Method for realizing steel slag decrement cyclic utilization based on self-heat-release fluxing agent

Through the combination of self-exothermic flux and reducing agent, the problems of low efficiency and high energy consumption of steel slag dephosphorization technology are solved, and efficient steel slag smelting and recycling are achieved, which improves the recovery rate and added value of phosphorus and iron resources.

CN118957178APending Publication Date: 2024-11-15CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411071097.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing steel slag dephosphorization technology is low in efficiency and high energy consumption, which leads to a bottleneck in the internal circulation of steel slag smelting, and fails to effectively utilize the phosphorus and iron resources in the steel slag, limiting its recyclability in the smelting process.

Method used

The combination of self-exothermic flux and reducing agent is used to reduce the steel slag by stirring, maintain the molten state, reduce the energy consumption of external heat sources, improve the interface reaction speed, achieve efficient dephosphorization and iron recovery, and optimize the recycling of phosphorus and iron resources.

Benefits of technology

It significantly improves the dephosphorization efficiency and iron recovery rate of steel slag, reduces slag production, reduces process costs, realizes efficient direct smelting of steel slag, and increases the added value of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957178A_ABST
    Figure CN118957178A_ABST
Patent Text Reader

Abstract

The invention relates to a method for dephosphorizing and recycling molten steel slag, in particular to a method for realizing steel slag decrement recycling based on a self-heat-release fluxing agent. For the smelted molten steel slag, the crusting of the steel slag is inhibited through the self-heat-release fluxing agent and stirring, and the on-line rapid reduction dephosphorization of the molten steel slag is realized by matching with the reducing agent. By means of the process, the CaO-SiO2-Al2O3-MgO series hot slag with high alkalinity, low total iron and low phosphorus can be produced, the rotary furnace steelmaking link can be directly circulated, consumption of mineral slag formers such as lime can be reduced, the energy-saving and carbon-reducing effects in the smelting process are remarkably improved, and meanwhile steel slag is reduced. In the reductive dephosphorization process, carbon-saturated iron prepared in advance is introduced as a capturing agent, phosphorus and iron generated through reduction can be efficiently captured, and a small amount of ferrophosphorus alloy is formed. The process is reasonable in design, simple and accurate to control and convenient for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for dephosphorizing and recycling molten steel slag, and in particular to a method for reducing and recycling steel slag based on a self-exothermic flux. Background Art

[0002] In recent years, with the rapid development of my country's steel industry, crude steel output has continued to rise and has jumped to the first place in the world. As a result, the discharge of bulk solid wastes such as steel slag has also increased sharply. It is in urgent need of safe, effective and proper treatment and utilization. At present, my country's steel slag is mainly used in cement building materials and other fields, but the overall utilization rate is low and the added value is low. Domestic policies will restrict the use of steel slag as a cement admixture. Therefore, it is urgent to establish a smelting and disposal mode for steel slag and source reduction. However, because steel slag contains phosphorus elements that are harmful to steel products, its recyclability in the smelting process is greatly limited. Steel slag contains a large amount of ferrophosphorus resources. It is estimated that my country's annual steel slag contains more than 4.8 million tons of phosphorus, which is equivalent to 1 / 3 of the country's annual phosphorus production. With the huge demand for phosphorus in the new energy storage market, steel slag phosphorus resources are gradually being included in the research field. Every year, the amount of iron oxides that are not effectively recovered in steel slag is approximately 16-32 million tons, which can meet the annual iron ore demand of large steel companies with an annual output of tens of millions of tons. Developing technologies for efficient extraction and utilization of phosphorus and iron resources in steel slag and breaking through the constraints of the internal circulation of steel slag smelting not only provides excellent industry opportunities, but also conforms to the country's strategic development deployment.

[0003] In recent years, Japan, South Korea, Germany and other countries have attached great importance to the dephosphorization and recycling of steel slag, and have successively developed technologies such as high-temperature gasification reduction dephosphorization, molten reduction dephosphorization, slag static dephosphorization, and low-temperature magnetic separation dephosphorization. Some of these technologies have been piloted and industrialized, attracting widespread attention from the international community. However, my country has not yet made any breakthrough progress in the field of steel slag recycling. At present, the domestic steel slag direct utilization technology uses mechanical separation to separate the slag and iron in the steel slag from the recovery process of iron elements in the steel slag, and mainly uses the difference in magnetism and density between the two to recover metallic iron, but it is easy to produce wastewater and dust and pollute the environment. In addition, the weak magnetic iron oxides contained in the steel slag are difficult to remove by magnetic separation, resulting in a waste of resources such as iron oxides. In addition, the high-temperature resources of steel slag are not utilized, which is a treatment process with low added value.

[0004] Phosphorus in steel slag is mainly in the form of 2CaO·SiO 2 -3CaO·P 2 O 5It exists in the form of solid solution. The most effective way to recycle iron oxides in steel slag is to reduce it to metallic iron. Some scholars have used reducing agents such as carbon silicon and coal powder to reduce steel slag at high temperatures. However, there are problems such as difficulty in separating slag and iron and greenhouse gas emissions. At present, most of the processes adopted for steel slag belong to "late-stage modification technology", which often requires additional physical (magnetic field, gravity field, mechanical energy, etc.), chemical (reducing agent) or thermodynamic (heat) excitation, so it is inevitable to consume more energy during the modification process. In fact, molten steel slag itself has very high heat and good fluidity, but this part of energy is difficult to be effectively utilized in the process of steel slag treatment. In order to increase the internal circulation ratio of steel slag smelting and achieve the reduction of steel slag at the source, it is necessary to break through key technical difficulties such as low dephosphorization efficiency of steel slag and insufficient value-added conversion of phosphorus iron resources. In this regard, our research group has made some achievements in the early stage, such as the patent "A technology for full utilization of steel slag based on low-carbon dephosphorization of molten slag" (application number: 2023108100596); but it requires an electric furnace for reduction. The patent "Online direct reduction method for iron extraction from electric furnace steel slag" (application number: 202310771568.2) realizes the reduction treatment of high-temperature electric furnace slag in the slag pot to realize Fe-Mn alloy by adding aluminum ash balls, but the iron in the slag still needs to be recovered by magnetic separation, and does not pay attention to the recovery of phosphorus and the recycling of tailings, nor does it involve the problem of recycling and enrichment of phosphorus-containing molten iron. The patent "A method for comprehensive recycling of valuable components in steel slag" (application number: 201811366079.4) recovers Fe-Mn alloy in molten steel slag by adding silicon ash modification and aluminum ash, but it requires an electric furnace for reduction, and does not pay attention to the recovery of phosphorus and the recycling and enrichment of phosphorus-containing molten iron. The patent "A method for online adjustment of slag basicity of a smelting reduction furnace using red mud" (application number: 202110118234.6) adds granulated red mud, converter molten steel slag, and coke into a smelting reduction furnace, heats the slag with graphite electrodes, and smelts the steel slag to obtain molten iron and reconstructed active material (alkalinity of 0.70-1.50). A heating system is also required, and the reconstructed active material has a low alkalinity and is used to replace cement in large proportions. Summary of the invention

[0005] The present invention is to develop and utilize domestic steel slag resources and solve the problem that the existing steel slag has high phosphorus content and cannot be used industrially. Regardless of whether it is based on a rotary kiln or an electric furnace, the reduction dephosphorization technology will face the problem of temperature drop caused by reduction endothermicity, which is easy to cause the crusting and agglomeration of high-melting-point steel slag, which not only greatly reduces the dephosphorization efficiency of the steel slag, but also affects the slag speed after the cycle. Therefore, the present invention attempts for the first time to use a combination of a self-exothermic flux and a reducing agent to maintain the molten state of the steel slag during the reduction process without the need for an external heat source, expand the reduction operable temperature zone, and increase the interface reaction speed, which can effectively reduce the energy consumption of the external heat source, reduce the process cost, reduce the slag production, and break through the core problem of the bottleneck of the hot cycle of steel slag.

[0006] The combination of the self-exothermic co-solvent and the reducing agent designed and developed by the invention can improve the efficiency of slag reduction, maintain the metallurgical properties of the slag, and realize the direct smelting cycle of hot slag, which has high research value and important application prospects.

[0007] The design idea of ​​the present invention is:

[0008] The invention pours high-temperature molten steel slag into a slag pot filled with molten iron and / or molten steel, adds mixed self-exothermic flux and reducing agent in a certain proportion, and stirs to achieve the purpose of melting and reducing the steel slag.

[0009] Since phosphorus in steel slag is mainly in the form of 2CaO·SiO 2 -3CaO·P 2 O 5 It exists in the form of solid solution, with a phosphorus content of about 2% to 5%. Its direct circulation will have an adverse effect on the converter. Therefore, reducing it to elemental phosphorus or non-solid phosphorus is a prerequisite for dephosphorization. The main reaction processes involved are:

[0010] Ca 3 (PO 4 ) 2 (s) + 5 C (s) = 3 CaO (s) + P 2 (g) + 5 CO (g)

[0011] Under high temperature conditions, the reduced elemental phosphorus will be absorbed by the carbon-saturated iron and the reduced iron, and the following reaction will occur:

[0012] P 2 =2[P]

[0013] Thereby converting into a stable ferrophosphorus phase.

[0014] Since the phosphorus reduction process is an endothermic reaction, in order to solve the problems of insufficient heat, slag crusting and agglomeration, and low dephosphorization rate in the reduction process, the present invention has developed a self-exothermic flux and a stirring technology that matches it. The flux raw materials of the present invention include electrolytic aluminum ash, ferrosilicon, silicon powder, CaC 2 Etc. The ratio of flux and slag is determined by the viscosity of slag. If the viscosity is too high, the slag will crust, the reduction kinetics will deteriorate, and it is not conducive to the reduction of slag; if the viscosity is too low, it means that the flux consumption is too large, resulting in a decrease in the basicity of the reduced tailings and an increase in the amount of slag. By adjusting the ratio of flux and slag, the slag composition and the metallic iron composition are close to the fusible area, which is conducive to the aggregation and growth of iron particles in the slag.

[0015] In addition, reducing agents include carbon powder, graphite, coke, activated carbon, lignite, bituminous coal, anthracite and biomass charcoal, etc. The ratio of reducing agent to steel slag is determined according to the content of carbon in the reducing agent and oxygen in the iron oxide in the steel slag, and the amount of reducing agent added is also determined based on the content of oxygen contained in the iron oxide in the steel slag. The molar ratio of carbon in the reducing agent to oxygen contained in the iron oxide in the steel slag also needs to be accurately calculated. If the ratio of reducing agent to steel slag is too high, it will lead to a large loss of phosphorus gasification, and the consumption of reducing agent will also increase; if the ratio of reducing agent to steel slag is too low, it indicates that the oxide in the slag system is not fully reduced, resulting in a low recovery rate of iron elements and poor dephosphorization effect. By optimizing the ratio of reducing agent to steel slag, the efficiency and effect of the reduction process can be improved, and a higher iron recovery rate and dephosphorization rate can be achieved.

[0016] In the present invention, the high-temperature molten steel slag used for the first time can be prepared by the following process: the iron ore is sintered and pelletized, and then reduced in a blast furnace to obtain molten iron, and then smelted in a converter to obtain qualified molten steel and by-product molten steel slag that meet the requirements.

[0017] The invention discloses a method for dephosphorizing and recycling molten steel slag, which comprises the following steps: pouring high-temperature molten steel slag into a slag pot filled with a certain amount of molten iron and / or molten steel, adding a self-exothermic flux and a reducing agent mixed in a certain proportion, and stirring to achieve the purpose of melting and reducing the steel slag; stirring and reducing in the slag pot, then stopping stirring, standing for stratification, pouring the reduced tail slag at the top into another slag pot, and transporting it to a converter for use as a slag-making agent; the self-exothermic flux is selected from electrolytic aluminum ash, ferrosilicon, silicon powder, CaC 2 , at least one of metal aluminum and SiC;

[0018] The molten iron and / or molten steel pre-placed in the slag pot is used as a capture agent to form phosphorus-containing molten iron; the phosphorus-containing molten iron is used as a new capture agent until its phosphorus content is greater than or equal to 9wt%.

[0019] No additional heat needs to be introduced to melt and reduce the slag.

[0020] Preferably, a method for dephosphorizing and recycling molten steel slag of the present invention comprises the following steps:

[0021] Step 1

[0022] Weigh the respective exothermic flux components in proportion, mix them evenly, and prepare a self-exothermic flux. The self-exothermic flux includes the following components by mass percentage: Al 30-50%, Al 2 O 3 10-25%, Si 10-20%, Fe 5-15%, Ca 10-15%, C 5-10%.

[0023] Step 2

[0024] The high-temperature molten steel slag is poured into a slag pot containing a certain amount of molten iron and / or molten steel, and a self-exothermic flux and a reducing agent mixed in a certain proportion are added and stirred to achieve the purpose of melting and reducing the steel slag; wherein the amount of the self-exothermic flux added is 3-10% of the total weight of the steel slag; the molar ratio of carbon in the reducing agent to oxygen contained in the iron oxide in the steel slag is: C / O=1.2-1.6;

[0025] Step 3

[0026] The stirring reduction time in the slag pot is 20-50 minutes, preferably 30-40 minutes; then the stirring is stopped, and after standing for stratification, the reduced tailings on the top are poured into another slag pot and transported to the converter for use as a slag-making agent;

[0027] Step 4

[0028] The reduced tailings are recycled until they contain the following components by mass percentage:

[0029] TFe 2-5.0%, CaO 20-40%, SiO 2 20-35%, Al 2 O 3 5-10%, MgO 5-8%, P 2 O 5 0.1-0.5%, at this time the reduced tailings can be used as stone raw materials,

[0030] Phosphorus-containing molten iron is used as a new capture agent until it includes the following components by mass percentage:

[0031] C 1-3.0%, Si 0.5-2%, P 3.0-15.0%, Mn 0.2-0.8%, and the balance is Fe. At this time, it can be used as an alloy raw material, or return to the smelting process after diluting phosphorus with scrap steel.

[0032] Preferably, the reducing agent in step 2 is selected from at least one of carbon powder, graphite, coke, activated carbon, lignite, bituminous coal, anthracite and biochar.

[0033] Preferably, in step three, the molten iron and / or molten steel pre-placed in the slag pot is used as a capture agent for the reduced phosphorus and iron to form phosphorus-containing molten iron.

[0034] Preferably, in step three, the capture agent pre-placed in the slag pot for the first time comprises, by mass percentage, the following components: C 3.2-5.0%, Si 1-2.5%, P 0-0.1%, Mn 0.2-1%, and the remainder Fe.

[0035] Preferably, the first reduction tailings obtained comprises the following components by mass percentage: TFe 0.3-3.0%, CaO 40-60%, SiO 2 10-30%, Al 2 O 3 3-5%, MgO 5-10%, P 2 O 5 Less than 0.2%.

[0036] Preferably, the phosphorus-containing molten iron obtained after one or two reductions comprises, by mass percentage, C 0.5-3.0%, Si 0.05-0.5%, P 1.0-7.0% (preferably 3-7%), Mn 0.5-2%, and the balance Fe.

[0037] The invention discloses a method for dephosphorizing and recycling molten steel slag. In each stage of recycling, the recovery rate of iron is greater than or equal to 90%, and the recovery rate of phosphorus is greater than or equal to 70%.

[0038] The invention discloses a method for dephosphorizing and recycling molten steel slag. After recycling, the recycling volume of steel slag is increased by more than 45%, the consumption of lime is reduced by more than 50%, and the average amount of slag produced per ton of qualified molten steel is reduced to 35-80 kg.

[0039] The present invention discloses a method for dephosphorizing and recycling molten steel slag. The molten steel slag can be recycled for more than 2 times and can be recycled for 3 times or more after optimization.

[0040] The present invention mainly includes that iron ore powder is sintered and pelletized, and then enters a blast furnace for reduction to generate molten iron. The molten iron enters a converter for dephosphorization and decarburization treatment to generate qualified molten steel and molten steel slag. The molten steel slag is poured into a slag pot filled with a certain amount of molten iron and / or molten steel, and a mixed self-exothermic flux and reducing agent are added. The stirring and reduction time in the slag pot is 20-50 minutes, preferably 30-40 minutes, and then the stirring is stopped. After standing for stratification, the reduced tailings at the top are poured into another slag pot, and transported to the subsequent converter for use as a slag-making agent. The molten iron and / or molten steel in the high slag pot at the bottom are used as a scavenger to form phosphorus-containing molten iron; the phosphorus-containing molten iron is used as a new scavenger until its phosphorus content is greater than or equal to 9wt%, and then poured out for the preparation of ferrophosphorus alloy.

[0041] Compared with the prior art, the present invention has the following advantages:

[0042] The present invention designs a self-exothermic flux for online thermal reduction of steel slag and a preparation method thereof, aiming to break through the energy efficiency bottleneck of steel slag reduction dephosphorization. During the slag reduction process, large pieces of condensation are very likely to occur due to heat absorption and cooling, which not only hinders the mass transfer of phosphorus in the slag and reduces the reduction dephosphorization efficiency, but also increases the slag burden of the post-cycle smelting process. Therefore, accelerating the reduction process and maintaining the slag state are the core issues for achieving efficient slag reduction. Traditional slag reduction research focuses more on gasification dephosphorization, but due to the low gasification reaction rate, it is difficult to achieve a breakthrough in dephosphorization efficiency.

[0043] In order to solve this problem, the present invention utilizes the synergistic effect of multiple self-exothermic co-solvents, and cooperates with multiple types of highly active reducing agents to disperse the reduction interface, capture phosphorus with iron, accelerate the reaction process, thereby breaking through the energy efficiency bottleneck of reduction dephosphorization and expanding the application prospects of the technology.

[0044] 1. The present invention makes full use of molten steel slag, greatly promotes its recyclability in the smelting process, and reduces the output of steel slag from the source.

[0045] 2. By using a self-exothermic co-solvent, a large amount of heat is released, the reaction rate is accelerated, the mass transfer conditions are optimized, and the efficiency of reduction dephosphorization is significantly improved.

[0046] 3. Avoid slag condensation caused by heat absorption and cooling, ensure the smooth progress of the reduction process, and reduce the slag burden.

[0047] 4. Through the synergistic effect of self-exothermic co-solvents, combined with multiple types of highly active reducing agents, the reduction interface is dispersed, phosphorus is captured with iron, the reaction process is accelerated, and the difficult problem of steel slag dephosphorization is overcome. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a schematic diagram of the new process for comprehensive utilization of high-phosphorus iron ore of the present invention. DETAILED DESCRIPTION

[0049] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0050] See also Figure 1 The present invention mainly includes that the iron ore powder is sintered and pelletized, and then enters the blast furnace for reduction to generate molten iron. The molten iron enters the converter for dephosphorization and decarburization treatment to generate qualified molten steel and molten steel slag. The qualified molten steel is further processed into the final steel product, and the molten steel slag is poured into a slag pot filled with carbon-saturated iron, and a self-exothermic flux and a reducing agent are added for stirring and reduction. The reduced high-phosphorus molten iron is formed at the bottom and becomes a phosphorus-iron alloy by capturing phosphorus multiple times; the reduced tailings are discharged from the top and recycled multiple times until the smelting performance decreases and it is treated as a stone raw material. The effects of the embodiment and the comparative example are shown in Table 1.

[0051] Table 1 Effects of Examples and Comparative Examples

[0052]

[0053]

[0054] In order to better illustrate the present invention, the following examples are selected to further illustrate the present invention.

[0055] Embodiment 1:

[0056] First, the prepared steel slag was placed in a muffle furnace in the laboratory and heated to 1500°C to obtain molten steel slag. The composition of the steel slag is shown in Table 2. The respective exothermic fluxes (including electrolytic aluminum ash, ferrosilicon, silicon powder, CaC 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 3 14.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C 7.1%. Secondly, pour 100g of high-temperature molten steel slag into a magnesium oxide crucible containing 5g of carbon-saturated iron, add 5g of self-exothermic flux, the amount of which is 5% of the total weight of the steel slag, add the prepared carbon powder (C / O=1.2), stir to melt and reduce the steel slag, melt and reduce for 30 minutes, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 3.5%, and the phosphorus recovery rate is 79.1%; the recovery rate of metallic iron is 91.2%, the basicity of the reduced tailings is 2.5, and the P content in the tailings is 1.3%. 2 O 5 The content is 0.16%.

[0057] Table 2 Composition and mass% of steel slag used in the experiment

[0058]

[0059] Example 2: First, the tailings in Example 1 are used as slag-making agents and poured into the molten iron in the induction furnace to reduce the steel slag obtained after smelting. Then, the respective exothermic fluxes (including electrolytic aluminum ash, ferrosilicon, silicon powder, CaC 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 314.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C7.1%. Secondly, pour 100g of high-temperature molten slag after one cycle into the magnesium oxide crucible containing the iron block in Example 1, add 5g of self-exothermic flux, the amount of which is 5% of the total weight of the slag, add the prepared carbon powder (C / O=1.2), stir to melt and reduce the slag, melt and reduce for 30 minutes, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 5.8%, and the phosphorus recovery rate is 74.3%; the recovery rate of metallic iron is 90.2%. The composition of the tailings after one cycle is shown in Table 3. The basicity of the reduced tailings is 2.2, and the P content in the tailings is 1.3%. 2 O 5 The content is 0.18%.

[0060] Table 3 Composition and mass% of tailings after one cycle

[0061]

[0062] Example 3: First, the tailings in Example 2 are used as slag-making agents and poured into the molten iron in the induction furnace to reduce the steel slag obtained after smelting. 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 3 14.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C7.1%. Secondly, pour 100g of high-temperature molten slag after one cycle into the magnesium oxide crucible containing the iron block in Example 2, add 5g of self-exothermic flux, the amount of which is 5% of the total weight of the slag, add the prepared carbon powder (C / O=1.2), stir to melt and reduce the slag, melt and reduce for 30 minutes, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 7.6%, and the phosphorus recovery rate is 72.2%; the recovery rate of metallic iron is 90.5%. The composition of the tailings after two cycles is shown in Table 4. The basicity of the reduced tailings is 2.0, and the P content in the tailings is 1.3%. 2 O 5 The content is 0.21%.

[0063] Table 4 Composition and mass% of steel slag after two cycles

[0064]

[0065] Example 4: First, the tailings in Example 3 are used as slag-making agents and poured into the molten iron in the induction furnace to reduce the steel slag obtained after the smelting. 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 3 14.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C7.1%. Secondly, pour 100g of high-temperature molten slag after one cycle into the magnesium oxide crucible containing the iron block in Example 3, add 5g of self-exothermic flux, the amount of which is 5% of the total weight of the slag, add the prepared carbon powder (C / O=1.2), stir to melt and reduce the slag, melt and reduce for 30 minutes, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 9.3%, and the phosphorus recovery rate is 70.2%; the recovery rate of metallic iron is 90.6%. The composition of the tailings after three cycles is shown in Table 5. The basicity of the reduced tailings is 1.6, and the P content in the tailings is 1.6. 2 O 5 The content is 0.25%. At this time, the circulation of high-phosphorus iron blocks that have reached the phosphorus capture limit and the reduced tailings with reduced smelting performance is stopped. The high-phosphorus iron blocks can be used as phosphorus iron alloys, and the reduced tailings can be used as raw materials for preparing stone.

[0066] Table 5 Composition and mass% of steel slag after three cycles

[0067]

[0068] Embodiment 5:

[0069] First, the prepared steel slag was placed in a muffle furnace in the laboratory and heated to 1600°C to obtain molten steel slag. The composition of the steel slag is shown in Table 6. The respective exothermic fluxes (including electrolytic aluminum ash, ferrosilicon, silicon powder, CaC 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 314.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C 7.1%. Secondly, pour 100g of high-temperature molten steel slag into a magnesium oxide crucible containing 5g of carbon-saturated iron, add 10g of self-exothermic flux, the amount of which is 10% of the total weight of the steel slag, add the prepared carbon powder (C / O=1.4), stir to melt and reduce the steel slag, melt and reduce for 40 minutes, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 3.8%, and the phosphorus recovery rate is 81.1%; the recovery rate of metallic iron is 90.6%, the basicity of the reduced tailings is 2.3, and the P in the tailings is 1.3. 2 O 5 The content is 0.14%.

[0070] Table 6 Composition and mass% of steel slag used in the experiment

[0071]

[0072] Example 6: First, the tailings in Example 5 are used as slag-making agents and poured into the molten iron in the induction furnace to reduce the steel slag obtained after smelting. 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 3 14.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C7.1%. Secondly, pour 100g of high-temperature molten slag after one cycle into the magnesium oxide crucible containing the iron block in Example 5, add 10g of self-exothermic flux, the amount of which is 10% of the total weight of the slag, add the prepared carbon powder (C / O=1.4), stir to melt and reduce the slag, melt and reduce for 40min, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 6.0%, and the phosphorus recovery rate is 76.3%; the recovery rate of metallic iron is 90.2%. The composition of the tailings after one cycle is shown in Table 7. The basicity of the reduced tailings is 2.1, and the P content in the tailings is 2.1. 2 O 5 The content is 0.17%.

[0073] Table 7 Composition and mass% of tailings after one cycle

[0074]

[0075] Example 7: First, the tailings in Example 6 are used as slag-making agents and poured into the molten iron in the induction furnace to reduce the steel slag obtained after the smelting. Then, the respective exothermic fluxes (including electrolytic aluminum ash, ferrosilicon, silicon powder, CaC 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 3 14.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C7.1%. Secondly, pour 100g of high-temperature molten slag after one cycle into the magnesium oxide crucible containing the iron block in Example 6, add 10g of self-exothermic flux, the amount of which is 10% of the total weight of the slag, add the prepared carbon powder (C / O=1.4), stir to melt and reduce the slag, melt and reduce for 40min, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 8.1%, and the phosphorus recovery rate is 72.9%; the recovery rate of metallic iron is 90.3%. The composition of the tailings after two cycles is shown in Table 8. The basicity of the reduced tailings is 1.9, and the P content in the tailings is 1.3. 2 O 5 The content is 0.19%.

[0076] Table 8 Composition and mass% of steel slag after two cycles

[0077]

[0078] Example 8: First, the tailings in Example 7 are used as slag-making agents and poured into the molten iron in the induction furnace to reduce the steel slag obtained after the smelting. 2 , metal aluminum, SiC, etc.) components are mixed evenly to prepare a self-exothermic flux, which includes the following components by mass percentage: Al 45.2%, Al 2 O 314.8%, Si 14.4%, Fe 10.6%, Ca 7.9%, C7.1%. Secondly, pour 100g of high-temperature molten slag after one cycle into the magnesium oxide crucible containing the iron block in Example 7, add 10g of self-exothermic flux, the amount of which is 10% of the total weight of the slag, add the prepared carbon powder (C / O=1.4), stir to melt and reduce the slag, melt and reduce for 40 minutes, stop stirring, and after cooling to room temperature, take out the crucible and separate the iron block and tailings. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 9.8%, and the phosphorus recovery rate is 70.8%; the recovery rate of metallic iron is 90.1%. The composition of the tailings after three cycles is shown in Table 9. The basicity of the reduced tailings is 1.5, and the P content in the tailings is 1.5. 2 O 5 The content is 0.22%. At this time, the high-phosphorus iron blocks that have reached the phosphorus capture limit and the reduced tailings with reduced smelting performance stop circulating. The high-phosphorus iron blocks can be used as phosphorus iron alloys, and the reduced tailings can be used as raw materials for preparing stone.

[0079] Table 9 Composition and mass% of steel slag after three cycles

[0080]

[0081] Comparative Example 1: This comparative example is basically the same as Example 1, except that no flux is added. Finally, chemical composition analysis shows that the phosphorus content in the iron block is 1.3%, the phosphorus recovery rate is 29.2%, the recovery rate of metallic iron is 65.2%, the basicity of the reduced tailings is 2.6, and the phosphorus content in the tailings is 1.3%. 2 O 5 The content is 2.13%. The phosphorus content of the tailings used once is too high, and the phosphorus iron recovery rate is low, which is not conducive to industrial application.

[0082] Comparative Example 2: This comparative example is basically the same as Example 1, except that a flux accounting for 15% is added. Finally, chemical composition analysis shows that the phosphorus content in the iron block is 3.5%, the phosphorus recovery rate is 60.5%, the recovery rate of metallic iron is 85.2%, the basicity of the reduced tailings is 1.5, and the phosphorus content in the tailings is 1.5. 2 O 5 The content is 2.33%, the tailings basicity is too low, the ferrophosphorus recovery rate is low and it does not have a recycling function. At the same time, the ferrophosphorus recovery rate is too low.

[0083] Comparative Example 3: This comparative example is basically the same as Example 1, except that the C / O is 1. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 0.3%, the phosphorus recovery rate is 18.5%, the recovery rate of metallic iron is 79.6%, the basicity of the reduced tailings is 2.2, and the P in the tailings is 1.5%. 2 O 5The content is 1.95%. The phosphorus content of the tailings used once is too high, and the phosphorus iron recovery rate is low, which is not conducive to industrial application.

[0084] Comparative Example 4: This comparative example is basically the same as Example 1, except that the C / O ratio is 2. Finally, chemical composition analysis shows that the phosphorus content in the iron block is 3.1%, the phosphorus recovery rate is 55.2%, the recovery rate of metallic iron is 88.5%, the basicity of the reduced tailings is 2.1, and the P content in the tailings is 1.3%. 2 O 5 The content is 0.22%. The large carbon consumption causes serious phosphorus gasification and low recovery rate.

[0085] Comparative Example 5: This comparative example is basically the same as Example 1, except that the reduction time is 10 min. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 0.1%, the phosphorus recovery rate is 13.6%, the recovery rate of metallic iron is 41.2%, the basicity of the reduced tailings is 2, and the phosphorus content in the tailings is 1.3%. 2 O 5 The content is 2.58%, the tailings contain high phosphorus content and do not have a recycling function, and the phosphorus recovery rate is too low.

[0086] Comparative Example 6: This comparative example is basically the same as Example 1, except that the reduction time is 60 min. Finally, chemical composition analysis shows that the phosphorus content in the iron block is 3.0%, and the phosphorus recovery rate is 63.6%; the recovery rate of metallic iron is 89.9, the basicity of the reduced tailings is 2.2, and the phosphorus content in the tailings is 1.3%. 2 O 5 The content is 0.11%. The reduction time is too long, resulting in serious phosphorus gasification, low recovery rate, and time-consuming. It does not meet the requirements of rapid reduction and does not have a circulation function. At the same time, the phosphorus recovery rate is too low.

[0087] Comparative Example 7: This comparative example is basically the same as Example 1, except that the flux composition is Al 15%, Al 2 O 3 30%, Si 25%, Fe 20%, Ca 7%, C 3%, which are not within the range of self-exothermic flux. Finally, the chemical composition analysis shows that the phosphorus content in the iron block is 1.2%, the phosphorus recovery rate is 35.6%, the recovery rate of metallic iron is 78.2%, the basicity of the reduced tailings is 1.6, and the P in the tailings is 1.2%. 2 O 5 The content is 1.56%. The phosphorus content of the tailings used once is too high, and the phosphorus iron recovery rate is low, which is not conducive to industrial application.

Claims

1. A method for dephosphorizing and recycling molten steel slag, Features: The high-temperature molten steel slag is poured into a slag pot filled with a certain amount of molten iron and / or molten steel, and a mixed self-exothermic flux and reducing agent are added in a certain proportion, and stirred to achieve the purpose of melting and reducing the steel slag; stirring and reducing are carried out in the slag pot, and then stirring is stopped, and after standing for stratification, the reduced tailings on the top are poured into another slag pot, and transferred to the converter for use as a slag-making agent; the self-exothermic flux is selected from electrolytic aluminum ash, ferrosilicon, silicon powder, CaC 2 , at least one of metal aluminum and SiC; The molten iron and / or molten steel pre-placed in the slag pot is used as a capture agent to form phosphorus-containing molten iron; the phosphorus-containing molten iron is used as a new capture agent until its phosphorus content is greater than or equal to 9wt%.

2. A method for dephosphorizing and recycling molten steel slag according to claim 1, Features: No additional heat needs to be introduced to melt and reduce the slag.

3. A method for dephosphorizing and recycling molten steel slag according to claim 1, Features The steps include: Step 1 Weigh the respective exothermic flux components in proportion, mix them evenly, and prepare a self-exothermic flux. The self-exothermic flux includes the following components by mass percentage: Al 30-50%, Al 2 O 3 10-25%, Si 10-20%, Fe 5-15%, Ca 10-15%, C 5-10%. Step 2 The high-temperature molten steel slag is poured into a slag pot containing a certain amount of molten iron and / or molten steel, and a self-exothermic flux and a reducing agent mixed in a certain proportion are added and stirred to achieve the purpose of melting and reducing the steel slag; wherein the amount of the self-exothermic flux added is 3-10% of the total weight of the steel slag; the molar ratio of carbon in the reducing agent to oxygen contained in the iron oxide in the steel slag is: C / O=1.2-1.6; Step 3 The stirring reduction time in the slag pot is 20-50 minutes, preferably 30-40 minutes; then the stirring is stopped, and after standing for stratification, the reduced tailings on the top are poured into another slag pot and transported to the converter for use as a slag-making agent; Step 4 The reduced tailings are recycled until they contain the following components by mass percentage: TFe 2-5.0%, CaO 20-40%, SiO 2 20-35%, Al 2 O 3 5-10%, MgO 5-8%, P 2 O 5 0.1-0.5%, at this time the reduced tailings can be used as stone raw materials. Phosphorus-containing molten iron is used as a new capture agent until it includes the following components by mass percentage: C 1-3.0%, Si 0.5-2%, P 3.0-10.0%, Mn 0.2-0.8%, and the balance is Fe. At this time, it can be used as an alloy raw material, or return to the smelting process after diluting phosphorus with scrap steel.

4. A method for dephosphorizing and recycling molten steel slag according to claim 3, Features: The reducing agent described in step 2 is selected from at least one of carbon powder, graphite, coke, activated carbon, lignite, bituminous coal, anthracite, and biochar.

5. A method for dephosphorizing and recycling molten steel slag according to claim 3, Features: In step three, the reduced phosphorus and iron are captured by using molten iron and / or molten steel previously placed in a slag pot to form phosphorus-containing molten iron.

6. A method for dephosphorizing and recycling molten steel slag according to claim 3, Features: In step 3, the capture agent pre-placed in the slag pot for the first time has the following components in mass percentage: C 3.2-5.0%, Si 1-2.5%, P 0-0.1%, Mn 0.2-1%, and the balance Fe.

7. A method for dephosphorizing and recycling molten steel slag according to claim 3, Features: The first reduction tailings obtained include the following components by mass percentage: TFe 0.3-3.0%, CaO 40-60%, SiO 2 10-30%, Al 2 O 3 3-5%, MgO 5-10%, P 2 O 5 Less than 0.2%.

8. A method for dephosphorizing and recycling molten steel slag according to claim 3, Features: The phosphorus-containing molten iron obtained after one or two reductions includes, by mass percentage, 0.5-3.0% C, 0.05-0.5% Si, 1.0-7.0% P, 0.5-2% Mn, and the balance Fe.

9. A method for dephosphorizing and recycling molten steel slag according to claim 3, Features: The recovery rate of iron is greater than or equal to 90%, and the recovery rate of phosphorus is greater than or equal to 70%.

10. A method for dephosphorizing and recycling molten steel slag according to claim 3, Features: After recycling, the steel slag recycling volume can reach more than 45%, the lime consumption can be reduced by 50%, and an average of 40-80 kg of slag is produced per ton of qualified molten steel.

Citation Information

Cited By

  • Rare earth electroslag steel containing alloyed rare earth elements and manufacturing method of rare earth electroslag steel

    CN121428279A