Preparation method of P (VDF-TrFE-CFE) ferroelectric polymer film
P(VDF-TrFE) ferroelectric polymer film was prepared by introducing CFE groups in P(VDF-TrFE) and spin coating using DMF and DMSO solvents, and the P(VDF-TrFE) ferroelectric polymer hysteresis and The problem of side effects of radiation has achieved efficient electrostrictive performance and film uniformity.
Patent Information
- Application Number
- CN202410907303.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-15
AI Technical Summary
There is a large hysteresis in the transition process between the ferroelectric phase and the non-ferroelectric phase at room temperature, and side effects caused by high-energy radiation such as free radical formation and chain breakage affect electricity. Scaling performance.
Use P(VDF-TrFE-CFE) terpolymer to replace P(VDF-TrFE), and prepare thin films by introducing large volume CFE groups into P(VDF-TrFE), combining mixed solvents of DMF and DMSO for spin coating. , avoid irradiation processes, simplify processing and improve the uniformity and flatness of the film.
It achieves a smaller hysteresis and a greater electrostrictive performance at room temperature, while avoiding adverse side effects caused by radiation, and improving the uniformity and flatness of the film.
Smart Images

Figure BDA0004932511250000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ferroelectric polymers, and more specifically relates to a method for preparing a P (VDF-TrFE-CFE) ferroelectric polymer film. Background Art
[0002] Ferroelectrics are technologically important smart materials that can be used in capacitors, sensors, transducers, nonvolatile memories, and electro-optic modulators. Ferroelectric polymers, especially vinylidene fluoride homopolymer PVDF and its random copolymer with trifluoroethylene P(VDF-TrFE)s, have attracted considerable attention for more than 30 years.
[0003] Among them, P(VDF-TrFE) is a ferroelectric polymer whose ferroelectric phase has an all-trans conformation. By heating the polymer above the ferroelectric, paraelectric (F, P) transition temperature, the ferroelectric phase is transformed into a paraelectric (non-polar) phase, which is a mixture of trans and torsion bonds. The change between the molecular conformations between these two phases leads to more than 7% strain. However, in P(VDF-TrFE) copolymers, this transition process occurs at temperatures close to 100°C and involves very large hysteresis. To address this, one of the solutions is to introduce defects through high-energy irradiation, breaking the long-range polar regions into microdomains, thereby stabilizing the non-polar phase at room temperature and significantly reducing or even eliminating the transition barrier between the polar phase and the non-polar phase. Therefore, at room temperature, an external electric field can induce a continuous transition from the non-polar phase to the polar phase with very little hysteresis. This process directly leads to large electrostrain because of the conformational change. Summary of the invention
[0004] The present invention aims to provide a method for preparing a P(VDF-TrFE-CFE) ferroelectric polymer film, which uses a P(VDF-TrFE-CFE) terpolymer to replace a P(VDF-TrFE) copolymer, and introduces a small amount of a bulky group (CFE) into the P(VDF-TrFE) to form the P(VDF-TrFE-CFE), thereby obtaining a smaller hysteresis and a larger electrostriction. The advantage of the terpolymer method is that it eliminates the irradiation process, thereby simplifying the processing of the electrostrictive polymer; and removes the adverse side effects caused by the polymer irradiation, such as the formation of free radicals, chain scission and cross-linking.
[0005] The P(VDF-TrFE-CFE) terpolymer is soluble in a highly polar organic solvent. The present invention dissolves the P(VDF-TrFE-CFE) terpolymer in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), and then spin-coats the film, thereby ensuring the solubility of the P(VDF-TrFE-CFE) terpolymer while also greatly improving the uniformity and flatness of the resulting film. DMSO has a higher dipole moment (4.1D at 20°C) and boiling point (189°C). When the volume ratio of DMF:DMSO is 1:1, the film formed exhibits good uniformity, while when the DMSO content is greater than 50%, the solution viscosity is too high, which is not conducive to drop casting and spin coating of uniform films.
[0006] In order to achieve the above object, the present invention is implemented by the following technical scheme: a method for preparing a P (VDF-TrFE-CFE) ferroelectric polymer film, comprising the following steps:
[0007] Step 1: Add the P(VDF-TrFE-CFE) trimer powder into a mixed solution of DMF and DMSO and stir to fully dissolve it;
[0008] Step 2: Spin coating the obtained polymer solution into a film and drying it;
[0009] Step 3: The obtained film is subjected to vacuum annealing.
[0010] Further preferably, the volume ratio of DMF to DMSO in the mixed solution is 1:1.
[0011] More preferably, the ratio of the amount of the P(VDF-TrFE-CFE) trimer powder to the amount of the mixed solution is 0.2-0.4 g:5 mL.
[0012] More preferably, the particle size of the P(VDF-TrFE-CFE) terpolymer powder is 1-5 μm.
[0013] Further preferably, the stirring time is not shorter than 12 h.
[0014] More preferably, the volume of the polymer solution used for spin coating the polymer solution into a film is 0.5-1.0 mL, and the spin coating thickness is 10-15 μm.
[0015] Further preferably, the spin coating has a rotation speed of 200-250 rpm, a time of 10-30 s, and an acceleration of 30-50 r / s.
[0016] The film formation is most ideal when prepared at this spin coating speed, time, acceleration and solution dosage.
[0017] More preferably, the drying is carried out in an oven at 60-70° C. for 12-14 hours.
[0018] Further preferably, the annealing is performed in a vacuum oven at 120-140° C. for 24-30 h, with a vacuum pressure of -0.3 MPa to -0.1 MPa.
[0019] The second technical solution of the present invention: a P (VDF-TrFE-CFE) ferroelectric polymer film prepared by the above preparation method.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] (1) The use of P(VDF-TrFE-CFE) instead of electron irradiation can avoid the adverse side effects caused by polymer irradiation.
[0022] (2) By dissolving the P(VDF-TrFE-CFE) terpolymer in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) and then spin coating the film, the solubility of the P(VDF-TrFE-CFE) terpolymer can be ensured while the uniformity and flatness of the obtained film can be greatly improved. DETAILED DESCRIPTION
[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0024] Example 1
[0025] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 1:1, and stir overnight (14 h) to fully dissolve it.
[0026] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0027] Example 2
[0028] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 1:1, and stir overnight (14 h) to fully dissolve it.
[0029] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0030] Step 3: Place the obtained film in a vacuum oven at 120°C for annealing for 24 hours with a vacuum pressure of -0.1 MPa.
[0031] Example 3
[0032] Step 1: Add 0.4 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 1:1, and stir overnight (14 h) to fully dissolve it.
[0033] Step 2: Drop 1.0 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 15 μm. The spin coater is set to a speed of 250 rpm, a spin time of 20 s, and an acceleration of 30 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0034] Example 4
[0035] Step 1: Add 0.4 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 1:1, and stir overnight (14 h) to fully dissolve it.
[0036] Step 2: Drop 1.0 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 15 μm. The spin coater is set to a speed of 250 rpm, a spin time of 20 s, and an acceleration of 30 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0037] Step 3: Place the obtained film in a vacuum oven at 120°C for annealing for 24 hours with a vacuum pressure of -0.2MPa.
[0038] Comparative Example 1
[0039] Step 1: Dissolve 0.3 g of P(VDF-TrFE) dimer powder in 5 mL of DMF solution and stir overnight (14 h) to allow it to fully dissolve.
[0040] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0041] Step 3: Place the obtained film in a vacuum oven at 120°C for annealing for 24 hours with a vacuum pressure of -0.1 MPa.
[0042] Comparative Example 2
[0043] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of DMF solution and stir overnight (14 h) to fully dissolve it.
[0044] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0045] Comparative Example 3
[0046] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of DMF solution and stir overnight (14 h) to fully dissolve it.
[0047] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0048] Step 3: Place the obtained film in a vacuum oven at 120°C for annealing for 24 hours with a vacuum pressure of -0.1 MPa.
[0049] Comparative Example 4
[0050] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of DMF solution and stir overnight (14 h) to fully dissolve it.
[0051] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0052] Step 3: Heat the obtained film to 135°C and keep it for 2 hours to remove the microstructure formed during the evaporation of DMF. The film is then quenched with 20°C water to freeze the microstructure.
[0053] Comparative Example 5
[0054] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of DMF solution and stir overnight (14 h) to fully dissolve it.
[0055] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0056] Step 3: Heat the obtained film to 135°C and keep it for 2 hours to remove the microstructure formed during the evaporation of DMF. The film is then quenched with 20°C water to freeze the microstructure.
[0057] Step 4: Place the obtained film in a vacuum oven at 120°C for annealing for 24 hours with a vacuum pressure of -0.1 MPa.
[0058] Comparative Example 6
[0059] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 4:6, and stir overnight (14 h) to fully dissolve it.
[0060] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0061] Comparative Example 7
[0062] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 4:6, and stir overnight (14 h) to fully dissolve it.
[0063] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0064] Step 3: Place the obtained film in a vacuum oven at 120°C for annealing for 24 hours with a vacuum pressure of -0.1 MPa.
[0065] Comparative Example 8
[0066] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 1:1, and stir overnight (14 h) to fully dissolve it.
[0067] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0068] Step 3: Heat the obtained film to 135°C and keep it for 2 hours. Then quench the film with 20°C water.
[0069] Comparative Example 9
[0070] Step 1: Add 0.3 g of P(VDF-TrFE-CFE) terpolymer powder into 5 mL of a mixed solution of DMF and DMSO in a volume ratio of 1:1, and stir overnight (14 h) to fully dissolve it.
[0071] Step 2: Drop 0.8 mL of the obtained polymer solution on a clean glass substrate and form a film by spin coating to obtain a film with a thickness of 12 μm. The spin coater is set to a speed of 200 rpm, a spin time of 20 s, and an acceleration of 50 r / s. Dry in an oven at 60°C for 12 h, and finally peel the film from the glass plate.
[0072] Step 3: Heat the obtained film to 120°C and keep it for 12 hours. Then quench the film with 20°C water.
[0073] The films prepared in the examples and comparative examples were placed in an electric field of 130 MV / m, and the strain in the thickness direction of each film was recorded. The strain records are shown in Table 1 below.
[0074] Table 1
[0075]
[0076] As shown in Table 1, compared with the P(VDF-TrFE) used in Comparative Example 1, the P(VDF-TrFE) used in Example 1 is different from the P(VDF-TrFE) which is mainly in the all-trans conformation (tttt), and a larger CFE monomer is introduced, so that a large number of tttg conformations are added to the P(VDF-TrFE-CFE). When an electric field is applied to it, the tttg conformation is transformed into the tttt conformation, thereby causing a change in the size of the molecular chain, which in turn causes the stretching strain.
[0077] Comparing Example 1 with Example 2, there is little difference in strain between Example 3 and Example 4. This is because for the configured solution, the tttg conformation that can be introduced by adding the polymer has almost reached saturation, so subsequent additions will no longer have a significant effect.
[0078] The reason why the film in Example 1 has a greater strain than that in Comparative Example 2 is that DMSO has a greater dipole moment than DMF. Therefore, the film made with DMSO and DMF as a mixed solvent has a greater strain than the film made with DMF alone.
[0079] Comparative Examples 6 and 7 have smaller strains than Comparative Examples 1 and 2. This is because the film formed when the DMF:DMSO ratio is 1:1 has the best uniformity, while when DMSO exceeds 50%, the viscosity of the solution is too high, and the uniformity of the formed film is poor, so the strain exhibited is also worse.
[0080] Comparing Example 1 with Example 2, and Comparative Example 2 with Comparative Example 3, it can be seen that annealing can increase the strain of the film. This may be due to the memory effect of the fluoropolymer, in which a portion of the ordered structure can be retained during annealing or melting and serve as the nucleus for subsequent crystal growth. During the high-temperature annealing process, a large amount of tttg in the film is retained, and it can even promote the growth of more tttg conformations. In other words, the annealing operation can obtain more tttg sequences, so that more polymer chains will flip under the action of the electric field, which in turn leads to the fact that the strain of the annealed film is generally greater than the strain of the unannealed film.
[0081] The film strain in Comparative Example 4 dropped suddenly because when the film was heated to 135°C, a large number of tttt conformations were generated, and when the tttt conformation had not yet been transformed into the tttg conformation, it was immediately quenched with 20°C water, freezing the microstructure, thus retaining a large number of tttt conformations and a small number of tttg conformations, which resulted in a lower strain of the film after the electric field was applied than in other embodiments. Even if the film in Comparative Example 5 was annealed again, its film strain was slightly lower than that in Comparative Example 3.
[0082] Comparative Example 9 has a smaller strain than Comparative Example 8. This is because low-temperature quenching from a higher temperature can freeze more tttt conformations. Therefore, compared with Comparative Example 8, Comparative Example 9 will have more tttg conformations after quenching at 120°C for a period of time, and thus the strain exhibited will be slightly greater than that of Comparative Example 8.
[0083] The above embodiments of the present invention are merely examples for illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all the embodiments here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a P (VDF-TrFE-CFE) ferroelectric polymer film, characterized in that: The steps include: Step 1: Add the P(VDF-TrFE-CFE) trimer powder into a mixed solution of DMF and DMSO and stir to fully dissolve it; Step 2: Spin coating the obtained polymer solution into a film and drying it; Step 3: The obtained film is subjected to vacuum annealing.
2. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer thin film according to claim 1, characterized in that: The volume ratio of DMF to DMSO in the mixed solution is 1:
1.
3. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer film according to claim 1, characterized in that: The ratio of the amount of the P(VDF-TrFE-CFE) trimer powder to the amount of the mixed solution is 0.2-0.4 g:5 mL.
4. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer film according to claim 1, characterized in that: The particle size of the P(VDF-TrFE-CFE) terpolymer powder is 1-5 μm.
5. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer film according to any one of claims 1 to 4, characterized in that: The stirring time should not be shorter than 12h.
6. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer film according to claim 1, characterized in that: When the polymer solution is spin-coated to form a film, the volume of the polymer solution used is 0.5-1.0 mL, and the spin-coating thickness is 10-15 μm.
7. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer film according to claim 1, characterized in that: The spin coating has a rotation speed of 200-250 rpm, a time of 10-30 s, and an acceleration of 30-50 r / s.
8. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer film according to claim 1, 6 or 7, characterized in that: The drying is carried out in an oven at 60-70° C. for 12-14 hours.
9. The method for preparing the P(VDF-TrFE-CFE) ferroelectric polymer film according to claim 1, 6 or 7, characterized in that: The annealing is performed in a vacuum oven at 120-140° C. for 24-30 hours, and the vacuum pressure is -0.3 MPa to -0.1 MPa.
10. A P(VDF-TrFE-CFE) ferroelectric polymer film prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Irradiation modified ferroelectric polymer and preparation method thereof
CN119978511A