Multifunctional PET-based supercritical carbon dioxide foaming material and preparation method thereof

Through the ball milling method, the electrostatic accumulation and conductive network construction problems of polymer-based foaming materials are solved, and the efficient and low-cost PET-based supercritical carbon dioxide foaming is achieved. The preparation of materials improves the antistatic properties and conductivity of materials.

CN118955990AActive Publication Date: 2024-11-15SICHUAN UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411184422.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The application of existing polymer-based foamed materials in high-end fields is limited by the electrostatic accumulation problems caused by their mechanical strength, heat resistance and high resistivity, and the commonly used conductive network construction processes are complex and costly.

Method used

The ball milling method is used to coat the carbon-based conductive filler PET beads, and combined with supercritical CO2 foaming technology, PET-based supercritical carbon dioxide foaming material with an isolated structure conductive network is prepared, reducing the amount of conductive filler added and improving antistatic properties. .

Benefits of technology

The preparation of PET-based supercritical carbon dioxide foaming materials with high antistatic properties has significantly reduced the amount of conductive filler added, reduced costs and increased efficiency, and improved conductivity under the same conditions. It is suitable for packaging, insulation and buffering materials. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955990A_ABST
    Figure CN118955990A_ABST
Patent Text Reader

Abstract

The invention provides a multifunctional PET (Polyethylene Terephthalate)-based supercritical carbon dioxide foaming material and a preparation method thereof, PET beads and a carbon-based conductive filler are subjected to ball-milling mixing treatment, so that the surface of the PET beads is coated with the carbon-based conductive filler, the carbon-based conductive filler is used as a blending material to be placed in a container for supercritical CO2 foaming, CO2 is introduced, and the carbon-based conductive filler is added into the container for supercritical CO2 foaming to prepare the multifunctional PET-based supercritical carbon dioxide foaming material. And carrying out supercritical CO2 foaming to prepare the PET-based supercritical carbon dioxide foaming material. According to the PET-based supercritical carbon dioxide foaming material and the preparation method thereof, the surfaces of PET beads are coated with the carbon-based conductive filler on the basis of a ball milling method, and the PET-based supercritical carbon dioxide foaming material with the antistatic performance of the conductive network with the isolation structure is prepared through a supercritical CO2 foaming technology; the addition amount of the used carbon-based conductive filler can be reduced by one order of magnitude, so that the purposes of greatly reducing cost and increasing efficiency are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of supercritical CO2-assisted PET-based bead foaming materials, and relates to a multifunctional PET-based supercritical carbon dioxide foaming material and a preparation method thereof, in particular to a PET-based supercritical carbon dioxide foaming material with multifunctional properties such as high antistatic properties and a preparation method thereof. Background Art

[0002] In the field of polymer materials, polymer-based foam materials have the advantages of light weight, heat insulation, sound absorption, etc. With the changing times, the demand for high performance and multifunctionality (such as antistatic performance, high flame retardancy, etc.) of polymer-based foam materials is increasing. However, the commonly used polymer-based foam materials are made of general plastics, and their mechanical strength and heat resistance are poor and cannot meet the needs of high-end fields such as aerospace and military industries, which greatly limits their application scope.

[0003] In addition, due to the high resistivity of polymer-based foam materials, electrostatic charge accumulation will inevitably occur during friction during actual use, which will affect precision electronic components and cause safety issues. In order to solve this problem, a conductive network structure or conductive layer is usually designed inside or outside the material. Among them, the introduction of a conductive network structure inside the material usually involves how the conductive phase is dispersed in the polymer matrix. The commonly used method is melt blending, which is suitable for large-scale production, but there are problems such as uneven dispersion of conductive fillers in the matrix and agglomeration. The prepared composite material is difficult to achieve ideal conductive properties. The method of setting a conductive layer on the outside of the material usually involves more complex technical methods and special equipment, which has a higher cost in actual industrialization.

[0004] Polyethylene terephthalate (PET) is an engineering plastic and a thermoplastic polyester with excellent mechanical properties and high temperature resistance. It is often used in the fields of automobiles, construction, and packaging. After being processed by the foaming process, PET-based foam materials not only retain the original excellent properties of PET, such as good heat resistance and mechanical strength, but also have excellent thermal insulation properties, low density, and environmental friendliness. However, PET-based foam materials also have the above-mentioned defects of high resistivity of polymer-based foam materials.

[0005] In order to solve the above problems, the Chinese invention patent "An omnidirectional conductive foam and its production method" (CN101431885B) discloses an omnidirectional conductive foam and its production method. The substrate of the conductive foam is a sheet of highly elastic foam sponge with polyester, polyether or PET as the main component, which is wrapped with a breathable mesh cloth. The thickness of the laminated foam is between 1-10mm. The surface of the conductive foam has a chemical copper plating layer, an electroplated nickel layer and a resin protective layer from the inside to the outside.

[0006] However, the above-mentioned prior art still has the disadvantages of complex process and high cost. Therefore, there is an urgent need for a PET-based foaming material with simple process, low cost and multifunctional properties such as high antistatic properties, so as to have better industrial application prospects. Summary of the invention

[0007] In order to solve the problems in the above-mentioned prior art, the present invention provides a multifunctional PET-based supercritical carbon dioxide foaming material and a preparation method thereof. Based on the ball milling method, carbon-based conductive fillers are coated on the surface of PET beads and supercritical CO2 foaming technology is used to prepare a PET-based supercritical carbon dioxide foaming material with an isolated structure conductive network and antistatic properties. Compared with the process of realizing the conductive network by melt blending, the addition amount of the carbon-based conductive filler used in the present invention can be reduced by one order of magnitude, so as to achieve the purpose of significantly reducing costs and increasing efficiency.

[0008] To achieve the above objectives, the present invention is implemented by adopting a technical solution consisting of the following technical measures.

[0009] The present invention provides a method for preparing a PET-based supercritical carbon dioxide foaming material, which mainly comprises the following steps:

[0010] (1) PET beads and carbon-based conductive fillers are mixed by ball milling, so that the carbon-based conductive fillers are coated on the surface of the PET beads, and the mixture is used as a blend;

[0011] The amount of the carbon-based conductive filler added is 0.8-1 wt% of the blend.

[0012] The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min;

[0013] (2) placing the blend obtained in step (1) in a supercritical CO2 foaming container, introducing CO2, and then maintaining the pressure for 3 to 6 hours at a pressure of 8 to 11 MPa and a temperature of 40 to 50° C. After the time is up, the temperature is raised to 243 to 247° C., and the foaming pressure is maintained at no more than 25 MPa during the heating process. After reaching the set temperature, the pressure is quickly released and the container is cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material.

[0014] In this article, the PET beads in step (1) are conventional polyethylene terephthalate (PET) bead raw materials, and usually chemical raw material grade PET bead raw materials can be directly selected and used, such as PET bead raw materials with models of CB602, FR530, CR8863, and CZ328.

[0015] In this article, the carbon-based conductive filler described in step (1) is a conventional carbon-based conductive filler that can construct a conductive network structure outside or inside a polymer matrix. In one technical solution, the carbon-based conductive filler described in step (1) includes any one of carbon nanotubes, nanographene, nanocarbon black, and carbon nanofibers.

[0016] In one of the technical solutions, in order to further expand the functionality of the prepared PET-based supercritical carbon dioxide foamed material, the PET beads and the carbon-based conductive filler are mixed by ball milling in step (1), so that the carbon-based conductive filler is coated on the surface of the PET beads, and then the PET beads are immersed in a flame retardant and then taken out so that the flame retardant adheres to the surface; the flame retardant is selected from the flame retardant conventionally added to the polymer-based foaming material, and the technicians in this field can select a suitable flame retardant according to the addible flame retardants recorded in the prior art literature or the existing process methods.

[0017] Furthermore, in order to better illustrate the present invention and provide a preferred technical scheme for reference, the above-mentioned flame retardant selection includes any one of DOPO-KH560 flame retardant, diphenyl sulfone thiophenylphosphonate (PSTPP), liquid flame retardant DTFR-6007, etc.; the DOPO-KH560 flame retardant is the flame retardant disclosed in the previous article by the applicant of the present invention (Lu Jin, Jia Lu, Liu Xingang, et al. Preparation and Properties of DOPO-KH560 Modified Polyethylene Oxide Polymer Solid Electrolyte [J]. Polymer Materials Science and Engineering, 2021. DOI: 10.16865 / j.cnki.1000-7555.2021.0054.).

[0018] It should be noted that, due to the fact that the blend obtained in step (1) is prone to moisture regain during transportation and storage of raw materials, it is advisable to dry it before foaming to minimize its moisture content, which helps to improve the stability of the subsequent preparation process. For example, the blend is dried at a temperature of 120-140° C. for at least 4 hours.

[0019] One of the inventive points of the present invention is that by selecting a ball milling method with appropriate process parameters, the carbon-based conductive filler is coated on the surface of the PET beads. First, it can effectively improve the dispersibility of the carbon-based conductive filler on the surface of the beads, reduce the agglomeration phenomenon, and is more conducive to the construction and integrity of the conductive network, thereby improving the antistatic performance. Secondly, by using the ball milling method to coat the carbon-based conductive filler on the surface of the PET beads, the amount of carbon-based conductive filler added can be significantly reduced while ensuring high antistatic performance. In particular, compared with the process of melt blending the carbon-based conductive filler with the polymer matrix to realize the conductive network, the amount of carbon-based conductive filler added can be reduced by an order of magnitude to achieve the purpose of significantly reducing costs and increasing efficiency. However, it should be noted that too high or too low ball milling parameters will significantly hinder the dispersion of carbon-based conductive fillers on the surface of the beads, resulting in filler agglomeration or possible fragmentation of the PET beads. The present invention finally confirmed the ball milling mixing process parameters of 120 to 140 minutes at 350 to 400 rpm through comparative experiments.

[0020] In addition, another inventive point of the present invention is that, based on the ball milling method to coat the carbon-based conductive filler on the surface of the PET beads and the supercritical CO2 foaming technology, a PET-based supercritical carbon dioxide foaming material with an isolated structure conductive network and antistatic properties is prepared. In the actual experimental process, it was accidentally discovered that its foaming expansion rate significantly affects the conductivity. Through comparative experiments, it was finally found that the conductivity of the prepared PET-based supercritical carbon dioxide foaming material can reach up to 0.004S / m.

[0021] Based on the above invention, in one of the preferred technical schemes, the blended material in step (2) is placed in a supercritical CO2 foaming container, that is, 4 to 6 g of the blended material is placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and the foaming expansion rate is controlled by the size of the container, thereby further improving the conductivity of the prepared PET-based supercritical carbon dioxide foaming material.

[0022] It should be noted that in step (2), CO2 is introduced and then the pressure is maintained at 8-11 MPa and 40-50°C for 3-6 hours, wherein the pressure conditions change dynamically during the entire pressure-maintaining process but are always maintained within the range of 8-11 MPa.

[0023] It should be noted that the heating rate of step (2) to 243-247° C. is the default heating rate of a conventional supercritical CO 2 foaming device, for example, 3-7° C. / min.

[0024] It should be noted that the step (2) of maintaining the foaming pressure at no more than 25 MPa during the heating process is usually controlled by a pressure relief valve. The foaming pressure gradually increases during the heating process, but the pressure relief valve is required to maintain the foaming pressure at no more than 25 MPa. In one preferred technical solution, the step (2) of maintaining the foaming pressure at no more than 20 MPa during the heating process.

[0025] In order to further improve the conductivity of the prepared PET-based supercritical carbon dioxide foamed material, during the experiment, the inventor accidentally discovered that the synergistic effect of carbon nanotubes and nanographene can be achieved through the following more preferred technical solution, which mainly includes the following steps:

[0026] (I) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend A for later use;

[0027] Wherein, the addition amount of the carbon nanotubes is 0.8-1wt% of the mass of the blend A.

[0028] The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min;

[0029] (II) mixing the PET beads and nano-graphene by ball milling, so that the nano-graphene is coated on the surface of the PET beads, and the mixture is used as blend B for standby use;

[0030] Wherein, the addition amount of the nanographene is 0.8-1wt% of the mass of the blend B,

[0031] The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min;

[0032] (III) After blending blend A and blend B in a mass ratio of 1:(0.8-1.2) and mixing evenly, 4-6 g of the blend is weighed and placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and CO2 is introduced. Then, the pressure is maintained for 3-6 hours at a pressure of 8-11 MPa and a temperature of 40-50°C. After the time is up, the temperature is raised to 243-247°C, and the foaming pressure is maintained at no more than 25 MPa during the heating process. After reaching the set temperature, the pressure is quickly released and the mixture is cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material.

[0033] The PET-based supercritical carbon dioxide foaming material prepared by the above preferred method, under the same feed ratio and foaming expansion rate conditions, surprisingly found that its conductivity can be close to 0.007S / m, which exceeds the PET-based supercritical carbon dioxide foaming material prepared when nanographene / carbon nanotubes are used alone as fillers.

[0034] It should be noted that the inventors have also tried to use a variety of carbon-based conductive fillers when selecting carbon-based conductive fillers, first blending them evenly and then coating them on the surface of PET beads by ball milling. However, actual experiments found that in actual operation, the dispersion effect of various carbon-based conductive fillers was poor when coated on the surface of PET beads, and a conductive network structure could not be formed.

[0035] In this article, the mixing and drying are carried out in accordance with the conventional principles of chemical processes, and those skilled in the art can perform specific operations according to common knowledge.

[0036] The PET-based supercritical carbon dioxide foamed material prepared by the present invention can be applied to packaging materials, insulating materials, cushioning materials and other fields, for example, in construction engineering, vehicle manufacturing, and sports goods.

[0037] The present invention has the following beneficial effects:

[0038] 1. The present invention provides a method for preparing a PET-based supercritical carbon dioxide foamed material. Based on the ball milling method, a carbon-based conductive filler is coated on the surface of PET beads and supercritical CO2 foaming technology is used to prepare a PET-based supercritical carbon dioxide foamed material with an isolated structure conductive network and antistatic properties. When a single carbon-based conductive filler is selected, the electrical conductivity can reach up to 0.004S / m.

[0039] 2. The present invention provides a method for preparing a PET-based supercritical carbon dioxide foaming material. By selecting a ball milling method with appropriate process parameters, the carbon-based conductive filler is coated on the surface of the PET beads. First, the dispersion of the carbon-based conductive filler on the surface of the beads can be effectively improved, the agglomeration phenomenon can be reduced, and it is more conducive to the construction and integrity of the conductive network, thereby improving the antistatic performance. Secondly, by coating the carbon-based conductive filler on the surface of the PET beads through the ball milling method, the amount of carbon-based conductive filler added can be significantly reduced while ensuring high antistatic performance. In particular, compared with the process of melt-blending the carbon-based conductive filler with the matrix to realize the conductive network, the amount of carbon-based conductive filler added can be reduced by an order of magnitude, so as to achieve the purpose of significantly reducing costs and increasing efficiency.

[0040] 3. The present invention provides a method for preparing a PET-based supercritical carbon dioxide foaming material. It is accidentally discovered that under the same feed ratio and foaming expansion rate conditions, when PET beads coated with carbon nanotubes and PET beads coated with nano-graphene are foamed under blending conditions, it is surprisingly found that the electrical conductivity can be close to 0.007S / m, which exceeds the PET-based supercritical carbon dioxide foaming material prepared when nano-graphene / carbon nanotubes are used alone as fillers, proving that the synergistic effect of carbon nanotubes and nano-graphene can be achieved through the above-mentioned preferred process. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of the process for preparing the PET-based supercritical carbon dioxide foaming material in Examples 7 to 9 of the present invention.

[0042] Figure 2 It is a comparative line graph of expansion rate / conductivity of the PET-based supercritical carbon dioxide foamed materials prepared in Examples 1 to 9 of the present invention. DETAILED DESCRIPTION

[0043] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously change or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention. Although it is believed that those of ordinary skill in the art fully understand the following terms, the following definitions are still stated to help illustrate the subject matter disclosed by the present invention.

[0044] The present invention provides a method for preparing a PET-based supercritical carbon dioxide foaming material, which mainly comprises the following steps:

[0045] (1) PET beads and carbon-based conductive fillers are mixed by ball milling, so that the carbon-based conductive fillers are coated on the surface of the PET beads, and the mixture is used as a blend;

[0046] The amount of the carbon-based conductive filler added is 0.8-1 wt% of the blend.

[0047] The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min;

[0048] (2) placing the blend obtained in step (1) in a supercritical CO2 foaming container, introducing CO2, and then maintaining the pressure for 3 to 6 hours at a pressure of 8 to 11 MPa and a temperature of 40 to 50° C. After the time is up, the temperature is raised to 243 to 247° C., and the foaming pressure is maintained at no more than 25 MPa during the heating process. After reaching the set temperature, the pressure is quickly released and the container is cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material.

[0049] In this article, the PET beads in step (1) are conventional polyethylene terephthalate (PET) bead raw materials, and generally chemical raw material grade PET bead raw materials can be directly selected and used. In one embodiment, for example, PET bead raw materials of models CB602, FR530, CR8863, and CZ328 are selected.

[0050] In this article, the carbon-based conductive filler in step (1) is a conventional carbon-based conductive filler that can construct a conductive network structure outside or inside a polymer matrix. In one embodiment, the carbon-based conductive filler in step (1) includes any one of carbon nanotubes, nanographene, nanocarbon black, and carbon nanofibers.

[0051] In one embodiment, in order to further expand the functionality of the prepared PET-based supercritical carbon dioxide foamed material, the step (1) further comprises immersing the PET beads and the carbon-based conductive filler in a flame retardant and then taking it out so that the flame retardant adheres to the surface of the PET beads after ball milling so that the carbon-based conductive filler is coated on the surface of the PET beads; the flame retardant is selected from the flame retardant conventionally added to the polymer-based foamed material, and those skilled in the art can select a suitable flame retardant according to the addible flame retardants recorded in the prior art literature or the existing process methods.

[0052] Furthermore, in order to better illustrate the present invention and provide a preferred embodiment for reference, the above-mentioned flame retardant selection includes any one of DOPO-KH560 flame retardant, diphenyl sulfone thiophenylphosphonate (PSTPP), liquid flame retardant DTFR-6007, etc.; the DOPO-KH560 flame retardant is the flame retardant disclosed in the previous article by the applicant of the present invention (Lu Jin, Jia Lu, Liu Xingang, et al. Preparation and Properties of DOPO-KH560 Modified Polyethylene Oxide Polymer Solid Electrolyte [J]. Polymer Materials Science and Engineering, 2021. DOI: 10.16865 / j.cnki.1000-7555.2021.0054.).

[0053] It should be noted that, due to the fact that the blend obtained in step (1) is prone to moisture regain during raw material transportation and storage, it is advisable to dry it before foaming to minimize its moisture content, which helps to improve the stability of the subsequent preparation process. In one embodiment, for example, the blend is dried at a temperature of 120 to 140° C. for at least 4 hours.

[0054] In one embodiment, the amount of the carbon-based conductive filler added in step (1) is 0.8-1wt% of the mass of the blend, for example, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1wt% or any range or point value therebetween.

[0055] In one embodiment, the process parameters of the ball milling mixing treatment in step (1) are: processing at 350-400 rpm for 120-140 min, for example, 350 rpm, 360 rpm, 370 rpm, 380 rpm, 390 rpm, 400 rpm or any range or point value therebetween, and processing time for 120 min, 125 min, 130 min, 135 min, 140 min or any range or point value therebetween.

[0056] One of the inventive points of the present invention is that by selecting a ball milling method with appropriate process parameters, the carbon-based conductive filler is coated on the surface of the PET beads. First, it can effectively improve the dispersibility of the carbon-based conductive filler on the surface of the beads, reduce the agglomeration phenomenon, and is more conducive to the construction and integrity of the conductive network, thereby improving the antistatic performance. Secondly, by using the ball milling method to coat the carbon-based conductive filler on the surface of the PET beads, the amount of carbon-based conductive filler added can be significantly reduced while ensuring high antistatic performance. In particular, compared with the process of melt blending the carbon-based conductive filler with the polymer matrix to realize the conductive network, the amount of carbon-based conductive filler added can be reduced by an order of magnitude to achieve the purpose of significantly reducing costs and increasing efficiency. However, it should be noted that too high or too low ball milling parameters will significantly hinder the dispersion of carbon-based conductive fillers on the surface of the beads, resulting in filler agglomeration or possible fragmentation of the PET beads. The present invention finally confirmed the ball milling mixing process parameters of 120 to 140 minutes at 350 to 400 rpm through comparative experiments.

[0057] In addition, another inventive point of the present invention is that, based on the ball milling method to coat the carbon-based conductive filler on the surface of the PET beads and the supercritical CO2 foaming technology, a PET-based supercritical carbon dioxide foaming material with an isolated structure conductive network and antistatic properties is prepared. In the actual experimental process, it was accidentally discovered that its foaming expansion rate significantly affects the conductivity. Through comparative experiments, it was finally found that the conductivity of the prepared PET-based supercritical carbon dioxide foaming material can reach up to 0.004S / m.

[0058] Based on the above invention, in one preferred embodiment, the blended material in step (2) is placed in a supercritical CO2 foaming container, that is, 4 to 6 g of the blended material is placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and the foaming expansion rate is controlled by the size of the container, thereby further improving the conductivity of the prepared PET-based supercritical carbon dioxide foaming material.

[0059] In one embodiment, the pressure condition in step (2) is 8-11 MPa, for example, 8 MPa, 8.5 MPa, 9 MPa, 9.5 MPa, 10 MPa, 10.5 MPa, 11 MPa or any range or point value therebetween; the temperature condition is 40-50°C, for example, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C or any range or point value therebetween; the pressure is maintained for 3-6 h, for example, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h or any range or point value therebetween; after the time is reached, the temperature is raised to 243-247°C, for example, 243°C, 244°C, 245°C, 246°C, 247°C or any range or point value therebetween.

[0060] It should be noted that in step (2), CO2 is introduced and then the pressure is maintained at 8-11 MPa and 40-50°C for 3-6 hours, wherein the pressure conditions change dynamically during the entire pressure-maintaining process but are always maintained within the range of 8-11 MPa.

[0061] It should be noted that the heating rate of step (2) to 243-247° C. is the default heating rate of a conventional supercritical CO 2 foaming device, for example, 3-7° C. / min.

[0062] It should be noted that the step (2) of maintaining the foaming pressure at no more than 25 MPa during the heating process is usually controlled by a pressure relief valve. The foaming pressure gradually increases during the heating process, but the pressure relief valve is required to maintain the foaming pressure at no more than 25 MPa. In one preferred technical solution, the step (2) of maintaining the foaming pressure at no more than 20 MPa during the heating process.

[0063] In order to further improve the conductivity of the prepared PET-based supercritical carbon dioxide foamed material, during the experiment, the inventor accidentally discovered that the synergistic effect of carbon nanotubes and nanographene can be achieved through the following more preferred implementation method, which mainly includes the following steps:

[0064] (I) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend A for later use;

[0065] Wherein, the addition amount of the carbon nanotubes is 0.8-1wt% of the mass of the blend A.

[0066] The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min;

[0067] (II) mixing the PET beads and nano-graphene by ball milling, so that the nano-graphene is coated on the surface of the PET beads, and the mixture is used as blend B for standby use;

[0068] Wherein, the addition amount of the nanographene is 0.8-1wt% of the mass of the blend B,

[0069] The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min;

[0070] (III) After blending blend A and blend B in a mass ratio of 1:(0.8-1.2) and mixing evenly, 4-6 g of the blend is weighed and placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and CO2 is introduced. Then, the pressure is maintained for 3-6 hours at a pressure of 8-11 MPa and a temperature of 40-50°C. After the time is up, the temperature is raised to 243-247°C, and the foaming pressure is maintained at no more than 25 MPa during the heating process. After reaching the set temperature, the pressure is quickly released and the mixture is cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material.

[0071] The PET-based supercritical carbon dioxide foaming material prepared by the above preferred method, under the same feed ratio and foaming expansion rate conditions, surprisingly found that its conductivity can be close to 0.007S / m, which exceeds the PET-based supercritical carbon dioxide foaming material prepared when nanographene / carbon nanotubes are used alone as fillers.

[0072] It should be noted that the inventors have also tried to use a variety of carbon-based conductive fillers when selecting carbon-based conductive fillers, first blending them evenly and then coating them on the surface of PET beads by ball milling. However, actual experiments found that in actual operation, the dispersion effect of various carbon-based conductive fillers was poor when coated on the surface of PET beads, and a conductive network structure could not be formed.

[0073] In this article, the mixing and drying are carried out in accordance with the conventional principles of chemical processes, and those skilled in the art can perform specific operations according to common knowledge.

[0074] The PET-based supercritical carbon dioxide foamed material prepared by the present invention can be applied to packaging materials, insulating materials, cushioning materials and other fields, for example, in construction engineering, vehicle manufacturing, and sports goods.

[0075] The present invention will be further explained in detail with reference to the following examples. However, it should be understood by those skilled in the art that these examples are provided for illustrative purposes only and are not intended to limit the present invention.

[0076] Example

[0077] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. The specific conditions not specified in the examples are carried out according to the conditions recommended by normal conditions or manufacturers. The reagents used or the instruments not specified by the manufacturer are all conventional products that can be obtained commercially. The application should not be construed as being limited to the specific examples described.

[0078] 1. Raw materials

[0079] PET (polyethylene terephthalate) beads, CB602, Suzhou Qingshun Plastic Raw Materials Co., Ltd.; carbon nanotubes, NC7000, Nanocyl SA, Belgium

[0080] Graphene, Changzhou Sixth Element Materials Technology Co., Ltd.

[0081] Carbon dioxide (purity 99%), Chengdu Xuyuan Gas Co., Ltd.

[0082] Example 1

[0083] (1) PET beads and carbon nanotubes were mixed by ball milling (QM-3SP2 planetary ball mill, Nanjing Nanda Instrument Co., Ltd., grinding ball diameter 7.65 mm, the same below) so that the carbon-based conductive filler was coated on the surface of the PET beads, and the mixture was used as a blend;

[0084] Wherein, the addition amount of the carbon-based conductive filler is 1wt% of the blend mass,

[0085] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0086] (2) Weigh 4 g of the blend obtained in step (1) and place it in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and introduce CO2. Then, maintain the pressure for 4 h at a pressure of 10 MPa and a temperature of 45°C. After the time is up, raise the temperature to 245°C, and keep the foaming pressure no more than 20 MPa during the heating process. After reaching the set temperature, quickly release the pressure within 10 seconds, cool to room temperature, and prepare a PET-based supercritical carbon dioxide foaming material, which is tested as a sample and recorded as PET / CNTs.

[0087] Example 2

[0088] (1) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend;

[0089] Wherein, the addition amount of the carbon nanotubes is 1wt% of the blend mass,

[0090] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0091] (2) Weigh 5 g of the blend obtained in step (1) and place it in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and introduce CO2. Then, maintain the pressure for 4 h at a pressure of 10 MPa and a temperature of 45°C. After the time is up, raise the temperature to 245°C, and keep the foaming pressure no more than 20 MPa during the heating process. After reaching the set temperature, quickly release the pressure within 10 seconds, cool to room temperature, and prepare a PET-based supercritical carbon dioxide foaming material, which is tested as a sample and recorded as PET / CNTs.

[0092] Example 3

[0093] (1) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend;

[0094] Wherein, the addition amount of the carbon nanotubes is 1wt% of the blend mass,

[0095] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0096] (2) Weigh 6 g of the blend obtained in step (1) and place it in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and introduce CO2. Then, maintain the pressure for 4 h at a pressure of 10 MPa and a temperature of 45°C. After the time is up, raise the temperature to 245°C, and keep the foaming pressure no more than 20 MPa during the heating process. After reaching the set temperature, quickly release the pressure within 10 seconds, cool to room temperature, and prepare a PET-based supercritical carbon dioxide foaming material, which is tested as a sample and recorded as PET / CNTs.

[0097] Example 4

[0098] (1) mixing PET beads and graphene by ball milling, so that the graphene is coated on the surface of the PET beads, and the mixture is used as a blend;

[0099] Wherein, the addition amount of graphene is 1wt% of the blend mass,

[0100] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0101] (2) Weigh 4 g of the blend obtained in step (1) and place it in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and introduce CO2. Then, maintain the pressure for 4 hours at a pressure of 10 MPa and a temperature of 45°C. After the time is up, raise the temperature to 245°C, and keep the foaming pressure no more than 20 MPa during the heating process. After reaching the set temperature, quickly release the pressure within 10 seconds, cool to room temperature, and prepare a PET-based supercritical carbon dioxide foaming material, which is tested as a sample and recorded as PET / Gr.

[0102] Example 5

[0103] (1) mixing PET beads and graphene by ball milling, so that the graphene is coated on the surface of the PET beads, and the mixture is used as a blend;

[0104] Wherein, the addition amount of graphene is 1wt% of the blend mass,

[0105] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0106] (2) Weigh 5 g of the blend obtained in step (1) and place it in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and introduce CO2. Then, maintain the pressure for 4 hours at a pressure of 10 MPa and a temperature of 45°C. After the time is up, raise the temperature to 245°C, and keep the foaming pressure no more than 20 MPa during the heating process. After reaching the set temperature, quickly release the pressure within 10 seconds, cool to room temperature, and prepare a PET-based supercritical carbon dioxide foaming material, which is tested as a sample and recorded as PET / Gr.

[0107] Example 6

[0108] (1) mixing PET beads and graphene by ball milling, so that the graphene is coated on the surface of the PET beads, and the mixture is used as a blend;

[0109] Wherein, the addition amount of graphene is 1wt% of the blend mass,

[0110] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0111] (2) Weigh 6 g of the blend obtained in step (1) and place it in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and introduce CO2. Then, maintain the pressure for 4 hours at a pressure of 10 MPa and a temperature of 45°C. After the time is up, raise the temperature to 245°C, and keep the foaming pressure no more than 20 MPa during the heating process. After reaching the set temperature, quickly release the pressure within 10 seconds, cool to room temperature, and prepare a PET-based supercritical carbon dioxide foaming material, which is tested as a sample and recorded as PET / Gr.

[0112] Example 7

[0113] (I) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend A for later use;

[0114] Wherein, the addition amount of the carbon nanotubes is 1wt% of the mass of the blend A.

[0115] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0116] (II) mixing the PET beads and nano-graphene by ball milling, so that the nano-graphene is coated on the surface of the PET beads, and the mixture is used as blend B for standby use;

[0117] Wherein, the addition amount of the nanographene is 1wt% of the mass of the blend B,

[0118] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0119] (III) After blending blend A and blend B in a mass ratio of 1:1, 4 g of the mixture was weighed and placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and CO2 was introduced. The pressure was then maintained at a pressure of 10 MPa and a temperature of 45°C for 4 hours. After the time was up, the temperature was raised to 245°C, and the foaming pressure was maintained at no more than 20 MPa during the heating process. After reaching the set temperature, the pressure was quickly released and the mixture was cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material, which was tested as a sample and recorded as PET / CNTs / Gr.

[0120] Example 8

[0121] (I) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend A for later use;

[0122] Wherein, the addition amount of the carbon nanotubes is 1wt% of the mass of the blend A.

[0123] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0124] (II) mixing the PET beads and nano-graphene by ball milling, so that the nano-graphene is coated on the surface of the PET beads, and the mixture is used as blend B for standby use;

[0125] Wherein, the addition amount of the nanographene is 1wt% of the mass of the blend B,

[0126] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0127] (III) After blending blend A and blend B in a mass ratio of 1:1, 5 g of the mixture was weighed and placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and CO2 was introduced. The pressure was then maintained at 10 MPa and 45°C for 4 h. After the time was up, the temperature was raised to 245°C, and the foaming pressure was maintained at no more than 20 MPa during the heating process. After reaching the set temperature, the pressure was quickly released and the mixture was cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material, which was tested as a sample and recorded as PET / CNTs / Gr.

[0128] Example 9

[0129] (I) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend A for later use;

[0130] Wherein, the addition amount of the carbon nanotubes is 1wt% of the mass of the blend A.

[0131] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0132] (II) mixing the PET beads and nano-graphene by ball milling, so that the nano-graphene is coated on the surface of the PET beads, and the mixture is used as blend B for standby use;

[0133] Wherein, the addition amount of the nanographene is 1wt% of the mass of the blend B,

[0134] The process parameters of the ball milling mixing treatment are: processing at 350 rpm for 120 min;

[0135] (III) After blending blend A and blend B in a mass ratio of 1:1, 6 g of the mixture was weighed and placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and CO2 was introduced. Then, the pressure was maintained at 10 MPa and 45°C for 4 hours. After the time was up, the temperature was raised to 245°C, and the foaming pressure was kept below 20 MPa during the heating process. After reaching the set temperature, the pressure was quickly released and the mixture was cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material, which was tested as a sample and recorded as PET / CNTs / Gr.

[0136] 3. Test Methods

[0137] The conductivity of the samples was measured using a four-point probe conductivity meter FT-371A.

[0138] 4. Test Results

[0139] like Figure 2 As shown in Table 1 below, under the same feed ratio and foaming expansion rate conditions, it was surprisingly found that the conductivity of the PET / CNTs / Gr prepared in Example 9 was close to 0.007S / m, which exceeded the PET-based supercritical carbon dioxide foaming material prepared when nanographene / carbon nanotubes were used alone as fillers.

[0140] It was also found that by adding different masses of blends into a fixed foaming container, the expansion rate of the prepared PET-based supercritical carbon dioxide foaming material can be effectively controlled and further affect its conductivity.

[0141] Table 1 Comparison of expansion rate and conductivity of PET-based supercritical carbon dioxide foamed materials prepared in Examples 1 to 9

[0142]

[0143] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a PET-based supercritical carbon dioxide foamed material, characterized in that The main steps include: (1) PET beads and carbon-based conductive fillers are mixed by ball milling, so that the carbon-based conductive fillers are coated on the surface of the PET beads, and the mixture is used as a blend; The amount of the carbon-based conductive filler added is 0.8-1 wt% of the blend. The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min; (2) placing the blend obtained in step (1) in a supercritical CO2 foaming container, introducing CO2, and then maintaining the pressure for 3 to 6 hours at a pressure of 8 to 11 MPa and a temperature of 40 to 50° C. After the time is up, the temperature is raised to 243 to 247° C., and the foaming pressure is maintained at no more than 25 MPa during the heating process. After reaching the set temperature, the pressure is quickly released and the container is cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material.

2. The preparation method according to claim 1, characterized in that: The carbon-based conductive filler in step (1) includes any one of carbon nanotubes, nanographene, nanocarbon black, and carbon nanofibers.

3. The preparation method according to claim 1, characterized in that: In step (1), the PET beads and the carbon-based conductive filler are mixed by ball milling so that the carbon-based conductive filler is coated on the surface of the PET beads, and the step further includes immersing the PET beads in a flame retardant and then taking them out so that the flame retardant adheres to the surface of the PET beads.

4. The preparation method according to claim 3, characterized in that: The flame retardant includes any one of DOPO-KH560 flame retardant, diphenyl sulfone thiophenylphosphonate, and liquid flame retardant DTFR-6007.

5. The preparation method according to claim 1, characterized in that: The blend obtained in step (1) is dried at a temperature of 120-140° C. for at least 4 hours.

6. The preparation method according to claim 1, characterized in that: The blended material in step (2) is placed in a supercritical CO2 foaming container, which is to place 4 to 6 g of the blended material in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm.

7. The preparation method according to claim 1, characterized in that: In step (2), the foaming pressure is maintained at no more than 20 MPa during the heating process.

8. The preparation method according to claim 1, characterized in that The main steps include: (I) mixing PET beads and carbon nanotubes by ball milling, so that the carbon nanotubes are coated on the surface of the PET beads, and the mixture is used as a blend A for later use; Wherein, the addition amount of the carbon nanotubes is 0.8-1wt% of the mass of the blend A. The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min; (II) mixing the PET beads and nano-graphene by ball milling, so that the nano-graphene is coated on the surface of the PET beads, and the mixture is used as blend B for standby use; Wherein, the addition amount of the nanographene is 0.8-1wt% of the mass of the blend B, The process parameters of the ball milling mixing treatment are: processing at 350-400 rpm for 120-140 min; (III) After blending blend A and blend B in a mass ratio of 1:(0.8-1.2) and mixing evenly, 4-6 g of the blend is weighed and placed in a cylindrical supercritical CO2 foaming container with an inner cavity diameter of 30 mm and a height of 20 mm, and CO2 is introduced. Then, the pressure is maintained for 3-6 hours at a pressure of 8-11 MPa and a temperature of 40-50°C. After the time is up, the temperature is raised to 243-247°C, and the foaming pressure is maintained at no more than 25 MPa during the heating process. After reaching the set temperature, the pressure is quickly released and the mixture is cooled to room temperature to prepare a PET-based supercritical carbon dioxide foaming material.

9. The PET-based supercritical carbon dioxide foamed material prepared by the method for preparing a PET-based supercritical carbon dioxide foamed material according to any one of claims 1 to 8.

10. Use of the PET-based supercritical carbon dioxide foaming material as claimed in claim 9 as packaging material, insulating material and cushioning material.

Citation Information

Patent Citations

  • All-directional conductive foam and producing method thereof

    CN101431885B

  • Preparation method of polymer-based conductive microporous foam composite material

    CN102718983A

  • Novel method for preparing bimodal structure through supercritical carbon dioxide

    CN104558670A

  • Preparation method of microwave sintered PBAT ScCO2 foaming material

    CN116874876A

  • Thermoplastic polyurethane elastomer foam material composition, foam material and preparation and application thereof

    CN117986846A