Steel for straight seam welding hollow anchor rod body for railway tunnel and preparation method of straight seam welding hollow anchor rod body

By optimizing the composition and preparation process of steel for hollow anchor rod body, the mechanical properties of the hollow anchor rod body are improved, the problem of insufficient performance in the existing technology is solved, the technical requirements of railway tunnels are met, and the application is expanded scope.

CN118957442APending Publication Date: 2024-11-15PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411069226.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the performance indicators of the straight seam welded hollow anchor rod body do not meet the technical requirements of railway tunnels, especially the mechanical performance is insufficient, which cannot meet the application requirements of the hollow anchor rod body in railway tunnels.

Method used

By optimizing the composition of the steel for hollow anchor rod body, including the content of C, Si, Mn, Cr, Ti, Nb, Al, P, S and N, combined with smelting, converter, LF refining, continuous casting, heating, rough rolling, Process steps such as hot rolling, finishing rolling, laminar cooling, welding and high-frequency heating are used to regulate the structure and performance of the structure and performance and improve the mechanical properties of the materials.

Benefits of technology

The yield, tensile force and maximum force total elongation of the straight-sea welded hollow anchor rod body has reached the technical requirements of "Railway Tunnel Anchor Bolt" (TB/T 3356-2021), and is suitable for railway tunnel support, and Expand and apply to highways, tunnels, bridges and mining fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980338830000024
    Figure BDA0004980338830000024
  • Figure BDA0004980338830000043
    Figure BDA0004980338830000043
  • Figure BDA0004980338830000111
    Figure BDA0004980338830000111
Patent Text Reader

Abstract

The invention provides steel for a rod body of a straight seam welding hollow anchor rod for a phi 25 * 3.5 mm railway tunnel. The steel comprises the following components: 0.20-0.24% of C; 0.20% to 0.40% of Si; 1.20% to 1.40% of Mn; the content of Ti is 0.030 to 0.050 percent; the content of Nb is 0.010 to 0.020 percent; 0.20% to 0.30% of Cr; the content of Als is 0.010 to 0.050 percent; and the balance of Fe. The invention further provides a preparation method of the straight seam welding hollow anchor rod body for the phi 25 * 3.5 mm railway tunnel. The low-cost design thought of increasing the content of C and reducing the content of Mn is adopted, meanwhile, in order to improve the hardenability of the material, a small amount of Cr element is added, and a small amount of Nb is added, so that the strength, plasticity and toughness are improved; and further, through precise structure property regulation and control, qualified products meeting the standard are obtained, and the method has the characteristics of high production efficiency, small quality, and low energy consumption and cost of whole-process production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hollow anchor steel, in particular to a The invention relates to steel for a straight seam welded hollow anchor rod body for railway tunnels and a preparation method of the straight seam welded hollow anchor rod body. Background Art

[0002] Anchor bolts are a primary support structure for roads, slopes, dams, tunnels, bridges, and mine tunnels, providing both support and reinforcement. With the advancement of technology, their application is becoming increasingly widespread, and demand is increasing. Anchor bolts operate by overcoming the disadvantage of rock and soil having a much lower tensile strength than its compressive strength through the longitudinal tension of the bolt body. This superficially limits the ability of rock and soil to break away from its original mass, while macroscopically increasing its cohesiveness, forming the ultimate rod-based system for rock and soil reinforcement.

[0003] Chinese invention patent publication number CN 115976409 A discloses a low-cost hollow anchor welded pipe, hot-rolled steel strip, and preparation method. The pipe is composed of the following components by weight: 0.18% ≤ C ≤ 0.25%, 0.10% ≤ Si ≤ 0.20%, 1.00% ≤ Mn ≤ 1.50%, P ≤ 0.020%, S ≤ 0.008%, 0.10% ≤ Cr ≤ 0.30%, with the remainder being Fe and unavoidable impurities. The C, Si, and Mn contents in this invention do not meet the requirements of TB / T 3356-2021. Therefore, the product covered by this invention does not meet the technical requirements for producing hollow anchor rods for railway tunnels, and the wall thickness of the anchor rods is not specified.

[0004] Chinese invention patent publication number CN 115976409 A discloses a low-cost hollow anchor welded pipe, hot-rolled steel strip, and preparation method. The pipe is composed of the following components by weight: 0.18% ≤ C ≤ 0.25%, 0.10% ≤ Si ≤ 0.20%, 1.00% ≤ Mn ≤ 1.50%, P ≤ 0.020%, S ≤ 0.008%, 0.10% ≤ Cr ≤ 0.30%, with the remainder being Fe and unavoidable impurities. The C, Si, and Mn contents in this invention do not meet the requirements of TB / T 3356-2021. Therefore, the product covered by this invention does not meet the technical requirements for producing hollow anchor rods for railway tunnels, and the wall thickness of the anchor rods is not specified.

[0005] In order to meet the technical requirements of the hollow anchor rod body in railway tunnels, a The straight seam welded hollow anchor rod body for railway tunnels is of great significance. Summary of the Invention

[0006] The technical problem solved by the present invention is to provide a The steel used for the rod body of the straight seam welded hollow anchor for railway tunnels enables the rod body of the straight seam welded hollow anchor to have better mechanical properties and meet the technical requirements of the hollow anchor rod body.

[0007] In view of this, the present application provides a Steel for the rod body of straight seam welded hollow anchor bolts for railway tunnels, calculated in percentage by mass, comprising:

[0008]

[0009] P≤0.015%;

[0010] S≤0.005%;

[0011] N≤0.0040%;

[0012] Fe balance.

[0013] Preferably, the C content is 0.22-0.24%, and the Si content is 0.25-0.37%.

[0014] Preferably, the Mn content is 1.23% to 1.38%, and the Ti content is 0.035% to 0.049%.

[0015] Preferably, the Cr content is 0.21-0.28%, and the Nb content is 0.012-0.018%.

[0016] The present application also provides a method for preparing the straight seam welded hollow anchor rod body, comprising the following steps:

[0017] The steel for the hollow anchor rod body for straight seam welding is prepared according to the mass ratio to obtain a mixture, and the mixture is sequentially subjected to smelting, converter, LF refining, continuous casting, heating, rough rolling, hot coil box coiling, finish rolling, laminar cooling and coiling to obtain a hot rolled coil;

[0018] The hot-rolled coil is sequentially striped, roll-formed and welded to obtain a straight seam welded pipe;

[0019] The straight seam steel pipe is subjected to high-frequency heating, three-roll rolling, online heat treatment and slow cooling in sequence to obtain a straight seam welded hollow anchor rod body.

[0020] Preferably, the S of the molten iron obtained by the smelting is ≤0.003% when it enters the converter, and the argon blowing time of the small platform process is ≥8 minutes; argon is blown throughout the LF refining process, and 70TiFe alloy is used for micro-titanium treatment before leaving the station; the heating temperature after continuous casting is 1200-1300°C, the time is 150-250 minutes, and the soaking time is ≥30 minutes.

[0021] Preferably, the rough rolling is performed in 5 or 7 passes; the finishing rolling is performed in 7 passes, the starting rolling temperature of the finishing rolling is 1000-1100°C, the reduction ratios of the last three stands are ≥17%, ≥15% and ≥12% respectively, and the final rolling temperature is 850-900°C.

[0022] Preferably, the laminar cooling adopts a front-stage cooling mode, the cooling rate is 50-70°C / s, and the coiling temperature is 595-625°C.

[0023] Preferably, the welding power is 100-110 kW, the frequency is 290-300 kHz, and the metal streamline angle of the welded joint is 55-65°; the temperature of the high-frequency heating is 890-900°C, and the quenching end temperature of the online heat treatment is 290-300°C.

[0024] This application also provides a A straight seam welded hollow anchor rod body for a railway tunnel is prepared from the steel used for the straight seam welded hollow anchor rod body.

[0025] This application provides a Steel for straight-seam welded hollow anchor rods for railway tunnels, comprising: C 0.20-0.24%; Si 0.20-0.40%; Mn 1.20-1.40%; Ti 0.030-0.050%; Nb 0.010-0.020%; Cr 0.20-0.30%; Als 0.010-0.050%; P ≤ 0.015%; S ≤ 0.005%; N ≤ 0.0040%; Fe balance. The steel for straight-seam welded hollow anchor rods provided in this application utilizes a low-cost design approach that increases the C content and reduces the Mn content. A small amount of Cr is added to improve the material's hardenability. The addition of a small amount of Nb also helps improve strength and ductility. Ultimately, the steel for straight-seam welded hollow anchor rods provided in this application can provide the straight-seam welded hollow anchor rods with excellent mechanical properties, meeting technical requirements.

[0026] Furthermore, the present application also provides a method for preparing a straight-seam welded hollow anchor rod body, which achieves precise organization and performance control by regulating some parameters in the preparation steps, obtains qualified products that meet performance standards, and has the characteristics of high production efficiency, low mass, and low energy consumption and cost in the entire production process.

[0027] Experimental results show that the straight-seam welded hollow anchor rod for railway tunnels prepared using the components and preparation method of the present invention has a yield force ≥160KN, a tensile strength ≥205KN, and a maximum force total elongation ≥7.5%, which meets the technical requirements for hollow anchor rods in "Railway Tunnel Anchor Rods" (TB / T 3356-2021). It is suitable for the production of steel anchor rods for railway tunnel support, and can be expanded to be used in roads, tunnels, bridges and mines, with broad market application prospects. DETAILED DESCRIPTION

[0028] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0029] In view of the problem that the performance index of the straight seam welded hollow anchor rod body in the prior art does not meet the technical requirements, the present application provides a The steel for the rod body of a straight seam welded hollow anchor for railway tunnels improves the performance of the rod body of a straight seam welded hollow anchor by selecting the composition and further combining the preparation method with precise control of the structure, thereby meeting the technical requirements. Specifically, the embodiment of the present invention discloses a Steel for the rod body of straight seam welded hollow anchor bolts for railway tunnels, calculated in percentage by mass, comprising:

[0030]

[0031] S≤0.005%;

[0032] N≤0.0040%;

[0033] Fe balance.

[0034] Specifically, regarding the steel for the straight seam welded hollow anchor rod described in this application, the carbon element (C) therein: Carbon is an effective strengthening element in steel. It can dissolve into the matrix to play a role in solid solution strengthening, and can combine with titanium to form carbide precipitates, which play a role in fine grain strengthening and precipitation strengthening. Increasing the carbon content is beneficial to improving strength; however, too high a carbon content will form a large number of coarse and brittle carbide particles in the steel, which is detrimental to plasticity and toughness. At the same time, it will form a segregation band in the center of the steel plate, which is detrimental to bending and forming properties. Therefore, the value range of C in the present invention is set to 0.20% to 0.24%, specifically, the C content is 0.22% to 0.24wt%. For example, the C content in this application is 0.20%, 0.21%, 0.22%, 0.23%, and 0.24%.

[0035] Silicon can dissolve in ferrite and austenite to increase the hardness and strength of steel, which is beneficial to refine the rust layer structure and reduce the overall corrosion rate of steel. However, too high a content will reduce the plasticity and toughness of the steel, making it difficult to remove scale during rolling. Therefore, the value range of Si in the present invention is set to 0.20% to 0.40%, specifically, the Si content is 0.25% to 0.37%; for example, the Si content of this application is 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.12%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33%, 0.34%, 0.35%, 0.36%, 0.37%, 0.38%, 0.39%, and 0.40%.

[0036] Manganese has a strong solid solution strengthening effect, can significantly reduce the phase transition temperature of steel, refine the microstructure of steel, and is an important strengthening and toughening element. However, when the Mn content is too high, the continuous casting process is prone to cracking of the ingot and may also cause component segregation in the core of the steel plate. Therefore, the value range of Mn in the present invention is set to 1.20% to 1.40%. Specifically, the Mn content is 1.23% to 1.38%. For example, the Mn content in this application is 1.20%, 1.21%, 1.22%, 1.23%, 1.24%, 1.25%, 1.26%, 1.27%, 1.28%, 1.29%, 1.30%, 1.31%, 1.32%, 1.33%, 1.34%, 1.35%, 1.36%, 1.37%, 1.38%, 1.39%, and 1.40%.

[0037] Excessive phosphorus content significantly reduces the steel's plasticity and low-temperature toughness. Therefore, the phosphorus content in this invention is set within a range of ≤0.015%, specifically 0.0014%, 0.008%, and 0.010%. Sulfur: Sulfur can adversely affect the microstructure and properties of steel plates. Excessive sulfur content can increase the steel's hot brittleness tendency and form sulfide inclusions, degrading the steel's properties. Therefore, the sulfur content in this invention is set within a range of S ≤0.005%, specifically 0.001%, 0.003%, and 0.004%.

[0038] Chromium can improve the hardenability of steel, achieve a martensitic structure under relatively stable conditions, and simultaneously achieve higher plasticity. Therefore, the Cr content in the present invention is set within a range of 0.20% to 0.30%. Specifically, the Cr content is 0.21% to 0.28%. For example, the Cr content in this application is 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, and 0.30%.

[0039] Titanium and nitrogen: Ti(C, N) precipitates formed by titanium, carbon and nitrogen can effectively refine austenite grains and produce precipitation strengthening effects. Increasing the titanium and nitrogen content can increase the volume fraction of Ti(C, N) precipitates and enhance the grain refinement and precipitation strengthening effects. However, excessive titanium and nitrogen content can easily form micron-sized TiN, resulting in decreased formability. Excessive nitrogen content can increase the aging tendency, cold brittleness and hot brittleness of steel, thereby damaging the cold bending performance of steel. Therefore, the value range of Ti in the present invention is set to 0.030% to 0.050%, and the value range of N is set to ≤0.0040%; specifically, the content of Ti is 0.035% to 0.049%, and the content of N is 0.0020% to 0.0039%; for example, the content of Ti in this application is 0.030%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.0 44%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, and 0.050%. The nitrogen content in this application is 0.0021%, 0.0022%, 0.0023%, 0.0024%, 0.0025%, 0.0026%, 0.0027%, 0.0028%, 0.0029%, 0.0030%, 0.0031%, 0.0032%, 0.0033%, 0.0034%, 0.0035%, 0.0036%, 0.0037%, 0.0038%, and 0.0039%.

[0040] Niobium is a carbide-forming element. NbC can pin austenite grain boundaries, preventing grain growth. It can also form a second phase strengthening agent, which helps improve the strength, ductility, and toughness of steel. However, excessive niobium content increases production costs, so it is generally not recommended to add too much. Therefore, the Nb content in the present invention is set within a range of 0.010% to 0.020%, specifically 0.012% to 0.018%. For example, the Nb content in this application is 0.010%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, and 0.020%.

[0041] Aluminum: Aluminum is added to steel to deoxidize it and improve its quality. However, if the aluminum content is too high, its nitrogen oxides tend to precipitate at austenite grain boundaries, causing cracks in the cast slab. Therefore, the Als content in the present invention is 0.010-0.050%, more specifically 0.031-0.046%, and even more specifically 0.035-0.042%.

[0042] Furthermore, the present application also provides a method for preparing steel for a straight seam welded hollow anchor rod body, comprising the following steps:

[0043] The steel for the hollow anchor rod body for straight seam welding is prepared according to the mass ratio to obtain a mixture, and the mixture is sequentially subjected to smelting, converter, LF refining, continuous casting, heating, rough rolling, hot coil box coiling, finish rolling, laminar cooling and coiling to obtain a hot rolled coil;

[0044] The hot-rolled coil is sequentially striped, roll-formed and welded to obtain a straight seam welded pipe;

[0045] The straight seam steel pipe is subjected to high-frequency heating, three-roll rolling, online heat treatment and slow cooling in sequence to obtain steel for a straight seam welded hollow anchor rod body.

[0046] During the preparation process, slabs are first smelted and continuously cast according to their components. When the molten iron enters the converter, S is ≤ 0.003%. The converter needs to be "washed" before smelting. The argon blowing time of the small platform process must be ≥ 8 minutes to ensure low nitrogen, oxygen, and hydrogen content in the molten steel and remove residual non-metallic inclusions in the molten steel. The LF refining process must be argon blown throughout, and the molten steel must not be exposed. 70TiFe alloy is used for micro-titanium treatment before leaving the station. The continuous casting process is fully protected and low-alloy protective slag is used. "Open pouring" is not allowed to obtain continuously cast steel billets whose chemical composition meets the design requirements. The billet thickness is 200mm.

[0047] Furthermore, in the step of heating the steel billet obtained after continuous casting, the heating temperature is 1200-1300°C, specifically, the heating temperature is 1240-1260°C, more specifically, the heating temperature is 1242-1253°C, more specifically, the heating temperature is 1245-1252°C; the heating time is 150-250min, specifically, the heating time is 171min-244min, more specifically, the heating time is 208-230min, wherein the soaking time is ≥30min, specifically, the soaking time is 33-49min, more specifically, the soaking time is 35-42min. The purpose of post-continuous casting heating is to homogenize the as-cast structure and component segregation, while also dissolving alloying elements. However, the steel used in the hollow anchor rod body of the present invention has a high carbon content, so the heating process requires sufficient temperature and time. Furthermore, higher heating temperatures help promote the dissolution of alloying elements, but excessively high temperatures and prolonged heating times can lead to burnout, overheating, and overburning. Therefore, the present invention requires that the continuously cast steel billet be hot-transferred and hot-loaded during the heating step, with the heating performed in a regenerative heating furnace.

[0048] Furthermore, during the rough rolling and hot coiling steps described in the above technical solution, the rough rolling must achieve sufficient deformation to ensure austenite recrystallization, refine the austenite grains, and prevent the formation of mixed-grain structures. If the intermediate bar thickness is too large, the rough rolling deformation may be insufficient, and if the finished product thickness is thin, the finishing rolling load may be excessive. If the intermediate bar thickness is too small, the finishing rolling deformation may be insufficient. Therefore, the rough rolling in the present invention preferably involves six rough rolling passes, with the deformation in passes 1 to 3 being ≥18% and the deformation in passes 4 to 6 being ≥20%. The intermediate bar thickness is 42±1 mm, with all odd-numbered passes undergoing descaling, followed by hot coiling and insulation.

[0049] Furthermore, finishing rolling is carried out afterwards. In the finishing rolling step, the three stands are basically rolled in the austenite non-recrystallization zone after finishing rolling. A large deformation rate is adopted, which can flatten and elongate the austenite grains that have been rolled in the recrystallization zone and refined to a certain extent, increase the grain boundary area of ​​austenite per unit volume, and at the same time generate a large number of deformation bands and high-density dislocations in the grains, thereby increasing the ferrite nucleation rate and obtaining a fine structure after phase transformation; if the finishing rolling start temperature is too high, the deformation amount in the austenite non-recrystallization zone during the finishing rolling process is insufficient, which is not conducive to structure refinement; if the final rolling temperature is too low, the difference from the start rolling temperature is too large, which makes the cooling rate of the finishing rolling process too fast, and there is a risk that the two stands are rolled in the two-phase zone after finishing rolling, resulting in poor comprehensive product performance; if the final rolling temperature is too high, the deformation amount in the non-recrystallization zone is insufficient, which is not conducive to final structure refinement. Therefore, in the present invention, the finishing rolling step is set to undergo seven finishing rolling passes, with the reduction ratios of the last three stands being ≥17%, ≥15%, and ≥12%, respectively. The starting temperature of the finishing rolling is 1000-1100°C, and the final rolling temperature is 850-900°C. Specifically, the starting temperature of the finishing rolling is 1035-1075°C, and the final rolling temperature is 860-892°C. More specifically, the starting temperature of the finishing rolling is 1050-1070°C, and the final rolling temperature is 872-885°C. The finished product thickness is 3.5 mm.

[0050] Furthermore, after the finish rolling, laminar cooling and coiling are sequentially performed to obtain the hot-rolled coil. Specifically, in the laminar cooling step, the use of a front-stage cooling mode can achieve a greater degree of undercooling, thereby refining the final microstructure, and a higher cooling rate can have a certain effect on improving the core banded microstructure. Therefore, the present invention adopts a front-stage cooling mode with a cooling rate of 60±10°C / s, specifically, the cooling rate is 55-69°C / s, and more specifically, the cooling rate is 57-60°C / s. Specifically, in the coiling step, if the coiling temperature is too low, the cooling rate in the laminar cooling stage will be too high, resulting in the formation of low-temperature microstructures such as martensite, leading to reduced plasticity. If the coiling temperature is too high, the grains will coarsen and the pearlite interlamellar spacing will increase, resulting in reduced strength and toughness. Therefore, in the present invention, the coiling temperature is set to 595-625°C, specifically, the coiling temperature is 600-623°C, and more specifically, the coiling temperature is 610-620°C. The finished coil thickness is 3.5mm.

[0051] The present application then sequentially strips, rolls and welds the hot-rolled coils to obtain straight seam welded pipes; the welding is specifically high-frequency resistance welding. If the welding power and frequency are too large, the weld joint will suffer serious metal burnout and the risk of welding quality defects will increase; if the welding power and frequency are too small, the weld will be poorly welded; whether the metal streamline angle is too large or too small, it will be detrimental to the performance of the weld joint and will cause the welded pipe to flatten and crack and fail. Therefore, in the present invention, the welding power is 100-110kW, the frequency is 290-300kHz, and the metal streamline angle of the weld joint is controlled to be 55-65°. Specifically, the welding power is 105-109kW, the frequency is 291-298kHz, and the metal streamline angle of the weld joint is controlled to be 58-62°. After the above steps, a straight seam welded pipe is obtained, and the cross-sectional dimensions of the finished straight seam welded pipe are

[0052] Finally, the present application sequentially subjects the straight seam steel pipe to high-frequency heating, three-roll rolling, online heat treatment, and slow cooling to obtain a straight seam welded hollow anchor rod body. During the high-frequency heating step, if the heating temperature is too high, the austenite grain size will be coarse, thereby reducing the strength after quenching; if the heating temperature is too low, insufficient austenitization will result, thereby reducing the plasticity after quenching. Therefore, the high-frequency heating temperature of the straight seam welded pipe in the present invention is set to 890-900°C. Specifically, the high-frequency heating temperature is 892-899°C, and more specifically, the high-frequency heating temperature is 895-898°C.

[0053] Specifically, in the on-line heat treatment step of the anchor rod body obtained by three-roll spinning, the three-roll rolling is specifically three-roll spinning rolling, rolling into a spiral shape. Hollow anchor rod body; the online heat treatment is specifically an online quenching heat treatment. If the quenching temperature is too high, the martensite content will decrease, resulting in a decrease in strength; if the quenching temperature is too low, the bainite content will decrease and the martensite content will increase, resulting in deterioration in plasticity. Therefore, in the present invention, the quenching temperature is set at 290-300°C, specifically 292-298°C, and more specifically 295-297°C. The quenching is performed online using a circular constant temperature cooling water.

[0054] Furthermore, in the cooling bed slow cooling step, the residual heat of the anchor rod body is used to perform self-tempering treatment and gradually cool to room temperature.

[0055] Furthermore, in the above technical solution, the raw material hot-rolled coil used to make the hollow anchor rod body has a thickness of 3.5 mm and is prepared in the following steps: molten iron desulfurization, converter, LF refining, continuous casting, heating in a heating furnace, rough rolling, hot coil box coiling, finish rolling, laminar cooling, and coiling. The resulting hot-rolled coil has a yield strength ≥ 525 MPa, a tensile strength ≥ 620 MPa, an elongation after fracture ≥ 30%, an elongation at maximum force ≥ 14.5%, and an impact energy of ≥ 30 J for a 1 / 4 size V-type specimen in a 180° bend test at -40°C and D = 0a. The microstructure of the hot-rolled coil is quasi-polygonal ferrite + pearlite, with the volume fractions of ferrite (F) being 85% to 90% and pearlite (P) being 10% to 15%.

[0056] Furthermore, in the above technical solution, the raw material hot-rolled coil is obtained after stripping, rounding and high-frequency resistance welding. The standard straight seam welded pipe has a yield strength of ≥670MPa, a tensile strength of ≥710MPa, an elongation after fracture of ≥14.5%, and an elongation at maximum force of ≥7.0%.

[0057] Furthermore, in the above technical solution, The straight seam welded pipes of different specifications are heated by high-frequency electric heating device, rolled into equal diameter by three-roller spinning, heat treated online, sawed, and cooled on cooling bed to obtain The standard straight seam welded hollow anchor rod body has a yield strength ≥160KN, a tensile strength ≥200KN, and a maximum force elongation ≥7.5%.

[0058] In order to further understand the present invention, the following embodiments are provided in conjunction with the present invention. The steel for the rod body of a straight seam welded hollow anchor for railway tunnels and its preparation method are described in detail, and the protection scope of the present invention is not limited by the following embodiments.

[0059] Example

[0060] This embodiment provides three sets of chemical compositions of the longitudinally welded hollow anchor rod body for railway tunnels and key process parameters in the preparation method thereof;

[0061] A sort of The chemical composition of the steel used for the longitudinal welded hollow anchor rod for railway tunnels is shown in Table 1, with the remainder being Fe and unavoidable impurities.

[0062] The steel for the hollow anchor rod body for straight seam welding is prepared according to the mass ratio of Table 1 to obtain a mixture, and the mixture is subjected to smelting, converter, LF refining, continuous casting, billet heating, rough rolling, hot coil box coiling, finish rolling, laminar cooling and coiling in sequence to obtain a hot-rolled coil;

[0063] The hot-rolled coil is sequentially subjected to striping, roll forming and high-frequency resistance welding to obtain a straight seam welded pipe;

[0064] The straight seam steel pipe is sequentially subjected to high-frequency heating, three-roll rolling, online quenching and slow cooling to obtain a straight seam welded hollow anchor rod body;

[0065] In the above steps, the control parameters involved in the steps of billet heating, rough rolling, finishing rolling, laminar cooling, and coiling, as well as the indicators such as the obtained mechanical properties, process properties, and microstructure types are shown in Tables 2 and 3;

[0066] In the above steps, the high-frequency resistance welding, high-frequency heating of the straight seam welded pipe, quenching temperature and mechanical properties obtained are shown in Table 4.

[0067] Table 1 Composition data of steel used for hollow anchor rod body for straight seam welding

[0068]

[0069]

[0070] Table 2: Related parameter data in the embodiment

[0071]

[0072] Table 3 Performance data of hot rolled coils prepared in Example

[0073]

[0074] Note: The test conditions for impact performance are -40℃ and the market size is 1 / 4 size V-type specimen. Note: The bending head diameter is D and the specimen thickness is a.

[0075] Table 4: Related parameters and performance data in the embodiment

[0076]

[0077]

[0078] It can be seen from Tables 3 and 4 that the performance of the hollow anchor rod body prepared in this application meets the technical requirements for hollow anchor rods in "Railway Tunnel Anchor Rods" (TB / T3356-2021).

[0079] The above embodiments are only intended to help understand the method and core concept of the present invention. It should be noted that those skilled in the art can make various improvements and modifications to the present invention without departing from the principles of the present invention, and such improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0080] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not limited to the embodiments shown herein but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A Steel for straight seam welded hollow anchor rod for railway tunnels, in percentage by mass, include: P≤0.015%; S≤0.005%; N≤0.0040%; Fe balance.

2. The steel for the straight seam welded hollow anchor rod body according to claim 1, It is characterized in that The C content is 0.22-0.24%, and the Si content is 0.25-0.37%.

3. The steel for the straight seam welded hollow anchor rod body according to claim 1, It is characterized in that The content of Mn is 1.23% to 1.38%, and the content of Ti is 0.035% to 0.049%.

4. The steel for the straight seam welded hollow anchor rod body according to claim 1, It is characterized in that The content of Cr is 0.21-0.28%, and the content of Nb is 0.012-0.018%.

5. The method for preparing the straight seam welded hollow anchor rod body according to claim 1, The following steps are involved: The mixture is prepared according to the mass ratio of the steel for the hollow anchor rod body for straight seam welding, and the mixture is smelted, subjected to a converter, LF refining, continuous casting, heated, roughly rolled, coiled in a hot coil box, finished rolled, laminar cooled and coiled in sequence to obtain a hot rolled coil; The hot-rolled coil is sequentially striped, roll-formed and welded to obtain a straight seam welded pipe; The straight seam steel pipe is subjected to high frequency heating, three-roll rolling, online heat treatment and slow cooling in sequence to obtain a straight seam welded hollow anchor rod body.

6. The preparation method according to claim 5, It is characterized in that The S of the molten iron obtained by the smelting is ≤0.003% when entering the converter, and the argon blowing time of the small platform process is ≥8min; the LF refining is argon-blown throughout the whole process, and 70TiFe alloy is used for micro-titanium treatment before leaving the station; the heating temperature after continuous casting is 1200-1300°C, the time is 150-250min, and the soaking time is ≥30min.

7. The preparation method according to claim 5, It is characterized in that The rough rolling is performed in 5 or 7 passes; the finish rolling is performed in 7 passes, the start rolling temperature of the finish rolling is 1000-1100°C, the reduction rates of the last three stands are ≥17%, ≥15% and ≥12% respectively, and the final rolling temperature is 850-900°C.

8. The preparation method according to claim 5, It is characterized in that The laminar cooling adopts a front-stage cooling mode, the cooling rate is 50-70°C / s, and the coiling temperature is 595-625°C.

9. The preparation method according to claim 5, It is characterized in that The welding power is 100-110 kW, the frequency is 290-300 kHz, and the metal flow line angle of the welding joint is 55-65°; the temperature of the high-frequency heating is 890-900°C, and the quenching end temperature of the online heat treatment is 290-300°C.

10. A The straight seam welded hollow anchor rod body for railway tunnel is prepared from the steel for the straight seam welded hollow anchor rod body according to any one of claims 1 to 4.

Citation Information

Cited By

  • Steel for 1000MPa-grade hollow anchor rod body and preparation method of rod body

    CN121472721A