Fe-Mn catalyst is a high-temperature resistant inorganic oxide, and the active components contain at least Fe and Mn. Based on the total mass of the catalyst as 100%, the catalyst contains 5-15% Fe and 0.5-2% Mn. The specific surface area of the catalyst is 10-300m 2 / g, pore volume is 0.2~0.65mL / g. The catalyst is prepared by impregnating Fe and Mn on a carrier, then calcining and reducing in a hydrogen atmosphere. The reaction conditions for hydrogenating the carbon three fraction using the catalyst are: reactor inlet temperature 30~50℃, reaction pressure 1.5~3.5MPa, liquid phase space velocity 15~120h -1 , hydrogen / MAPD=1-10. The catalyst uses Fe as an active component and does not involve a C3 fraction selective hydrogenation catalyst using Pd as an active component.
[0014] CN106925279A discloses an Fe-based selective hydrogenation catalyst, a preparation method and its application. The active component Fe content of the catalyst is 2-15wt%, the X content is 0-2wt%, X is selected from one or more of K, La and Ce, and the rest is oxygen and a carrier. The catalyst has a specific surface area of 10-300m 2 / g, pore volume is 0.2~0.65mL / g. The catalyst can be used for selective hydrogenation of acetylene, propyne and propadiene (MAPD) in C2~C3 cracking fractions. The document adopts impregnation method to load active components and uses roasting method for metal reduction to prepare a catalyst for selective hydrogenation of C2 and C3, which does not involve single atom catalyst preparation technology.
[0015] Developing a new method for selective hydrogenation of C3 fraction to remove alkynes has become one of the urgent problems to be solved in this field. Summary of the invention
[0016] In order to solve the above technical problems, the object of the present invention is to provide a method for selective hydrogenation of carbon three fractions to remove alkynes. The hydrogenation catalyst used in the method for selective hydrogenation of carbon three fractions provided by the present invention has an active component dispersed on a carrier at the atomic level and has good hydrogenation activity, selectivity and anti-coking performance.
[0017] In order to achieve the above-mentioned object, the present invention provides a method for selective hydrogenation of a C3 fraction to remove acetylene, which comprises the following steps: subjecting the C3 fraction to a selective hydrogenation reaction under the action of a hydrogenation catalyst to convert propyne (MA) and / or propadiene (PD) in the C3 fraction into propylene; wherein the hydrogenation catalyst comprises a carrier and an active component, the carrier is a phosphorus-doped carbon material, the active component comprises a main active component and a co-active component, the main active component comprises Pd, the co-active component comprises Pb, and the main active component and the co-active component are dispersed on the carrier at the atomic level.
[0018] In the above-mentioned method for selective hydrogenation of C3 fraction to remove alkynes, preferably, the hydrogenation reactor used in the selective hydrogenation reaction comprises a single-stage adiabatic fixed bed reactor and / or a two-stage adiabatic fixed bed reactor.
[0019] In the above-mentioned method for selective hydrogenation of C3 fraction to remove acetylene, preferably, the C3 fraction comes from the top of a depropanizer in a propylene preparation process using a sequential separation process. More preferably, the material composition of the C3 fraction from the top of the depropanizer includes, by volume percentage, propylene 70-90%, propane 5-30%, and propyne + propadiene 2.0-5.0%. More specifically, by volume percentage, when propyne + propadiene in the material composition of the C3 fraction from the top of the depropanizer is ≤4.0%, a single-stage adiabatic fixed bed reactor is used for selective hydrogenation reaction; when propyne + propadiene in the material composition of the C3 fraction from the top of the depropanizer is >4.0%, a two-stage adiabatic fixed bed reactor is used for selective hydrogenation reaction. Generally speaking, the material composition of the C3 fraction from the top of the depropanizer tower may also include a small amount of C2 fraction and a small amount of C4 and / or above fractions, and the present invention does not specifically limit their specific contents.
[0020] In the above-mentioned method for selective hydrogenation and acetylene removal of C3 fraction, preferably, the C3 fraction comes from the bottom of the deethanizer in the propylene preparation process using the pre-depropanization pre-hydrogenation process. More preferably, the material composition of the C3 fraction from the bottom of the deethanizer includes: 80-95% propylene, 5-20% propane, 0.05-0.2% propyne, and 0.05-0.2% propadiene in terms of volume percentage. More specifically, a single-stage adiabatic fixed bed reactor is used to selectively hydrogenate the C3 fraction from the bottom of the deethanizer. Generally speaking, the material composition of the C3 fraction from the bottom of the deethanizer may also include a small amount of C2 fraction and a small amount of C4 and / or above fractions, and the present invention does not specifically limit their specific contents.
[0021] In the above-mentioned method for selective hydrogenation of C3 fraction to remove alkynes, preferably, the process conditions of the selective hydrogenation reaction are: hydrogenation reactor inlet temperature 25-55°C, reaction pressure 1.8-4.0 MPa, liquid phase space velocity 10-90 h -1 , hydrogen / MAPD=1-3 (molar ratio); more preferably, the process conditions of the selective hydrogenation reaction are: hydrogenation reactor inlet temperature 30-50°C, reaction pressure 2.0-2.8MPa, liquid phase space velocity 20-60h -1 , hydrogen / MAPD=1.1~2.0 (molar ratio).
[0022] In the above-mentioned method for selective hydrogenation of C3 fraction to remove alkynes, preferably, based on the total mass of the hydrogenation catalyst as 100%, the content of the main active component is 0.10-0.50%, the content of the auxiliary active component is 0.10-4.0%, and the balance is the carrier.
[0023] In the above-mentioned method for selective hydrogenation of C3 fraction to remove alkynes, preferably, the hydrogenation catalyst comprises a carrier and an active component, the carrier is a phosphorus-doped carbon material, the active component comprises Pd and Pb, Pd and Pb are dispersed on the carrier at the atomic level, and based on the total mass of the hydrogenation catalyst as 100%, the Pd content is 0.10-0.50%, the Pb content is 0.10-4.0%, and the balance is the carrier.
[0024] In the above-mentioned method for selective hydrogenation of C3 fraction to remove alkynes, the carrier in the hydrogenation catalyst is a porous structure with a high specific surface area, and the main active component and the auxiliary active component are dispersed on the surface and in the pores of the carrier at the atomic level. Preferably, the specific surface area of the carrier is 500 to 700 cm 2 / g, the most probable pore diameter is 2-30nm, and the pore volume is 0.80-1.50mL / g.
[0025] In the above-mentioned method for selective hydrogenation of C3 fraction to remove alkynes, preferably, the hydrogenation catalyst is prepared by the following steps:
[0026] (1) mixing a phosphorus-containing compound and a carbohydrate in water, then subjecting the mixture to a hydrothermal reaction, and then at least drying and calcining the mixture to obtain a phosphorus-doped carbon material carrier;
[0027] (2) loading the active components onto the phosphorus-doped carbon material carrier to obtain a catalyst semi-finished product;
[0028] (3) Reducing the semi-finished catalyst to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0029] In the above-mentioned catalyst preparation steps, preferably, in step (1), the phosphorus-containing compound includes phosphoric acid and / or phytic acid, etc.
[0030] In the above-mentioned catalyst preparation steps, preferably, in step (1), the carbohydrate includes glucose and / or sucrose, etc.
[0031] In the above catalyst preparation steps, preferably, in step (1), the mixing molar ratio of the phosphorus-containing compound to the carbohydrate is 0.0001 to 1000, more preferably 0.001 to 10, and further preferably 0.02 to 0.4.
[0032] In the above catalyst preparation step (1), the concentrations of the phosphorus-containing compound and the carbohydrate in water can be routinely adjusted by those skilled in the art, as long as they can be fully dissolved and mixed in water and the reaction can proceed smoothly.
[0033] In the above catalyst preparation steps, preferably, in step (1), the mixing of the phosphorus-containing compound and the carbohydrate in water is carried out under stirring conditions, and the stirring time is 30 to 120 minutes.
[0034] In the above catalyst preparation steps, preferably, in step (1), the temperature of the hydrothermal reaction is 160-300° C. and the time is 4-12 hours. More specifically, the hydrothermal reaction is carried out in a hydrothermal kettle placed in an oven, and the process does not require stirring.
[0035] In the above catalyst preparation steps, preferably, in step (1), the drying temperature is 120 to 160° C. and the drying time is 4 to 12 hours.
[0036] In the above catalyst preparation steps, preferably, step (1) further comprises: ball milling to refine into powder, the ball milling is performed after the drying and before the calcination, and the ball milling time is 3 to 10 minutes.
[0037] In the above catalyst preparation steps, preferably, in step (1), the calcination is carried out under an inert atmosphere, the calcination temperature is 600 to 1000° C., and the calcination time is 1 to 5 hours.
[0038] In the above catalyst preparation steps, preferably, step (2) is to load the active component onto the phosphorus-doped carbon material carrier by a photodeposition method.
[0039] In the above catalyst preparation steps, preferably, step (2) specifically comprises:
[0040] (2)-a1: adding the phosphorus-doped carbon material carrier to the precursor solution of the main active component, mixing evenly, freezing in liquid nitrogen, then irradiating under an ultraviolet xenon lamp, freeze-drying, and then calcining to obtain a carrier loaded with the main active component;
[0041] (2)-a2: adding the carrier loaded with the main active component to the precursor solution of the auxiliary active component, mixing them evenly, freezing them in liquid nitrogen, irradiating them under an ultraviolet xenon lamp, freeze-drying them, and then calcining them to obtain the catalyst semi-finished product;
[0042] Alternatively, step (2) specifically includes:
[0043] (2)-b1: adding the phosphorus-doped carbon material carrier to the precursor solution of the auxiliary active component, mixing evenly, freezing in liquid nitrogen, then irradiating under an ultraviolet xenon lamp, freeze-drying, and then calcining to obtain a carrier loaded with the auxiliary active component;
[0044] (2)-b2: Add the carrier loaded with the auxiliary active component to the precursor solution of the main active component, mix well, freeze in liquid nitrogen, then irradiate under an ultraviolet xenon lamp, freeze-dry, and then calcine to obtain the catalyst semi-finished product.
[0045] In the above catalyst preparation step (2), the main active component may be loaded on the carrier first, and then the auxiliary active component; or the auxiliary active component may be loaded on the carrier first, and then the main active component.
[0046] In the above-mentioned catalyst preparation steps, preferably, in step (2), the precursor of the main active component includes a palladium salt compound (more preferably a soluble palladium salt compound), specifically including one or a combination of palladium chloride, palladium nitrate and palladium sulfate.
[0047] In the above-mentioned catalyst preparation steps, preferably, in step (2), the precursor of the co-active component includes a lead salt compound (more preferably a soluble lead salt compound), specifically lead nitrate and / or lead acetate.
[0048] In the above catalyst preparation steps, preferably, in step (2), the concentration of the main active component in the precursor solution of the main active component is 0.1-5 mg Pd / mL Pd precursor solution.
[0049] In the above catalyst preparation steps, preferably, in step (2), the concentration of the co-active component in the precursor solution of the co-active component is 0.1-10 mgPb / mL Pb precursor solution.
[0050] In the above-mentioned catalyst preparation step (2), the amount of the carrier added to the active component precursor solution can be routinely adjusted by a person skilled in the art, as long as it can be fully mixed and the content of the active component in the prepared catalyst meets the requirements of the present invention.
[0051] In the above catalyst preparation steps, preferably, in step (2), the irradiation time under the ultraviolet xenon lamp is 0.5 to 5.0 hours.
[0052] In the above catalyst preparation steps, preferably, in step (2), the freeze-drying time is 2 to 7 hours, and the vacuum degree of the freeze-drying is 15 to 20 Pa.
[0053] In the above catalyst preparation steps, preferably, in step (2), the calcination is carried out under an inert atmosphere, the calcination temperature is 300 to 500° C., and the calcination time is 0.5 to 5 h.
[0054] In the above catalyst preparation steps, preferably, in step (3), the catalyst semi-finished product is reduced using a H2 and He mixed gas or pure hydrogen with a H2 volume percentage of 10 to 100%, a reduction temperature of 50 to 300° C., a reduction pressure of 0.1 to 2.0 MPa, and a reduction time of 0.5 to 10 h. More preferably, the reduction temperature is 100 to 200° C., the reduction pressure is 0.5 to 1.0 MPa, and the reduction time is 2 to 6 h.
[0055] The present invention provides a method for selective hydrogenation and alkyne removal, in particular, a method for selective hydrogenation and alkyne removal using a Pd-Pb-PC single-atom catalyst in a process for hydrogenation and alkyne removal of a carbon three fraction, thereby selectively hydrogenating and converting propyne (MA) and / or propadiene (PD) contained in the carbon three fraction into propylene, and almost no propylene is lost. The catalyst used in the traditional alkyne removal method has active components in the form of nanoparticles or sub-nano cluster structures, thereby affecting the performance of the catalyst. The method for selective hydrogenation and alkyne removal of a carbon three fraction of the present invention preferably uses a Pd-Pb-PC single-atom catalyst to selectively hydrogenate the material. The hydrogenation catalyst of the present invention uses a phosphorus-doped carbon material as a carrier, the carrier is a porous structure, has a high specific surface area, and uses a photoreduction method to disperse the active components (preferably palladium and lead) in a single-atom state on the carrier (on the surface and in the pores), rather than forming nanoparticles or sub-nano cluster structures. The atomically dispersed Pd and Pb have the following characteristics during the selective hydrogenation reaction of the present invention: since the active components are dispersed at the atomic level, the utilization rate of metal atoms is improved, thereby improving the hydrogenation activity of the catalyst; the adsorption capacity for olefins is reduced, thereby improving the hydrogenation selectivity of the catalyst; the probability of simultaneous adsorption of alkynes / dienes at adjacent active sites is reduced, thereby significantly reducing the probability of polymerization coking, thereby improving the anti-coking performance of the catalyst. Therefore, the hydrogenation catalyst of the present invention exhibits excellent hydrogenation activity, selectivity and anti-coking performance. Using the method for selective hydrogenation and removal of alkynes from C3 fractions of the present invention, even if the hydrogenation material contains a relatively heavy fraction and the amount of green oil generated by the catalyst is greatly increased, the catalyst activity and selectivity still do not show a downward trend. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 This is a spherical aberration corrected transmission electron microscope image of the hydrogenation catalyst provided in Example 1.
[0057] Figure 2 This is a transmission electron microscope image of the hydrogenation catalyst provided for Comparative Example 1.
[0058] Figure 3 This is a transmission electron microscopy image of the hydrogenation catalyst provided for Comparative Example 5.
[0059] Figure 4The present invention is a process flow chart of the hydrogenation of the C3 fraction of the propylene production process using a sequential separation process.
[0060] Figure 5 This is a process flow chart for hydrogenation of the C3 fraction of a propylene production process using a pre-depropanization and pre-hydrogenation process.
[0061] Description of Figure Numbers:
[0062] 1-cracking furnace; 2-quenching system; 3-oil washing tower; 4-water washing tower; 5-heat exchanger; 6-alkali washing tower; 7-demethanizer; 8-deethanizer; 9-depropanizer; 10-C3 fraction hydrogenation reactor; 11-front depropanizer; 12-C2 fraction hydrogenation reactor; 13-compressor. DETAILED DESCRIPTION
[0063] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0064] According to a specific embodiment of the present invention, preferably, the hydrogenation catalyst used in the method for selective hydrogenation of C3 fraction to remove alkynes provided by the present invention is prepared by the following steps:
[0065] (1) fully stirring and mixing a phosphorus-containing compound and a carbohydrate in water for 30 to 120 minutes to obtain a mixed solution; subjecting the mixed solution to a hydrothermal reaction in a hydrothermal reactor in an oven at 160 to 300° C. for 4 to 12 hours, and then drying the mixed solution at 120 to 160° C. for 4 to 12 hours, and then ball milling the mixed solution for 3 to 10 minutes to obtain a powder; and calcining the powder at 600 to 1000° C. for 1 to 5 hours under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0066] Wherein, the phosphorus-containing compound includes phosphoric acid and / or phytic acid, etc.; the carbohydrate includes glucose and / or sucrose, etc.; the mixing molar ratio of the phosphorus-containing compound to the carbohydrate is 0.0001 to 1000, preferably 0.001 to 10, and more preferably 0.02 to 0.4;
[0067] (2)-a1: adding the phosphorus-doped carbon material carrier to the palladium precursor aqueous solution, stirring evenly, placing it in liquid nitrogen for rapid freezing, and then irradiating it under an ultraviolet xenon lamp for 0.5 to 5.0 hours; then freeze-drying it under a vacuum condition of 15 to 20 Pa for 2 to 7 hours, and then calcining it at 300 to 500° C. for 0.5 to 5 hours under an inert atmosphere to obtain a palladium-loaded carrier;
[0068] (2)-a2: adding the palladium-loaded carrier to the lead precursor aqueous solution, stirring evenly, placing it in liquid nitrogen for rapid freezing, and then irradiating it under an ultraviolet xenon lamp for 0.5 to 5.0 hours; then freeze-drying it under a vacuum condition of 15 to 20 Pa for 2 to 7 hours, and then calcining it at 300 to 500° C. for 0.5 to 5 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0069] or,
[0070] (2)-b1 Add the phosphorus-doped carbon material carrier to the lead precursor aqueous solution, stir evenly, place it in liquid nitrogen for rapid freezing, and then illuminate it under a UV xenon lamp for 0.5 to 5.0 hours; then freeze-dry it under a vacuum condition of 15 to 20 Pa for 2 to 7 hours, and then calcine it at 300 to 500° C. for 0.5 to 5 hours under an inert atmosphere to obtain a lead-loaded carrier;
[0071] (2)-b2: adding the lead-loaded carrier to the aqueous solution of the palladium precursor, stirring evenly, placing it in liquid nitrogen for rapid freezing, and then irradiating it under a UV xenon lamp for 0.5 to 5.0 hours; then freeze-drying it under a vacuum condition of 15 to 20 Pa for 2 to 7 hours, and then calcining it at 300 to 500° C. for 0.5 to 5 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0072] The palladium precursor includes a soluble salt compound of palladium, specifically palladium chloride, palladium nitrate, palladium sulfate, etc., or a combination thereof; the concentration of palladium in the palladium precursor aqueous solution is 0.1 to 5 mgPd / mL Pd precursor aqueous solution;
[0073] The lead precursor includes a soluble salt compound of lead, specifically lead nitrate and / or lead acetate, etc.; the concentration of lead in the lead precursor aqueous solution is 0.1-10 mgPb / mL Pb precursor aqueous solution;
[0074] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 10 to 100% or pure hydrogen, the reduction temperature is 50 to 300°C (preferably 100 to 200°C), the reduction pressure is 0.1 to 2.0 MPa (preferably 0.5 to 1.0 MPa), and the reduction time is 0.5 to 10 h (preferably 2 to 6 h) to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0075] The technical solution of the present invention is further described below through specific embodiments.
[0076] In the following specific embodiments and comparative examples, the analytical testing methods used include:
[0077] Content of active components in catalyst: atomic absorption method;
[0078] Specific surface area of carrier: GB / T-5816;
[0079] Single atom morphology characterization: spherical aberration corrected transmission electron microscopy;
[0080] The conversion rate and selectivity are calculated according to the following formula:
[0081] Propyne, propadiene (MAPD) conversion (%) = 100 × (inlet MAPD content - outlet MAPD content) / inlet MAPD content,
[0082] Propylene selectivity (%) = 100 × (outlet propylene content - inlet propylene content) / (inlet MAPD content - outlet MAPD content).
[0083] Example 1
[0084] This embodiment provides a hydrogenation catalyst, which is prepared by the following steps:
[0085] (1) 10 g of phosphoric acid and 120 g of glucose were fully stirred in water for 40 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 160° C. for 4 h, then dried at 120° C. for 4 h, and then ball-milled for 3 min to obtain a powder; the powder was calcined at 600° C. for 1 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0086] (2) taking an appropriate amount of 1 mg Pd / mL Pd(NO3)2 aqueous solution, adding 10 g of the phosphorus-doped carbon material carrier, stirring evenly at room temperature, placing it in liquid nitrogen for rapid freezing, and then irradiating it under a UV xenon lamp for 0.5 h; then freeze-drying it under a vacuum condition of 15 Pa for 2 h, and then calcining it at 300°C for 1 h under an inert atmosphere to obtain a palladium-loaded carrier;
[0087] The palladium-loaded carrier is added to a lead nitrate aqueous solution containing 63.9 mg of lead nitrate, stirred evenly at room temperature, and then placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 0.5 h; then freeze-dried under a vacuum condition of 15 Pa for 2 h, and then calcined at 300° C. for 1 h under an inert atmosphere to obtain a catalyst semi-finished product;
[0088] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 10%, the reduction temperature is 65° C., the reduction pressure is 0.5 MPa, and the reduction time is 1 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0089] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.15%, the Pb content was 0.4%, and the remainder was the phosphorus-doped carbon material carrier.
[0090] The specific surface area of the phosphorus-doped carbon material carrier is 589 cm 2 / g, the most probable pore diameter is 3.5nm, and the pore volume is 1.1mL / g.
[0091] The spherical aberration corrected transmission electron microscopy image of the hydrogenation catalyst provided in this embodiment is as follows Figure 1 As shown by Figure 1 It can be seen that Pd and Pb are dispersed on the support at the atomic level.
[0092] Example 2
[0093] This embodiment provides a hydrogenation catalyst, which is prepared by the following steps:
[0094] (1) 10 g of phytic acid and 120 g of sucrose were fully stirred in water for 90 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 200° C. for 6 h, then dried at 130° C. for 6 h, and then ball-milled for 5 min to obtain a powder; the powder was calcined at 700° C. for 2 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0095] (2) taking an appropriate amount of 1 mg Pd / mL PdCl2 aqueous solution, adding 10 g of the phosphorus-doped carbon material carrier, stirring evenly at room temperature, placing it in liquid nitrogen for rapid freezing, and then irradiating it under a UV xenon lamp for 1 hour; then freeze-drying it under a vacuum condition of 16 Pa for 2.5 hours, and then calcining it at 300°C for 2 hours under an inert atmosphere to obtain a palladium-loaded carrier;
[0096] The palladium-loaded carrier is added to a lead nitrate aqueous solution containing 159.9 mg of lead nitrate, stirred evenly at room temperature, and then placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 1 hour; then freeze-dried under a vacuum condition of 16 Pa for 2.5 hours, and then calcined at 300° C. for 2 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0097] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 20%, the reduction temperature is 90° C., the reduction pressure is 0.8 MPa, and the reduction time is 2 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0098] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.25%, the Pb content was 1.0%, and the remainder was the phosphorus-doped carbon material carrier.
[0099] Example 3
[0100] This embodiment provides a hydrogenation catalyst, which is prepared by the following steps:
[0101] (1) 10 g of phytic acid and 120 g of sucrose were fully stirred in water for 120 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 200 ° C for 8 h, and then dried at 140 ° C for 8 h, and then ball milled for 7 min to obtain a powder; the powder was calcined at 800 ° C for 3 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0102] (2) adding 10 g of the phosphorus-doped carbon support to an aqueous solution of lead nitrate in which 319.7 mg of lead nitrate was dissolved, stirring at room temperature, rapidly freezing the solution in liquid nitrogen, and then irradiating the solution under an ultraviolet xenon lamp for 2 h; then freeze-drying the solution under a vacuum of 17 Pa for 3 h, and calcining the solution at 350° C. for 3 h under an inert atmosphere to obtain a lead-loaded support;
[0103] An appropriate amount of 1 mg Pd / mL palladium sulfate aqueous solution is measured, and the lead-loaded carrier is added, and after being stirred evenly at room temperature, it is placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 2 hours; thereafter, freeze-dried for 3 hours under a vacuum condition of 17 Pa, and then calcined at 350° C. for 3 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0104] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 40%, the reduction temperature is 130° C., the reduction pressure is 1 MPa, and the reduction time is 4 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0105] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.3%, the Pb content was 2.0%, and the remainder was the phosphorus-doped carbon material carrier.
[0106] Example 4
[0107] This embodiment provides a hydrogenation catalyst, which is prepared by the following steps:
[0108] (1) 10 g of phytic acid and 120 g of glucose were fully stirred in water for 60 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 250° C. for 10 h, then dried at 150° C. for 10 h, and then ball-milled for 8 min to obtain a powder; the powder was calcined at 900° C. for 4 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0109] (2) adding 10 g of the phosphorus-doped carbon support to a lead nitrate aqueous solution containing 479.6 mg of lead nitrate, stirring at room temperature, rapidly freezing the mixture in liquid nitrogen, and then irradiating the mixture under an ultraviolet xenon lamp for 3 h; then freeze-drying the mixture under a vacuum of 18 Pa for 5.5 h, and calcining the mixture under an inert atmosphere at 400° C. for 4 h to obtain a lead-loaded support;
[0110] Take an appropriate amount of 1 mg Pd / mL Pd(NO3)2 aqueous solution, add the lead-loaded carrier, stir evenly at room temperature, quickly freeze in liquid nitrogen, and then illuminate under a UV xenon lamp for 3 hours; then freeze-dry under 18 Pa vacuum conditions for 5.5 hours, and then calcine at 400°C for 4 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0111] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 60%, the reduction temperature is 200° C., the reduction pressure is 1.5 MPa, and the reduction time is 6 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0112] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.4%, the Pb content was 3.0%, and the remainder was the phosphorus-doped carbon material carrier.
[0113] Example 5
[0114] This embodiment provides a hydrogenation catalyst, which is prepared by the following steps:
[0115] (1) 10 g of phosphoric acid and 120 g of sucrose were fully stirred in water for 90 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 300° C. for 12 h, then dried at 160° C. for 12 h, and then ball-milled for 10 min to obtain a powder; the powder was calcined at 1000° C. for 5 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0116] (2) taking an appropriate amount of 1 mg Pd / mL PdCl2 aqueous solution, adding 10 g of the phosphorus-doped carbon material carrier, stirring evenly at room temperature, placing it in liquid nitrogen for rapid freezing, and then irradiating it under a UV xenon lamp for 4.5 h; then freeze-drying it under a vacuum condition of 20 Pa for 6 h, and then calcining it at 500° C. for 5 h under an inert atmosphere to obtain a palladium-loaded carrier;
[0117] The palladium-loaded carrier is added to a lead nitrate aqueous solution containing 639.4 mg of lead nitrate, stirred evenly at room temperature, and then placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 4.5 hours; then freeze-dried under a vacuum condition of 20 Pa for 6 hours, and then calcined at 500° C. for 5 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0118] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 80%, the reduction temperature is 250° C., the reduction pressure is 2 MPa, and the reduction time is 8 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0119] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.5%, the Pb content was 4.0%, and the remainder was the phosphorus-doped carbon material carrier.
[0120] Comparative Example 1
[0121] This comparative example provides a hydrogenation catalyst, which is prepared by the following steps:
[0122] (1) 120 g of glucose was fully stirred in water for 40 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 160° C. for 4 h, then dried at 120° C. for 4 h, and then ball-milled for 3 min to obtain a powder; the powder was calcined at 600° C. for 1 h under an inert atmosphere to obtain a carbon material carrier;
[0123] (2) taking an appropriate amount of 1 mg Pd / mL Pd(NO3)2 aqueous solution, adding 10 g of the carbon material carrier, stirring evenly at room temperature, placing it in liquid nitrogen for rapid freezing, and then irradiating it under a UV xenon lamp for 0.5 h; then freeze-drying it under a vacuum condition of 15 Pa for 2 h, and then calcining it at 300°C for 1 h under an inert atmosphere to obtain a palladium-loaded carrier;
[0124] The palladium-loaded carrier is added to a lead nitrate aqueous solution containing 63.9 mg of lead nitrate, stirred evenly at room temperature, and then placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 0.5 h; then freeze-dried under a vacuum condition of 15 Pa for 2 h, and then calcined at 300° C. for 1 h under an inert atmosphere to obtain a catalyst semi-finished product;
[0125] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 10%, the reduction temperature is 65° C., the reduction pressure is 0.5 MPa, and the reduction time is 1 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0126] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.15%, the Pb content was 0.4%, and the remainder was the carbon material carrier.
[0127] The specific surface area of the carbon material carrier is 383 cm 2 / g, the most probable pore diameter is 3.5nm, and the pore volume is 0.3mL / g.
[0128] The transmission electron microscope image of the hydrogenation catalyst provided in this comparative example is as follows Figure 2 As shown by Figure 2 It can be seen that the active components in the hydrogenation catalyst are not all dispersed in single atoms, and nanoparticles are produced.
[0129] Comparative Example 2
[0130] This comparative example provides a hydrogenation catalyst, which is prepared by the following steps:
[0131] (1) A commercially available bimodal pore distribution spherical alumina carrier having a diameter of 4 mm is used as the carrier; the bimodal pore distribution spherical alumina carrier is subjected to high temperature calcination at 1250° C. for 4 h to obtain a catalyst carrier;
[0132] (2) taking an appropriate amount of 1 mg Pd / mL PdCl2 aqueous solution, adding 10 g of the catalyst carrier, stirring evenly at room temperature, placing in liquid nitrogen for rapid freezing, and then irradiating under a UV xenon lamp for 1 hour; then freeze-drying under a vacuum condition of 16 Pa for 2.5 hours, and then calcining at 300° C. for 2 hours under an inert atmosphere to obtain a palladium-loaded carrier;
[0133] The palladium-loaded carrier is added to a lead nitrate aqueous solution containing 159.9 mg of lead nitrate, stirred evenly at room temperature, and then placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 1 hour; then freeze-dried under a vacuum condition of 16 Pa for 2.5 hours, and then calcined at 300° C. for 2 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0134] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 20%, the reduction temperature is 90° C., the reduction pressure is 0.8 MPa, and the reduction time is 2 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0135] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.25%, the Pb content was 1.0%, and the remainder was the catalyst carrier.
[0136] Comparative Example 3
[0137] This comparative example provides a hydrogenation catalyst, which is prepared by the following steps:
[0138] (1) 10 g of phytic acid and 120 g of sucrose were fully stirred in water for 120 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 200 ° C for 8 h, and then dried at 140 ° C for 8 h, and then ball milled for 7 min to obtain a powder; the powder was calcined at 800 ° C for 3 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0139] (2) adding 10 g of the phosphorus-doped carbon support to an aqueous solution of lead nitrate in which 319.7 mg of lead nitrate was dissolved, stirring at room temperature, rapidly freezing the solution in liquid nitrogen, and then irradiating the solution under an ultraviolet xenon lamp for 2 h; then freeze-drying the solution under a vacuum of 17 Pa for 3 h, and calcining the solution at 350° C. for 3 h under an inert atmosphere to obtain a lead-loaded support;
[0140] An excess of 1 mg Pd / mL palladium sulfate aqueous solution is measured, and the lead-loaded carrier is added, and after being stirred evenly at room temperature, the mixture is placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 2 hours; thereafter, the mixture is freeze-dried under a vacuum condition of 17 Pa for 3 hours, and then calcined at 350° C. for 3 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0141] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 40%, the reduction temperature is 130° C., the reduction pressure is 1 MPa, and the reduction time is 4 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0142] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 3.0%, the Pb content was 2.0%, and the remainder was the phosphorus-doped carbon material carrier.
[0143] Comparative Example 4
[0144] This comparative example provides a hydrogenation catalyst, which is prepared by the following steps:
[0145] (1) 10 g of phytic acid and 120 g of glucose were fully stirred in water for 60 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 250° C. for 10 h, then dried at 150° C. for 10 h, and then ball-milled for 8 min to obtain a powder; the powder was calcined at 900° C. for 4 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0146] (2) adding 10 g of the phosphorus-doped carbon support to an aqueous solution of lead nitrate in which 959.1 mg of lead nitrate was dissolved, stirring at room temperature, rapidly freezing the mixture in liquid nitrogen, and then irradiating the mixture under an ultraviolet xenon lamp for 3 h; then freeze-drying the mixture under a vacuum of 18 Pa for 5.5 h, and calcining the mixture under an inert atmosphere at 400° C. for 4 h to obtain a lead-loaded support;
[0147] Take an appropriate amount of 1 mg Pd / mL Pd(NO3)2 aqueous solution, add the lead-loaded carrier, stir evenly at room temperature, quickly freeze in liquid nitrogen, and then illuminate under a UV xenon lamp for 3 hours; then freeze-dry under 18 Pa vacuum conditions for 5.5 hours, and then calcine at 400°C for 4 hours under an inert atmosphere to obtain a catalyst semi-finished product;
[0148] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 60%, the reduction temperature is 200° C., the reduction pressure is 1.5 MPa, and the reduction time is 6 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0149] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.4%, the Pb content was 6.0%, and the remainder was the phosphorus-doped carbon material carrier.
[0150] Comparative Example 5
[0151] This comparative example provides a hydrogenation catalyst, which is prepared by the following steps:
[0152] (1) 10 g of phosphoric acid and 120 g of sucrose were fully stirred in water for 90 min to obtain a mixed solution; the mixed solution was subjected to a hydrothermal reaction in a hydrothermal reactor in an oven at 300° C. for 12 h, then dried at 160° C. for 12 h, and then ball-milled for 10 min to obtain a powder; the powder was calcined at 1000° C. for 5 h under an inert atmosphere to obtain a phosphorus-doped carbon material carrier;
[0153] (2) taking an appropriate amount of 1 mg Pd / mL PdCl2 aqueous solution, adjusting the pH value of the PdCl2 aqueous solution to 2 with hydrochloric acid, adding 10 g of the phosphorus-doped carbon material carrier, stirring evenly, impregnating and adsorbing at room temperature for 1 h, drying at 110° C. for 2 h, and then calcining at 480° C. for 6 h to obtain a palladium-loaded carrier;
[0154] The palladium-loaded carrier is added to a lead nitrate aqueous solution containing 639.4 mg of lead nitrate, stirred evenly, and then immersed and adsorbed at room temperature for 1 hour, then dried at 100° C. for 3 hours, and then calcined at 500° C. for 4 hours to obtain a catalyst semi-finished product;
[0155] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 80%, the reduction temperature is 250° C., the reduction pressure is 2 MPa, and the reduction time is 8 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0156] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.5%, the Pb content was 4.0%, and the remainder was the phosphorus-doped carbon material carrier.
[0157] The transmission electron microscope image of the hydrogenation catalyst provided in this comparative example is as follows Figure 3 As shown by Figure 3 It can be seen that the active components in the hydrogenation catalyst are mostly in the form of nanoparticles.
[0158] Comparative Example 6
[0159] This comparative example provides a hydrogenation catalyst, which is prepared by the following steps:
[0160] (1) 12.5 g of melamine was weighed into a beaker, 30 mL of water was added, and then 27.8 mL of phytic acid solution (the mass ratio of phytic acid to melamine was 2:1) was added. After ultrasonication for 30 min, the beaker was placed in a microwave oven and heated at 1000 W for 120 s. After washing and drying, a nitrogen-phosphorus co-doped carbon support was obtained;
[0161] (2) taking an appropriate amount of 1 mg Pd / mL Pd(NO3)2 aqueous solution, adding 10 g of the nitrogen-phosphorus co-doped carbon carrier, stirring evenly at room temperature, placing it in liquid nitrogen for rapid freezing, and then irradiating it under a UV xenon lamp for 0.5 h; then freeze-drying it under a vacuum condition of 15 Pa for 2 h, and then calcining it at 300°C for 1 h under an inert atmosphere to obtain a palladium-loaded carrier;
[0162] The palladium-loaded carrier is added to a lead nitrate aqueous solution containing 63.9 mg of lead nitrate, stirred evenly at room temperature, and then placed in liquid nitrogen for rapid freezing, and then illuminated under an ultraviolet xenon lamp for 0.5 h; then freeze-dried under a vacuum condition of 15 Pa for 2 h, and then calcined at 300° C. for 1 h under an inert atmosphere to obtain a catalyst semi-finished product;
[0163] (3) The catalyst semi-finished product is reduced with a mixture of H2 and He with a H2 volume percentage of 10%, the reduction temperature is 65° C., the reduction pressure is 0.5 MPa, and the reduction time is 1 h to obtain a reduced catalyst, namely the hydrogenation catalyst.
[0164] The atomic absorption spectrometry test showed that, based on the total mass of the hydrogenation catalyst being 100%, the Pd content was 0.15%, the Pb content was 0.4%, and the remainder was the nitrogen-phosphorus co-doped carbon support.
[0165] Example 6 and Comparative Example 7
[0166] This embodiment and comparative example respectively provide methods for selective hydrogenation of C3 fraction to remove alkynes, and the methods respectively use the hydrogenation catalysts provided in embodiments 1 to 5 and comparative examples 1 to 6. The method for selective hydrogenation of C3 fraction to remove alkynes comprises the following steps: allowing the C3 fraction to enter a hydrogenation reactor, and performing a selective hydrogenation reaction under the action of a hydrogenation catalyst in the hydrogenation reactor to convert propyne and / or propadiene in the C3 fraction into propylene; wherein the hydrogenation catalysts are the hydrogenation catalysts provided in embodiments 1 to 5 and comparative examples 1 to 6.
[0167] The hydrogenation reactor adopts a single-stage adiabatic fixed bed reactor.
[0168] The C3 fraction comes from the top of a depropanizer in a propylene production process using a sequential separation process, or comes from the bottom of a deethanizer in a propylene production process using a pre-depropanization and pre-hydrogenation process.
[0169] The material compositions of the C3 fractions subjected to the selective hydrogenation reaction using the hydrogenation catalysts of different embodiments and comparative examples are shown in Table 1.
[0170] The process conditions of the selective hydrogenation reaction are as follows: the reaction pressure and liquid phase space velocity are shown in Table 2, the hydrogenation reactor inlet temperature is shown in Table 3, the catalyst loading in the hydrogenation reactor is 50 mL, and hydrogen / MAPD=1.2 (molar ratio).
[0171] The results of selective hydrogenation of C3 fraction to remove alkynes are shown in Table 3.
[0172] Table 1 Reaction material composition (volume percentage / %)
[0173]
[0174] Table 2 Reaction pressure and liquid phase space velocity
[0175]
[0176] Table 3 Results of selective hydrogenation and alkyne removal of C3 fraction
[0177]
[0178] Note: Coking amount = (loss on calcination at 600℃÷initial catalyst loading amount) × 100%
[0179] In the method for selective hydrogenation of C3 fraction to remove alkynes in this embodiment and comparative example, the C3 fraction hydrogenation process of the propylene preparation process using a sequential separation process is as follows: Figure 4As shown, the process mainly includes: the raw materials (mainly including petroleum hydrocarbon steam) in the propylene preparation process enter the cracking furnace 1 for high-temperature cracking, the product is first cooled by the quenching system 2, and then successively treated by the oil washing tower 3, the water washing tower 4, the heat exchanger 5, and the alkali washing tower 6, and then enters the demethanizer 7, the methane and hydrogen are separated from the top of the demethanizer 7, the material at the bottom enters the deethanizer 8, the carbon two fraction is separated from the top of the deethanizer 8, the material at the bottom enters the depropanizer 9, the material separated from the top of the depropanizer 9 enters the carbon three fraction hydrogenation reactor 10 (a single-stage adiabatic fixed bed reactor in this embodiment and the comparative example) for hydrogenation to remove MAPD, the carbon four and above fractions at the bottom of the depropanizer 9 are sent to the subsequent unit, and the product of the carbon three fraction hydrogenation reactor 10 can be further sent to the propylene distillation unit.
[0180] In the method for selective hydrogenation of C3 fraction to remove acetylene in this embodiment and comparative example, the C3 fraction hydrogenation process of the propylene preparation process using the pre-depropanization pre-hydrogenation process is as follows: Figure 5 As shown, the process mainly includes: the raw materials (mainly including petroleum hydrocarbon steam) in the propylene preparation process enter the cracking furnace 1 for high-temperature cracking, the product is first cooled by the quenching system 2, and then successively treated by the oil washing tower 3, the water washing tower 4, the heat exchanger 5, and the alkali washing tower 6, and then enters the front depropanizer 11, the propane and propylene are separated at the bottom of the front depropanizer 11, the material at the top of the tower enters the carbon two fraction hydrogenation reactor 12 for hydrogenation reaction, the reacted material is compressed by the compressor 13, and then enters the deethanizer 8, ethane and ethylene are separated at the top of the deethanizer 8, and the material at the bottom of the tower enters the carbon three fraction hydrogenation reactor 10 (a single-stage adiabatic fixed bed reactor in this embodiment and the comparative example) for hydrogenation to remove MAPD, and the product of the carbon three fraction hydrogenation reactor 10 can be further sent to the propylene distillation unit.
[0181] From the above results, it can be seen that the hydrogenation catalyst used in the method for selective hydrogenation of carbon three fractions to remove alkynes provided by the present invention has excellent hydrogenation activity, selectivity and anti-coking performance. Using the method for selective hydrogenation of carbon three fractions to remove alkynes of the present invention, even if the hydrogenation material contains more heavy fractions, the amount of green oil generated by the catalyst is greatly increased, and the catalyst activity and selectivity still have no downward trend.
[0182] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for selectively hydrogenating a C3 fraction to remove alkynes, comprising the following steps: subjecting the C3 fraction to a selective hydrogenation reaction under the action of a hydrogenation catalyst to convert propyne and / or propadiene in the C3 fraction into propylene; The hydrogenation catalyst comprises a carrier and an active component, wherein the carrier is a phosphorus-doped carbon material, the active component comprises a main active component and an auxiliary active component, the main active component comprises Pd, the auxiliary active component comprises Pb, and the main active component and the auxiliary active component are dispersed on the carrier at the atomic level.
2. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 1, wherein: The hydrogenation reactor used in the selective hydrogenation reaction includes a single-stage adiabatic fixed bed reactor and / or a two-stage adiabatic fixed bed reactor.
3. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 1 or 2, wherein: The C3 fraction comes from the top of a depropanizer in a propylene preparation process using a sequential separation process; Preferably, the material composition of the C3 fraction from the top of the depropanizer tower includes, by volume percentage: 70-90% propylene, 5-30% propane, and 2.0-5.0% propyne+propadiene; More preferably, when the propyne+propadiene in the material composition of the C3 fraction from the top of the depropanizer is ≤4.0% by volume, a single-stage adiabatic fixed-bed reactor is used for the selective hydrogenation reaction; when the propyne+propadiene in the material composition of the C3 fraction from the top of the depropanizer is greater than 4.0%, a two-stage adiabatic fixed-bed reactor is used for the selective hydrogenation reaction.
4. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 1 or 2, wherein: The C3 fraction comes from the bottom of the deethanizer in the propylene preparation process using a pre-depropanization and pre-hydrogenation process; Preferably, the material composition of the C3 fraction from the bottom of the deethanizer tower includes, by volume percentage: 80-95% propylene, 5-20% propane, 0.05-0.2% propyne, and 0.05-0.2% propadiene; More preferably, a single-stage adiabatic fixed-bed reactor is used to selectively hydrogenate the C3 fraction from the bottom of the deethanizer.
5. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 1 or 2, wherein: The process conditions of the selective hydrogenation reaction are: the inlet temperature of the hydrogenation reactor is 25-55°C, the reaction pressure is 1.8-4.0 MPa, and the liquid phase space velocity is 10-90 h -1 , hydrogen / MAPD=1-3; Preferably, the process conditions of the selective hydrogenation reaction are: the inlet temperature of the hydrogenation reactor is 30-50°C, the reaction pressure is 2.0-2.8 MPa, and the liquid phase space velocity is 20-60 h -1 , hydrogen / MAPD=1.1~2.
0.
6. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 1, wherein: Taking the total mass of the hydrogenation catalyst as 100%, the content of the main active component is 0.10-0.50%, the content of the auxiliary active component is 0.10-4.0%, and the balance is the carrier.
7. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 1 or 6, wherein: The specific surface area of the carrier in the hydrogenation catalyst is 500 to 700 cm 2 / g, the most probable pore diameter is 2-30nm, and the pore volume is 0.80-1.5mL / g.
8. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 1 or 6, wherein: The hydrogenation catalyst is prepared by the following steps: (1) mixing a phosphorus-containing compound and a carbohydrate in water, then subjecting the mixture to a hydrothermal reaction, and then at least drying and calcining the mixture to obtain a phosphorus-doped carbon material carrier; (2) loading the active components onto the phosphorus-doped carbon material carrier to obtain a catalyst semi-finished product; (3) Reducing the semi-finished catalyst to obtain a reduced catalyst, namely the hydrogenation catalyst.
9. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 8, wherein: In step (1), the phosphorus-containing compound includes phosphoric acid and / or phytic acid.
10. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 8, wherein: In step (1), the carbohydrates include glucose and / or sucrose.
11. The method for selective hydrogenation of C3 fraction to remove alkynes according to any one of claims 8 to 10, wherein: In step (1), the mixing molar ratio of the phosphorus-containing compound to the carbohydrate is 0.0001 to 1000, preferably 0.001 to 10, and more preferably 0.02 to 0.
4.
12. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 8, wherein: In step (1), the phosphorus-containing compound and the carbohydrate are mixed in water under stirring conditions, and the stirring time is 30 to 120 minutes; Preferably, in step (1), the temperature of the hydrothermal reaction is 160 to 300° C., and the time is 4 to 12 hours; Preferably, in step (1), the drying temperature is 120 to 160° C. and the drying time is 4 to 12 hours; Preferably, step (1) further comprises: ball milling to refine into powder, wherein the ball milling is performed after the drying and before the calcining, and the ball milling time is 3 to 10 minutes; Preferably, in step (1), the calcination is carried out under an inert atmosphere, the calcination temperature is 600 to 1000° C., and the calcination time is 1 to 5 hours.
13. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 8, wherein: Step (2) is to load the active component onto the phosphorus-doped carbon material carrier by using a photodeposition method.
14. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 8 or 13, wherein: Step (2) specifically includes: (2)-a1: adding the phosphorus-doped carbon material carrier to the precursor solution of the main active component, mixing evenly, freezing in liquid nitrogen, then irradiating under an ultraviolet xenon lamp, freeze-drying, and then calcining to obtain a carrier loaded with the main active component; (2)-a2: adding the carrier loaded with the main active component to the precursor solution of the auxiliary active component, mixing them evenly, freezing them in liquid nitrogen, irradiating them under an ultraviolet xenon lamp, freeze-drying them, and then calcining them to obtain the catalyst semi-finished product; Alternatively, step (2) specifically includes: (2)-b1: adding the phosphorus-doped carbon material carrier to the precursor solution of the auxiliary active component, mixing evenly, freezing in liquid nitrogen, then irradiating under an ultraviolet xenon lamp, freeze-drying, and then calcining to obtain a carrier loaded with the auxiliary active component; (2)-b2: Add the carrier loaded with the auxiliary active component to the precursor solution of the main active component, mix well, freeze in liquid nitrogen, then irradiate under an ultraviolet xenon lamp, freeze-dry, and then calcine to obtain the catalyst semi-finished product.
15. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 14, wherein: In step (2), the precursor of the main active component includes a palladium salt compound; preferably, the precursor of the main active component includes one or a combination of palladium chloride, palladium nitrate and palladium sulfate.
16. The method for selective hydrogenation of C3 fraction to remove acetylene according to claim 14, wherein: In step (2), the precursor of the co-active component includes a lead salt compound; preferably, the precursor of the co-active component includes lead nitrate and / or lead acetate.
17. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 14, wherein: In step (2), the concentration of the main active component in the precursor solution of the main active component is 0.1 to 5 mg Pd / mL Pd precursor solution; Preferably, in step (2), the concentration of the co-active component in the precursor solution of the co-active component is 0.1-10 mgPb / mL Pb precursor solution.
18. The method for selective hydrogenation of C3 fraction to remove alkynes according to claim 14, wherein: In step (2), the irradiation time under the ultraviolet xenon lamp is 0.5 to 5.0 hours; Preferably, in step (2), the freeze-drying time is 2 to 7 hours, and the vacuum degree of the freeze-drying is 15 to 20 Pa; Preferably, in step (2), the calcination is carried out under an inert atmosphere, the calcination temperature is 300 to 500° C., and the calcination time is 0.5 to 5 hours.
19. The method for selective hydrogenation of C3 fraction to remove acetylenes according to claim 8, wherein: In step (3), the catalyst semi-finished product is reduced using a mixture of H2 and He with a H2 volume percentage of 10 to 100% or pure hydrogen, the reduction temperature is 50 to 300° C., the reduction pressure is 0.1 to 2.0 MPa, and the reduction time is 0.5 to 10; preferably, the reduction temperature is 100 to 200° C., the reduction pressure is 0.5 to 1.0 MPa, and the reduction time is 2 to 6 hours.
Citation Information
Patent Citations
Selective hydrogenation method for C3 fraction
CN102206132A
Unsaturated hydrocarbon hydrogenation catalyst, preparation method and applications thereof
CN102218323A
Method for preparing monodisperse metal atom / graphene composite material employing electrochemical dissolved graphite
CN106654300A
Fe series selective hydrogenation catalyst, and preparation method and application thereof
CN106925279A
Hydrogenation method for C3 fraction
CN108250024A