Preparation method of antibacterial and antioxidant PE plastic master batch modified by polygonum cuspidatum extract

Through technical means such as functional carriers and aldehyde-based guar gum, the loading and PE resin modification of the kelp extract is solved, and the problem of insufficient antioxidant and antibacterial properties of PE plastic masterbatches is significantly improved. Its mechanical and anti-resistant properties are significantly improved Oxidation performance extends service life.

CN118955959AInactive Publication Date: 2024-11-15BYHERB BIGBIO TECH (QINGDAO) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410825038.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyethylene (PE) plastic masterbatches age, discolor, crack, become brittle or powdered under the action of atmosphere, sunlight and oxygen. They have poor antioxidant performance and poor antibacterial properties, resulting in shortening of service life, and kaminata extract The poor high temperature resistance performance leads to its easy carbonization and loss during the preparation process, affecting the antibacterial and antioxidant properties of PE plastic masterbatches.

Method used

The extract of karuta is loaded with functional carriers, and the activation and aminoation of maifanite is fully loaded into the pores of maifanite particles, and the reaction is combined with aldehyde-based guar gum and sodium borohydride to form Stable functional molecular nests improve the load stability of kasuka extract and modify the PE resin to enhance its surface activation and wetting properties, ensuring uniform dispersion and compatibility of components.

Benefits of technology

The PE plastic masterbatches produced have excellent antibacterial properties, antioxidant properties and mechanical properties, and are stable after ultraviolet irradiation, significantly improve antibacterial effects, strong antioxidant ability, and prolong service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a preparation method of antibacterial and antioxidant PE plastic master batches modified by using a polygonum cuspidatum extract, and belongs to the technical field of PE plastic master batches. The preparation method comprises the following steps: preparing a polygonum cuspidatum extract, preparing a functional carrier, loading, preparing a functional molecular nest, modifying PE resin, and mixing and granulating. The PE resin is modified, specifically, the PE resin is placed in modification liquid with the volume 7-9 times that of the PE resin to be subjected to homogenization treatment, the homogenization time is 3-5 min, the homogenization pressure is 4.8-5.2 MPa, the number of times of homogenization is two, dipping is conducted after homogenization treatment is finished, the dipping temperature is 68-72 DEG C, the dipping time is 55-59 min, cooling and drying are conducted after dipping is finished, and the modified PE resin is prepared; the modified liquid is a mixture of deionized water, polyethylene glycol 600 and nonylphenol polyoxyethylene ether sulfonate; the PE plastic master batch prepared by the method disclosed by the invention is good in antibacterial activity, excellent in oxidation resistance and excellent and stable in mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PE plastic masterbatches, and in particular relates to a method for preparing antibacterial and antioxidant PE plastic masterbatches modified with a knotweed extract. Background Art

[0002] Masterbatch is composed of carrier resin, various fillers and various additives; PE masterbatch refers to the granular material obtained by mixing additives, fillers and PE resin, and then metering, mixing, melting, extruding, pelletizing and other processing processes such as extruders; PE, also known as polyethylene, is a thermoplastic resin made by polymerization of ethylene. It is non-toxic and odorless, has excellent low-temperature resistance, and the lowest operating temperature can reach -100 to -70°C. It has good chemical stability, can withstand the corrosion of most acids and alkalis, has low water absorption, and has excellent electrical insulation. Under the influence of atmosphere, sunlight and oxygen, polyethylene will age, discolor, crack, become brittle or powdery, and lose its mechanical properties. Its antioxidant properties and antibacterial properties are poor, which seriously affects the performance of PE plastic masterbatch and shortens its service life.

[0003] Polygonum cuspidatum is a weed of the Polygonaceae family. It is rich in rhubarb and resveratrol, has good antibacterial effects on Staphylococcus aureus and Escherichia coli, and has excellent antioxidant properties. Therefore, when preparing PE plastic masterbatch, adding Polygonum cuspidatum extract can effectively enhance the antioxidant and antibacterial properties; however, Polygonum cuspidatum extract has poor high temperature resistance and is easily carbonized and lost when exposed to high temperature during the preparation process, which will lead to low enhancement of the antibacterial and antioxidant properties of PE plastic masterbatch; In order to improve the high temperature resistance of the knotweed extract, the applicant used porous materials to load the knotweed extract, thereby reducing the loss during the subsequent high temperature treatment process. However, the porous material has poor compatibility with the PE resin. During mixed extrusion, the two cannot be dispersed evenly, which affects the mechanical properties of the PE plastic masterbatch. In addition, the performance of the prepared PE plastic masterbatch is unstable, and the mechanical properties are severely lost after ultraviolet irradiation, which greatly shortens the service life. Summary of the invention

[0004] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing an antibacterial and antioxidant PE plastic masterbatch modified with a knotweed extract. The prepared PE plastic masterbatch has good antibacterial properties, excellent mechanical properties, good antioxidant properties, and high mechanical stability after ultraviolet irradiation.

[0005] In view of the above technical problems, the present invention adopts the following technical solutions: The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract comprises the steps of preparing Polygonum cuspidatum extract, preparing functional carrier, loading, preparing functional molecular nest, modifying PE resin, and mixing granulation. The specific operations are as follows: 1. Preparation of Polygonum cuspidatum Extract The polygonum cuspidatum is washed, dried at 123-128°C, and then crushed. After the crushing, it is placed in an ethanol solution with a volume of 3.0-4.0 times for ultrasonic extraction. The ultrasonic time is 4.3-4.7h, the ultrasonic temperature is 40-44°C, and the ultrasonic frequency is 26-28kHz. After the ultrasonic extraction, it is filtered to remove the filter residue to obtain a filtrate. The filtrate is vacuum concentrated to 28-32% of the original volume, the concentration temperature is controlled to 63-67°C, the vacuum degree is 0.06-0.08MPa, and spray-dried to obtain a polygonum cuspidatum extract. The volume concentration of the ethanol solution is 53-57%.

[0006] 2. Preparation of functional carriers (1) Medical stone pretreatment The medical stone is placed in a sodium hydroxide solution of 4.5-5.5 times the volume for soaking, the soaking time is 2.4-2.6h, the soaking temperature is 58-62°C, and after the soaking is completed, it is dried to obtain the medical stone after alkali soaking; the medical stone after alkali soaking is placed in deionized water of 6-8 times the mass, cocamidopropyl betaine and polyethylene glycol monolaurate are added for ball milling, the ball milling time is 28-32min, the ball milling speed is 137-143rpm, the ball-to-material ratio is 4-6:1, the ball milling temperature is 50-54°C, after the ball milling is completed, it is naturally reduced to room temperature, and dried to obtain the pretreated medical stone; The particle size of the medical stone is 264-276nm; The mass concentration of the sodium hydroxide solution is 38-42%; The mass ratio of the medical stone, cocamidopropyl betaine and polyethylene glycol monolaurate after alkali leaching is 10-14:0.8-1.1:0.9-1.3; (2) Amination The pretreated medical stone is placed in an ammonia solution and stirred at a stirring temperature of 26-30°C for 6-8 minutes. After stirring evenly, an amination reagent is added, and after stirring evenly, microwave heating is performed at a microwave power of 227-233W and a microwave time of 5-9 minutes. After the microwave is finished, the temperature is raised to 92-96°C at a rate of 1.2-1.4°C / min, and a stirring reaction is performed. The stirring speed is 200-212rpm and the stirring time is 5.7-6.3h. After the reaction is finished, washing and drying are performed to obtain a functional carrier; The mass concentration of the ammonia solution is 22-24%; The amination agent is a mixture of ethylenediamine and diethylenetriamine, and the mass ratio of ethylenediamine to diethylenetriamine is 1.4-1.6:1.2-1.4; The mass ratio of the pretreated medical stone, ammonia solution and amination reagent is 11-13:95-97:36-40; 3. Load The polygonum cuspidatum extract is mixed with deionized water, Tween 80 and coconut oil diethanolamide are added for ultrasonic treatment, the ultrasonic time is 13-17 minutes, the ultrasonic frequency is 28-32kHz, after the ultrasonic treatment, a solution containing the polygonum cuspidatum extract is obtained, a functional carrier is added to the solution containing the polygonum cuspidatum extract, and the ultrasonic treatment is continued, the ultrasonic time is 17-23 minutes, after the ultrasonic treatment, the solution is dried to obtain a functional extract; The mass ratio of the knotweed extract, deionized water, Tween 80, and coconut oil diethanolamide is 9-11:85-90:1.2-1.4:0.8-1.2; The mass ratio of the solution containing the knotweed extract to the functional carrier is 13:3.5-3.9.

[0007] 4. Preparation of Functional Molecular Nests (1) Aldehyde-modified guar gum The guar gum and deionized water are mixed, stirred evenly, and then sodium periodate is slowly added at a rate of 0.3-0.5 g / min. After the addition is completed, the temperature is controlled to be 32-36° C., and the reaction is carried out in the dark for 13-15 hours. Then, ethylene glycol is added to terminate the reaction, dialyzed for 3 days, precooled and dried for 1.1-1.3 hours at a precooling temperature of -25 to -23° C., and then freeze-dried for 22-26 hours at a freezing temperature of -48 to -45° C. After the freezing is completed, the aldehyded guar gum is obtained; The mass volume ratio of the guar gum, deionized water, sodium periodate and ethylene glycol is 9-11 g:93-100 g:8.2-8.6 g:194-205 mL; (2) Reaction Place the aldehyde-modified guar gum in dimethyl sulfoxide, stir for 1.1-1.3 hours, then add the functional extract, heat to 58-62°C at a rate of 1.8-2.2°C / min, react for 7.3-7.7 hours, naturally lower to room temperature after the reaction is completed, and then dry, then add sodium borohydride solution, lower the temperature to 3.5-3.7°C, perform reduction reaction, and the reaction time is 2.1-2.5 hours. After the reaction is completed, dry to obtain a functional molecular nest; The concentration of the sodium borohydride solution is 0.008-0.012 g / mL; The mass ratio of the aldehyded guar gum, dimethyl sulfoxide, functional extract and sodium borohydride solution is 0.5-0.7 g: 9-11 mL: 1.0-1.2 g: 0.4-0.6 g.

[0008] 5.PE resin modification The PE resin is placed in 7-9 times the volume of the modification liquid for homogenization, the homogenization time is 3-5 minutes, the homogenization pressure is 4.8-5.2MPa, the homogenization times are 2 times, and after the homogenization, it is impregnated at a temperature of 68-72°C and a time of 55-59 minutes. After the impregnation, it is cooled to room temperature and dried to obtain a modified PE resin; The melt index of the PE resin is 2.6-3.0 g / min; The modified liquid is a mixture of deionized water, polyethylene glycol 600 and nonylphenol polyoxyethylene ether sulfonate, and the mass ratio of the deionized water, polyethylene glycol 600 and nonylphenol polyoxyethylene ether sulfonate is 115-125:2.8-3.2:1.6-1.8.

[0009] 6. Mixing and granulation After mixing the functional molecular nest, modified PE resin, antioxidant 1010 and oleic acid amide, the mixture is put into a mixer for high-speed stirring, the high-speed stirring speed is controlled to be 750-768rpm, the high-speed stirring time is 5.6-5.8min, and after the high-speed stirring is completed, the mixture is placed in a twin-screw extruder for extrusion granulation, and the extrusion temperature is controlled to be 193-197°C to obtain PE masterbatch; The mass ratio of the functional molecular nest, the modified PE resin, the antioxidant 1010 and the oleic acid amide is 2.4-2.8:73-77:0.3-0.5:0.8-1.2.

[0010] Compared with the prior art, the present invention has achieved the following beneficial effects: 1. The present invention adopts a functional carrier to load the polygonum cuspidatum extract. In the preparation process of the functional carrier, the medical stone is firstly activated, and under the action of the mechanical force of the ball mill, the lattice defects and distortions of the medical stone particles are removed, and the surface activity is improved by combining with a surfactant, so that the medical stone particles are in a state of being dispersed separately, and then the polygonum cuspidatum extract is loaded after amino treatment, so that the polygonum cuspidatum extract is fully loaded into the holes of the medical stone particles, and the loss of the polygonum cuspidatum extract is reduced. The medical stone after the amino treatment is rich in amino groups, which provides more reactive sites for the medical stone particles. In the reaction step, the medical stone is subjected to an amino treatment with aldehyded guar gum. The present invention is to carry out a reaction, and after reduction with sodium borohydride, the binding force of guar gum and medical stone is stronger, the performance of the obtained functional molecular nest is more stable, and the load of the knotweed extract is more stable, thereby improving the antibacterial and antioxidant properties of the PE masterbatch, and enhancing the mechanical properties, and reducing the loss of mechanical properties under strong ultraviolet irradiation; the present invention modifies the PE resin, improves the surface activation and wetting properties of the PE resin, and enhances the compatibility with the functional molecular nest. In the mixing and granulation step, the components are evenly dispersed and have good compatibility. The obtained PE masterbatch has good homogeneity, strong antibacterial properties, good antioxidant capacity, and excellent and stable mechanical properties; 2. The PE plastic masterbatch prepared by the present invention is prepared into a test sample, and the tensile strength is 21.4-23.8MPa, the bending modulus is 1291-1308MPa, and the simply supported beam impact strength at -48°C is 18.4-20.3kJ / m 2 ; 3. The PE plastic masterbatch prepared by the present invention is prepared into a test sample, and the inhibition rate of Staphylococcus aureus is 93.8-95.2%, the inhibition rate of Escherichia coli is 92.7-93.7%, and the inhibition rate of Klebsiella pneumoniae is 93.1-94.0%; 4. The PE plastic masterbatch prepared by the present invention is prepared into a test sample, and the free radical removal rate is 95.0-96.8%; 5. The PE plastic masterbatch prepared in the present invention was prepared into a test sample and placed under ultraviolet light with an intensity of 820 W / m 2 After standing for 15 days in an environment, the tensile strength is 20.7-23.3MPa and the flexural modulus is 1230-1261MPa. DETAILED DESCRIPTION

[0011] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.

[0012] Example 1 1. Preparation of Polygonum cuspidatum Extract The polygonum cuspidatum was washed, dried at 125°C, and then crushed. After the crushing, it was placed in 3.5 times the volume of ethanol solution for ultrasonic extraction. The ultrasonic time was 4.5 hours, the ultrasonic temperature was 42°C, and the ultrasonic frequency was 27kHz. After the ultrasonic extraction, it was filtered to remove the filter residue to obtain a filtrate. The filtrate was vacuum concentrated to 30% of the original volume, the concentration temperature was controlled to 65°C, the vacuum degree was 0.07MPa, and spray-dried to obtain a polygonum cuspidatum extract. The volume concentration of the ethanol solution is 55%.

[0013] 2. Preparation of functional carriers (1) Medical stone pretreatment The medical stone is placed in a sodium hydroxide solution of 5 times the volume for soaking, the soaking time is 2.5 hours, the soaking temperature is 60°C, and after the soaking is completed, it is dried to obtain the medical stone after alkali soaking; the medical stone after alkali soaking is placed in deionized water of 7 times the mass, cocamidopropyl betaine and polyethylene glycol monolaurate are added for ball milling, the ball milling time is 30 minutes, the ball milling speed is 140rpm, the ball-to-material ratio is 5:1, the ball milling temperature is 52°C, after the ball milling is completed, it is naturally reduced to room temperature, and dried to obtain the pretreated medical stone; The particle size of the medical stone is 270nm; The mass concentration of the sodium hydroxide solution is 40%; The mass ratio of the medical stone, cocamidopropyl betaine and polyethylene glycol monolaurate after alkali leaching is 12:1.0:1.1; (2) Amination The pretreated medical stone was placed in an ammonia solution and stirred at a temperature of 28°C for 7 minutes. After stirring evenly, an amination reagent was added and stirred evenly, and microwave heating was performed. The microwave power was 230W and the microwave time was 7 minutes. After the microwave was finished, the temperature was raised to 94°C at a rate of 1.3°C / min, and the stirring reaction was performed. The stirring speed was 205rpm and the stirring time was 6 hours. After the reaction was finished, the functional carrier was washed and dried to obtain the functional carrier. The mass concentration of the ammonia solution is 23%; The amination agent is a mixture of ethylenediamine and diethylenetriamine, and the mass ratio of ethylenediamine to diethylenetriamine is 1.5:1.3; The mass ratio of the pretreated medical stone, ammonia solution and amination reagent is 12:96:38; 3. Load The polygonum cuspidatum extract was mixed with deionized water, Tween 80 and coconut oil diethanolamide were added for ultrasonic treatment, the ultrasonic time was 15 minutes, the ultrasonic frequency was 30kHz, after the ultrasonic treatment, a solution containing the polygonum cuspidatum extract was obtained, a functional carrier was added to the solution containing the polygonum cuspidatum extract, and the ultrasonic treatment was continued for 20 minutes. After the ultrasonic treatment, the solution was dried to obtain a functional extract; The mass ratio of the knotweed extract, deionized water, Tween 80, and coconut oil diethanolamide is 10:87:1.3:1.0; The mass ratio of the solution containing the knotweed extract to the functional carrier is 13:3.7.

[0014] 4. Preparation of Functional Molecular Nests (1) Aldehyde-modified guar gum The guar gum was mixed with deionized water, stirred evenly, and then sodium periodate was slowly added at a rate of 0.4 g / min. After the addition was completed, the temperature was controlled to be 34°C, and the reaction was carried out in the dark for 14 hours. Then, ethylene glycol was added to terminate the reaction, dialyzed for 3 days, and precooled and dried for 1.2 hours at a precooling temperature of -24°C. Then, freeze-dried for 24 hours at a freezing temperature of -47°C. After the freezing was completed, the aldehyded guar gum was obtained. The mass volume ratio of the guar gum, deionized water, sodium periodate and ethylene glycol is 10g:97g:8.4g:200mL; (2) Reaction The aldehyde-modified guar gum was placed in dimethyl sulfoxide and stirred for 1.2 hours. Then, the functional extract was added and the temperature was raised to 60°C at a rate of 2.0°C / min. The reaction was carried out for 7.5 hours. After the reaction was completed, the temperature was naturally lowered to room temperature and then dried. Then, sodium borohydride solution was added and the temperature was lowered to 3.6°C for reduction reaction. The reaction time was 2.3 hours. After the reaction was completed, the temperature was dried to obtain a functional molecular nest. The concentration of the sodium borohydride solution is 0.01 g / mL; The mass ratio of the aldehyded guar gum, dimethyl sulfoxide, functional extract and sodium borohydride solution is 0.6g:10mL:1.1g:0.5g.

[0015] 5.PE resin modification The PE resin was placed in 8 times the volume of the modification liquid for homogenization, the homogenization time was 4 minutes, the homogenization pressure was 5.0 MPa, the homogenization times were 2 times, and after the homogenization, it was impregnated at 70°C for 57 minutes. After the impregnation, it was cooled to room temperature and dried to obtain the modified PE resin; The melt index of the PE resin is 2.8 g / min; The modified liquid is a mixture of deionized water, polyethylene glycol 600, and nonylphenol polyoxyethylene ether sulfonate, and the mass ratio of the deionized water, polyethylene glycol 600, and nonylphenol polyoxyethylene ether sulfonate is 120:3.0:1.7.

[0016] 6. Mixing and granulation The functional molecular nest, modified PE resin, antioxidant 1010 and oleic acid amide were mixed and put into a mixer for high-speed stirring. The high-speed stirring speed was controlled to be 760 rpm and the high-speed stirring time was 5.7 min. After the high-speed stirring, the mixture was placed in a twin-screw extruder for extrusion granulation. The extrusion temperature was controlled to be 195° C. to obtain PE masterbatch. The mass ratio of the functional molecular nest, the modified PE resin, the antioxidant 1010 and the oleic acid amide is 2.6:75:0.4:1.0.

[0017] Example 2 1. Preparation of Polygonum cuspidatum Extract The polygonum cuspidatum was washed, dried at 123°C, and then crushed. After the crushing, it was placed in a 3.0 times volume of ethanol solution for ultrasonic extraction. The ultrasonic time was 4.3 hours, the ultrasonic temperature was 40°C, and the ultrasonic frequency was 26kHz. After the ultrasonic extraction, it was filtered to remove the filter residue to obtain a filtrate. The filtrate was vacuum concentrated to 28% of the original volume. The concentration temperature was controlled to be 63°C and the vacuum degree was 0.06MPa. After spray drying, a polygonum cuspidatum extract was obtained. The volume concentration of the ethanol solution is 53%.

[0018] 2. Preparation of functional carriers (1) Medical stone pretreatment The medical stone is placed in a sodium hydroxide solution of 4.5 times the volume for soaking, the soaking time is 2.4 hours, the soaking temperature is 58°C, and after the soaking is completed, it is dried to obtain the medical stone after alkali soaking; the medical stone after alkali soaking is placed in deionized water of 6 times the mass, cocamidopropyl betaine and polyethylene glycol monolaurate are added for ball milling, the ball milling time is 28 minutes, the ball milling speed is 137rpm, the ball-to-material ratio is 4:1, the ball milling temperature is 50°C, after the ball milling is completed, it is naturally reduced to room temperature, and dried to obtain the pretreated medical stone; The particle size of the medical stone is 264nm; The mass concentration of the sodium hydroxide solution is 38%; The mass ratio of the medical stone, cocamidopropyl betaine and polyethylene glycol monolaurate after alkali leaching is 10:0.8:0.9; (2) Amination The pretreated medical stone was placed in an ammonia solution and stirred at a temperature of 26°C for 6 minutes. After stirring evenly, an amination reagent was added and stirred evenly, and microwave heating was performed. The microwave power was 227W and the microwave time was 5 minutes. After the microwave was finished, the temperature was raised to 92°C at a rate of 1.2°C / min, and the stirring reaction was performed. The stirring speed was 200rpm and the stirring time was 5.7 hours. After the reaction was finished, the functional carrier was washed and dried to obtain the functional carrier. The mass concentration of the ammonia solution is 22%; The amination agent is a mixture of ethylenediamine and diethylenetriamine, and the mass ratio of ethylenediamine to diethylenetriamine is 1.4:1.2; The mass ratio of the pretreated medical stone, ammonia solution and amination reagent is 11:95:36; 3. Load The polygonum cuspidatum extract was mixed with deionized water, Tween 80 and coconut oil diethanolamide were added for ultrasonic treatment, the ultrasonic time was 13 minutes, the ultrasonic frequency was 28 kHz, after the ultrasonic treatment, a solution containing the polygonum cuspidatum extract was obtained, a functional carrier was added to the solution containing the polygonum cuspidatum extract, and the ultrasonic treatment was continued for 17 minutes. After the ultrasonic treatment, the solution was dried to obtain a functional extract; The mass ratio of the knotweed extract, deionized water, Tween 80, and coconut oil diethanolamide is 9:85:1.2:0.8; The mass ratio of the solution containing the knotweed extract to the functional carrier is 13:3.5.

[0019] 4. Preparation of Functional Molecular Nests (1) Aldehyde-modified guar gum The guar gum was mixed with deionized water, stirred evenly, and then sodium periodate was slowly added at a rate of 0.3 g / min. After the addition was completed, the temperature was controlled to be 32° C., and the reaction was carried out in the dark for 13 hours. Then, ethylene glycol was added to terminate the reaction, dialyzed for 3 days, and precooled and dried for 1.1 hours at a precooling temperature of -25° C. Then, freeze-dried for 22 hours at a freezing temperature of -48° C. After the freezing was completed, aldehyde-modified guar gum was obtained. The mass volume ratio of the guar gum, deionized water, sodium periodate, and ethylene glycol is 9g:93g:8.2g:194mL; (2) Reaction The aldehyde-modified guar gum was placed in dimethyl sulfoxide and stirred for 1.1 hours, and then the functional extract was added, and the temperature was raised to 58°C at a rate of 1.8°C / min, and the reaction was carried out for 7.3 hours. After the reaction was completed, the temperature was naturally lowered to room temperature and then dried. Then, sodium borohydride solution was added, and the temperature was lowered to 3.5°C for reduction reaction. The reaction time was 2.1 hours. After the reaction was completed, it was dried to obtain a functional molecular nest. The concentration of the sodium borohydride solution is 0.008 g / mL; The mass ratio of the aldehyded guar gum, dimethyl sulfoxide, functional extract and sodium borohydride solution is 0.5g:9mL:1.0g:0.4g.

[0020] 5.PE resin modification The PE resin was placed in 7 times the volume of the modification liquid for homogenization, the homogenization time was 3 minutes, the homogenization pressure was 4.8 MPa, the homogenization times were 2 times, and after the homogenization, it was impregnated at 68°C for 55 minutes. After the impregnation, it was cooled to room temperature and dried to obtain the modified PE resin; The melt index of the PE resin is 2.6 g / min; The modified liquid is a mixture of deionized water, polyethylene glycol 600, and nonylphenol polyoxyethylene ether sulfonate, and the mass ratio of the deionized water, polyethylene glycol 600, and nonylphenol polyoxyethylene ether sulfonate is 115:2.8:1.6.

[0021] 6. Mixing and granulation The functional molecular nest, modified PE resin, antioxidant 1010 and oleic acid amide were mixed and put into a mixer for high-speed stirring. The high-speed stirring speed was controlled to be 750 rpm and the high-speed stirring time was 5.6 min. After the high-speed stirring, the mixture was placed in a twin-screw extruder for extrusion granulation. The extrusion temperature was controlled to be 193°C to obtain PE masterbatch. The mass ratio of the functional molecular nest, the modified PE resin, the antioxidant 1010 and the oleic acid amide is 2.4:73:0.3:0.8.

[0022] Example 3 1. Preparation of Polygonum cuspidatum Extract The polygonum cuspidatum was washed, dried at 128°C, and then crushed. After the crushing, it was placed in a 4.0 times volume of ethanol solution for ultrasonic extraction. The ultrasonic time was 4.7 hours, the ultrasonic temperature was 44°C, and the ultrasonic frequency was 28kHz. After the ultrasonic extraction, it was filtered to remove the filter residue to obtain a filtrate. The filtrate was vacuum concentrated to 32% of the original volume. The concentration temperature was controlled to be 67°C and the vacuum degree was 0.08MPa. After spray drying, a polygonum cuspidatum extract was obtained. The volume concentration of the ethanol solution is 57%.

[0023] 2. Preparation of functional carriers (1) Medical stone pretreatment The medical stone is placed in a sodium hydroxide solution of 5.5 times the volume for soaking, the soaking time is 2.6 hours, the soaking temperature is 62°C, and after the soaking is completed, it is dried to obtain the medical stone after alkali soaking; the medical stone after alkali soaking is placed in deionized water of 8 times the mass, cocamidopropyl betaine and polyethylene glycol monolaurate are added for ball milling, the ball milling time is 32 minutes, the ball milling speed is 143rpm, the ball-to-material ratio is 6:1, the ball milling temperature is 54°C, after the ball milling is completed, it is naturally reduced to room temperature, and dried to obtain the pretreated medical stone; The particle size of the medical stone is 276nm; The mass concentration of the sodium hydroxide solution is 42%; The mass ratio of the medical stone, cocamidopropyl betaine and polyethylene glycol monolaurate after alkali leaching is 14:1.1:1.3; (2) Amination The pretreated medical stone was placed in an ammonia solution and stirred at a temperature of 30°C for 8 minutes. After stirring evenly, an amination reagent was added and stirred evenly, and microwave heating was performed. The microwave power was 233W and the microwave time was 9 minutes. After the microwave was finished, the temperature was raised to 96°C at a rate of 1.4°C / min, and the stirring reaction was performed. The stirring speed was 212rpm and the stirring time was 6.3h. After the reaction was finished, the functional carrier was washed and dried to obtain the functional carrier. The mass concentration of the ammonia solution is 24%; The amination agent is a mixture of ethylenediamine and diethylenetriamine, and the mass ratio of ethylenediamine to diethylenetriamine is 1.6:1.4; The mass ratio of the pretreated medical stone, ammonia solution and amination reagent is 13:97:40; 3. Load The polygonum cuspidatum extract was mixed with deionized water, Tween 80 and coconut oil diethanolamide were added for ultrasonic treatment, the ultrasonic time was 17 minutes, the ultrasonic frequency was 32kHz, after the ultrasonic treatment, a solution containing the polygonum cuspidatum extract was obtained, a functional carrier was added to the solution containing the polygonum cuspidatum extract, and the ultrasonic treatment was continued for 23 minutes. After the ultrasonic treatment, the solution was dried to obtain a functional extract; The mass ratio of the knotweed extract, deionized water, Tween 80, and coconut oil diethanolamide is 11:90:1.4:1.2; The mass ratio of the solution containing the knotweed extract to the functional carrier is 13:3.9.

[0024] 4. Preparation of Functional Molecular Nests (1) Aldehyde-modified guar gum The guar gum was mixed with deionized water, stirred evenly, and then sodium periodate was slowly added at a rate of 0.5 g / min. After the addition was completed, the temperature was controlled to be 36°C, and the reaction was carried out in the dark for 15 hours. Then, ethylene glycol was added to terminate the reaction, dialyzed for 3 days, and precooled and dried for 1.3 hours at a precooling temperature of -23°C. Then, freeze-dried for 26 hours at a freezing temperature of -45°C. After the freezing was completed, the aldehyde-modified guar gum was obtained. The mass volume ratio of the guar gum, deionized water, sodium periodate and ethylene glycol is 11 g:100 g:8.6 g:205 mL; (2) Reaction The aldehyde-modified guar gum was placed in dimethyl sulfoxide and stirred for 1.3 hours, then the functional extract was added, the temperature was raised to 62°C at a rate of 2.2°C / min, the reaction was carried out for 7.7 hours, after the reaction was completed, the temperature was naturally lowered to room temperature and then dried, then sodium borohydride solution was added, the temperature was lowered to 3.7°C, a reduction reaction was carried out, the reaction time was 2.5 hours, after the reaction was completed, the temperature was dried to obtain a functional molecular nest; The concentration of the sodium borohydride solution is 0.012 g / mL; The mass ratio of the aldehyded guar gum, dimethyl sulfoxide, functional extract and sodium borohydride solution is 0.7g:11mL:1.2g:0.6g.

[0025] 5.PE resin modification The PE resin was placed in 9 times the volume of the modification liquid for homogenization, the homogenization time was 5 minutes, the homogenization pressure was 5.2 MPa, the homogenization times were 2 times, and after the homogenization, it was impregnated at a temperature of 72°C and a time of 59 minutes. After the impregnation, it was cooled to room temperature and dried to obtain a modified PE resin; The melt index of the PE resin is 3.0 g / min; The modified liquid is a mixture of deionized water, polyethylene glycol 600, and nonylphenol polyoxyethylene ether sulfonate, and the mass ratio of the deionized water, polyethylene glycol 600, and nonylphenol polyoxyethylene ether sulfonate is 125:3.2:1.8.

[0026] 6. Mixing and granulation The functional molecular nest, modified PE resin, antioxidant 1010 and oleic acid amide were mixed and put into a mixer for high-speed stirring. The high-speed stirring speed was controlled to be 768 rpm and the high-speed stirring time was 5.8 min. After the high-speed stirring, the mixture was placed in a twin-screw extruder for extrusion granulation. The extrusion temperature was controlled to be 197°C to obtain PE masterbatch. The mass ratio of the functional molecular nest, the modified PE resin, the antioxidant 1010 and the oleic acid amide is 2.8:77:0.5:1.2.

[0027] Comparative Example 1 Based on Example 1, the changes are that the medical stone pretreatment and amination steps are omitted; in the loading step, the functional carrier is replaced by medical stone without any treatment in equal amounts, and the particle size of the medical stone is 270 nm; The rest of the operations are the same.

[0028] Comparative Example 2 Based on Example 1, the changes are as follows: (1) The aldehyde-modified guar gum step is omitted, and the aldehyde-modified guar gum is replaced with an equal amount of untreated guar gum in the reaction step; (2) The PE resin modification step is omitted, and in the mixing and granulation step, the modified PE resin is replaced by an equal amount of an untreated PE resin, wherein the melt index of the PE resin is 2.8 g / min; The rest of the operations are the same.

[0029] Test Example 1 The PE masterbatches of Examples 1-3 and Comparative Examples 1-2 were prepared into test specimens, and then the mechanical properties of the test specimens were tested. The specific results are as follows:

[0030] Test Example 2 The PE masterbatches of Examples 1-3 and Comparative Examples 1-2 were prepared into test samples, and then the antibacterial properties of the test samples were tested. The specific results are as follows:

[0031] Test Example 3 The PE masterbatches of Examples 1-3 and Comparative Examples 1-2 were prepared into test samples, and then the antioxidant capacity of the test samples was tested. The specific results are as follows:

[0032] Test Example 4 The PE plastic masterbatch of Examples 1-3 and Comparative Examples 1-2 was prepared into test samples, and then the test samples were placed in an ultraviolet light with an intensity of 820 W / m 2 After standing for 15 days in an environment, the performance of the test sample was tested again. The specific results are as follows:

[0033] The invention adopts a functional carrier to load the knotweed extract. In the preparation process of the functional carrier, the medical stone is firstly activated, and under the action of the mechanical force of the ball mill, the medical stone particles are lattice defective and distorted, and the surface activity is improved by combining with a surfactant, so that the medical stone particles are in a state of being dispersed separately, and then the knotweed extract is loaded after amino treatment, so that the knotweed extract is fully loaded into the holes of the medical stone particles, and the loss of the knotweed extract is reduced. The medical stone after the amino treatment is rich in amino groups, which provides more reactive sites for the medical stone particles. In the reaction step, the medical stone is subjected to an amino treatment with aldehyded guar gum. The invention relates to a method for preparing a PE masterbatch comprising: performing a reaction, reducing the PE masterbatch with sodium borohydride, so that the binding force of guar gum and medical stone is stronger, the performance of the obtained functional molecular nest is more stable, and the load of the polygonum cuspidatum extract is more stable, thereby improving the antibacterial and antioxidant properties of the PE masterbatch, enhancing the mechanical properties, and reducing the loss of the mechanical properties under strong ultraviolet irradiation; the invention modifies the PE resin, improves the surface activation and wetting properties of the PE resin, and enhances the compatibility with the functional molecular nest; in the mixing and granulating step, the components are evenly dispersed and have good compatibility; the obtained PE masterbatch has good homogeneity, strong antibacterial properties, good antioxidant capacity, and excellent and stable mechanical properties.

[0034] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.

[0035] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract, characterized in that: The preparation method comprises the steps of preparing a knotweed extract, preparing a functional carrier, loading, preparing a functional molecular nest, modifying a PE resin, and mixing and granulating; The preparation of the functional carrier comprises the steps of pretreatment of medical stone and amination; The steps of pre-treating the medical stone are as follows: soaking the medical stone in a sodium hydroxide solution of 4.5-5.5 times the volume, the soaking time is 2.4-2.6 hours, the soaking temperature is 58-62° C., and after the soaking, drying to obtain the medical stone after alkali soaking; placing the medical stone after alkali soaking in deionized water of 6-8 times the mass, adding cocamidopropyl betaine and polyethylene glycol monolaurate to carry out ball milling treatment, the ball milling time is 28-32 minutes, the ball milling speed is 137-143rpm, the ball-to-material ratio is 4-6:1, the ball milling temperature is 50-54° C., after the ball milling is completed, naturally lowering to room temperature, drying, and obtaining the pre-treated medical stone; The amination step comprises placing the pretreated medical stone in an ammonia solution, stirring at a temperature of 26-30° C. for 6-8 min, adding an amination agent after stirring evenly, and performing microwave heating treatment after stirring evenly, wherein the microwave power is 227-233 W and the microwave time is 5-9 min. After the microwave is finished, the temperature is raised to 92-96° C. at a rate of 1.2-1.4° C. / min, and the stirring reaction is performed, the stirring speed is 200-212 rpm, and the stirring time is 5.7-6.3 h. After the reaction is finished, washing and drying are performed to obtain a functional carrier; The amination agent is a mixture of ethylenediamine and diethylenetriamine; The preparation of the functional molecular nest comprises the steps of aldehyde-forming guar gum and reacting; The steps of aldehyde-forming guar gum are as follows: guar gum is mixed with deionized water, stirred evenly, and then sodium periodate is slowly added at a rate of 0.3-0.5 g / min. After the addition is completed, the temperature is controlled to be 32-36° C., and the reaction is carried out in the dark for 13-15 hours. Then, ethylene glycol is added to terminate the reaction, dialyzed for 3 days, precooled and dried for 1.1-1.3 hours at a precooling temperature of -25 to -23° C., and then freeze-dried for 22-26 hours at a freezing temperature of -48 to -45° C. After the freezing is completed, the aldehyde-forming guar gum is obtained. The reaction steps are as follows: placing the aldehyded guar gum in dimethyl sulfoxide, stirring for 1.1-1.3 hours, then adding the functional extract, heating to 58-62°C at a rate of 1.8-2.2°C / min, reacting for 7.3-7.7 hours, naturally lowering to room temperature and drying after the reaction, then adding sodium borohydride solution, lowering the temperature to 3.5-3.7°C, performing a reduction reaction, and the reaction time is 2.1-2.5 hours. After the reaction is completed, drying is performed to obtain a functional molecular nest; The PE resin modification step is to place the PE resin in a 7-9 times volume of the modification liquid for homogenization, the homogenization time is 3-5 minutes, the homogenization pressure is 4.8-5.2MPa, the homogenization times are 2 times, and after the homogenization treatment, the resin is impregnated at a temperature of 68-72°C and a time of 55-59 minutes. After the impregnation, the resin is cooled to room temperature and dried to obtain the modified PE resin. The modified liquid is a mixture of deionized water, polyethylene glycol 600 and nonylphenol polyoxyethylene ether sulfonate.

2. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: The steps of preparing the polygonum cuspidatum extract are: washing the polygonum cuspidatum, drying it at 123-128° C., and then crushing it; after the crushing, placing it in a 3.0-4.0 times volume of ethanol solution for ultrasonic extraction, the ultrasonic time is 4.3-4.7h, the ultrasonic temperature is 40-44° C., and the ultrasonic frequency is 26-28kHz; after the ultrasonic extraction is completed, filtering is performed to remove the filter residue to obtain a filtrate, and the filtrate is vacuum concentrated to 28-32% of the original volume, the concentration temperature is controlled to be 63-67° C., the vacuum degree is 0.06-0.08MPa, and spray drying is performed to obtain the polygonum cuspidatum extract; The volume concentration of the ethanol solution is 53-57%.

3. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: In the step of pre-treating the medical stone, the particle size of the medical stone is 264-276nm; The mass concentration of the sodium hydroxide solution is 38-42%; The mass ratio of the medical stone, cocamidopropyl betaine and polyethylene glycol monolaurate after alkali leaching is 10-14:0.8-1.1:0.9-1.

3.

4. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: In the amination step, the mass concentration of the ammonia solution is 22-24%; In the amination reagent, the mass ratio of ethylenediamine to diethylenetriamine is 1.4-1.6:1.2-1.4; The mass ratio of the pretreated medical stone, ammonia solution and amination reagent is 11-13:95-97:36-40.

5. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: The loading step comprises: mixing the polygonum cuspidatum extract with deionized water, adding Tween 80 and coconut oil diethanolamide for ultrasonic treatment, wherein the ultrasonic time is 13-17 minutes and the ultrasonic frequency is 28-32kHz. After the ultrasonic treatment, a solution containing the polygonum cuspidatum extract is obtained, and a functional carrier is added to the solution containing the polygonum cuspidatum extract, and the ultrasonic treatment is continued. The ultrasonic treatment time is 17-23 minutes. After the ultrasonic treatment, the solution is dried to obtain a functional extract. The mass ratio of the knotweed extract, deionized water, Tween 80, and coconut oil diethanolamide is 9-11:85-90:1.2-1.4:0.8-1.2; The mass ratio of the solution containing the knotweed extract to the functional carrier is 13:3.5-3.

9.

6. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: In the step of aldehyde-forming guar gum, the mass volume ratio of the guar gum, deionized water, sodium periodate and ethylene glycol is 9-11 g:93-100 g:8.2-8.6 g:194-205 mL.

7. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: In the step of the reaction, the concentration of the sodium borohydride solution is 0.008-0.012 g / mL; The mass ratio of the aldehyded guar gum, dimethyl sulfoxide, functional extract and sodium borohydride solution is 0.5-0.7 g: 9-11 mL: 1.0-1.2 g: 0.4-0.6 g.

8. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: In the step of modifying the PE resin, the melt index of the PE resin is 2.6-3.0 g / min; In the modified liquid, the mass ratio of the deionized water, polyethylene glycol 600, and nonylphenol polyoxyethylene ether sulfonate is 115-125:2.8-3.2:1.6-1.

8.

9. The method for preparing antibacterial and antioxidant PE plastic masterbatch modified with Polygonum cuspidatum extract according to claim 1, characterized in that: The mixing and granulation step comprises: mixing the functional molecular nest, the modified PE resin, the antioxidant 1010 and the oleic acid amide, and then putting the mixture into a mixer for high-speed stirring, wherein the high-speed stirring speed is controlled to be 750-768 rpm, and the high-speed stirring time is 5.6-5.8 min. After the high-speed stirring is completed, the mixture is placed in a twin-screw extruder for extrusion granulation, and the extrusion temperature is controlled to be 193-197° C., so as to obtain a PE masterbatch; The mass ratio of the functional molecular nest, the modified PE resin, the antioxidant 1010 and the oleic acid amide is 2.4-2.8:73-77:0.3-0.5:0.8-1.2.

Citation Information

Cited By

  • Antibacterial cool-feeling polyester fiber containing plant extract, textile and preparation method of antibacterial cool-feeling polyester fiber