Water-based UV jet printing ink for textile fabrics and preparation method of water-based UV jet printing ink
By preparing water-based UV inkjet inks with specific compositions and processes, the problems of poor adhesion, inconsistent drying speed, and insufficient color saturation in existing technologies have been solved, achieving high adhesion, rapid drying, and color saturation of the ink, thereby improving printing stability and quality.
Patent Information
- Application Number
- CN202411283860.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-15
AI Technical Summary
Existing UV inkjet inks suffer from problems such as poor adhesion, inconsistent drying speed, and insufficient color saturation, resulting in unstable printing effects.
A water-based UV inkjet ink composed of polyurethane resin, modified UV-curable resin, dyes, etc., is prepared by a modified UV-curable resin preparation method, including high-pressure reaction and vacuum degassing, to produce an ink with excellent hardness, scratch resistance and smoothness.
It improves ink adhesion, drying speed, and color saturation, enhances printing stability and quality, and exhibits suitable ink viscosity and low surface tension.
Smart Images

Figure BDA0005042516430000071 
Figure BDA0005042516430000081 
Figure BDA0005042516430000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of UV inkjet printing, and in particular relates to a water-based UV inkjet printing ink for textiles and a preparation method thereof. Background Art
[0002] Inkjet printing ink is a new printing technology that has developed rapidly in recent years. Inkjet printing ink is the main consumables for inkjet printing production. Water-based UV inkjet uses water as a solvent, which is more environmentally friendly than traditional solvent-based inks, and is more friendly to the environment and human body. It uses ultraviolet (UV) light sources to cure the ink, which can dry quickly and provide scratch resistance and light resistance. At the same time, it uses micro nozzles to spray the ink in precise droplets, which can achieve high-resolution printing on a variety of substrates. The combination of these technologies makes water-based UV inkjet have significant advantages in environmental protection, efficiency and printing quality.
[0003] The cost of existing UV inkjet printing inks and related equipment is usually higher than that of traditional inks, and some water-based UV inks have poor adhesion, which may lead to unstable printing effects. At the same time, water-based UV inks may have problems such as inconsistent drying speed or insufficient color saturation in some cases. A Chinese patent with publication number CN108729262A discloses an inkjet printing reactive dye ink for pure cotton fabrics, which uses a photoinitiator to quickly form free radicals in the system to assist the reactive dye to combine with the cotton fiber surface, significantly improving the dyeing effect, but it still has the problem of poor inkjet ink adhesion.
[0004] In view of the above technical defects, a solution is now proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a water-based UV inkjet printing ink for textiles and a preparation method thereof, which, compared with the existing inkjet printing ink, not only has excellent hardness, scratch resistance, alcohol resistance and smoothness, but also has the advantages of stable physical and chemical properties, rapid drying, appropriate ink viscosity, etc., which can greatly improve the printing stability.
[0006] To achieve the above technical purpose, the present invention adopts the following technical scheme: a water-based UV inkjet printing ink for textiles is composed of the following percentage components: 20-30% polyurethane resin, 1-3% ethyl propionate, 35-50% modified UV light-curing resin, 2-5% dye, 1-3% polyether silane, 1-3% polyvinyl pyrrolidone, 0.5-1% γ-epoxypropyl triethoxy silane, 0.5-1% γ-vinyl triethoxy silane, 0.5-1% γ-aminopropyl triethoxy silane, 3-5% polyacrylic acid, 3-5% polystyrene sulfonate, 2-5% polyvinyl alcohol and 2-5% ethyl benzoate;
[0007] The preparation method of the modified UV light-curable resin comprises the following steps:
[0008] A1: Add epoxy resin and glacial acetic acid into deionized water, heat in a three-necked flask equipped with a thermometer and a magnetic stirrer, adjust the reaction temperature to 65-85°C, set the speed to 1000-1200 rpm, and stir for 1.5-2 hours to obtain intermediate A;
[0009] A2: Add chitin to the intermediate A, use a high-pressure reactor equipped with a stirrer, a thermometer and a condenser, adjust the temperature to 120-150°C, the pressure to 10-15 MPa, and the stirring rate to 600-800 rpm, and stir the reaction for 30 minutes, then turn on the condenser to heat and reflux the product, and heat and reflux for 5-6 hours to obtain the intermediate B;
[0010] A3: Transfer intermediate B to a high shear mixer, add epoxy propiophenone, adjust the reaction temperature to 65-85°C, the speed of the device to 1000-1200 rpm, and stir for 1.5-2h to make the epoxy propiophenone evenly dispersed in the resin matrix to obtain intermediate C;
[0011] A4: Transfer intermediate C to a distillation tower, distill under high pressure and temperature, collect the distillation bottom product after distillation for 3-5 hours, transfer the distillation bottom product to room temperature and cool for 1-2 hours to obtain intermediate D;
[0012] A5: Transfer intermediate D to a vacuum degasser and perform vacuum degassing for 15 min to remove bubbles in intermediate D to obtain a modified UV light-curable resin;
[0013] Furthermore, the resin matrix of the modified UV light-curing resin is one or two of bisphenol A epoxy resin, bisphenol F epoxy resin, epoxyphenol resin, propylene oxide resin, aliphatic epoxy resin, glycidyl epoxy resin or dimer acid-modified epoxy resin.
[0014] Furthermore, the concentration of the glacial acetic acid described in step A1 is 9%; the mass ratio of the epoxy resin, glacial acetic acid and deionized water is 1:4:5; the chitin described in step A2 is a 80-mesh water-soluble powder; the mass ratio of the intermediate A to chitin is 5:1; the mass ratio of the intermediate B to epoxyphenylacetone described in step A3 is 10:1; the pressure of the distillation tower described in step A4 is 0.5atm; and the temperature is 150°C.
[0015] A method for preparing a water-based UV inkjet printing ink for textiles comprises the following steps:
[0016] B1: Preparation of modified UV light-curing resin;
[0017] B2: The modified UV light-curable resin and the polyurethane resin were mixed in a reaction kettle, stirred at 55-65°C and 800-1200 rpm for 30 min, then ethyl propionate, polyether silane and polyvinyl pyrrolidone were added, the reaction temperature was adjusted to 80-90°C, stirred at 800-1200 rpm for 1.5 h, then vacuum filtered, and the filter cake was washed to obtain product 1;
[0018] B3: Add γ-epoxypropyltriethoxysilane, γ-vinyltriethoxysilane and γ-aminopropyltriethoxysilane to product 1, transfer the reactor to an air bath, heat to 65-80°C with steam, heat for 30 minutes, add a magnetic rotor to the reactor, transfer the air bath to a magnetic rotor stirrer, set the speed to 900-1000 rpm, magnetically stir for 30 minutes, then remove the magnetic rotor to obtain product 2;
[0019] B4: Add polyacrylic acid, polystyrene sulfonate, polyvinyl alcohol and ethyl benzoate to product 2, adjust the temperature of the air bath to 55-60°C, set the speed of the magnetic rotor stirrer to 600-800 rpm, stir at a low speed for 2 hours to fully mix the components in the product, then transfer the product to an oil bath, adjust the temperature of the oil bath to 120-150°C, set the speed to 400-600 rpm and stir for 1.5 hours to obtain product 3;
[0020] B5: Add dye to product 3 and stir evenly with a glass rod to obtain product 4;
[0021] B6: The product 4 was transferred to a vacuum degasser and vacuum degassed for 15 minutes to remove the bubbles in the product 3 to obtain a water-based UV inkjet printing ink for textiles.
[0022] Due to the adoption of the above technical scheme, the beneficial effect of the present invention is that the present invention uses chitin-modified epoxy resin, which not only makes the inkjet ink prepared by the present invention have strong hardness, resistance to sliding and scratching, and alcohol resistance, but also obtains quite excellent smoothness; the inkjet ink prepared by the present invention has suitable ink viscosity, strong adhesion and low surface tension, which can greatly improve the stability of printing. At the same time, the present invention has stable physical and chemical properties and dries quickly, which can significantly improve the saturation of printed colors. DETAILED DESCRIPTION
[0023] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments and diagrams.
[0024] The experimental methods in the following examples, unless otherwise specified, are conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials and reagents used in the following examples, unless otherwise specified, can be obtained from commercial channels.
[0025] Furthermore, the concentration of the glacial acetic acid described in step A1 is 9%; the mass ratio of the epoxy resin, glacial acetic acid and deionized water is 1:4:5; the chitin described in step A2 is 80 mesh water-soluble powder; the mass ratio of the intermediate A and chitin is 5:1; the mass ratio of the intermediate B and epoxypropiophenone described in step A3 is 10:1.
[0026] Example 1
[0027] 1: Add 200g of bisphenol A epoxy resin and 800ml of glacial acetic acid to 1L of deionized water, heat in a three-necked flask equipped with a thermometer and a magnetic stirrer, adjust the reaction temperature to 85°C, set the speed to 1200rpm, and stir for 1.5h to obtain 1.8L of intermediate A;
[0028] 2: Add 360g of chitin to intermediate A, use a high-pressure reactor equipped with a stirrer, a thermometer and a condenser, adjust the temperature to 150°C, the pressure to 15Mpa, and the stirring rate to 800rpm, and stir the reaction for 30min. Then, turn on the condenser to heat and reflux the product. Heat and reflux the reaction for 5h to obtain 2L of intermediate B;
[0029] 3: Transfer 2L of intermediate B to a high shear mixer, add 200ml of epoxypropiophenone, adjust the reaction temperature to 85°C, the speed of the device to 1200rpm, and stir for 2h to make the epoxypropiophenone evenly dispersed in the resin matrix to obtain 2L of intermediate C;
[0030] 4: Transfer 2L of intermediate C to a distillation tower, distill under high pressure, adjust the temperature of the distillation tower to 150°C and the pressure to 0.5atm, collect the bottom product after distillation for 3h, transfer the bottom product to room temperature and cool for 2h to obtain 500g of intermediate D;
[0031] 5: 500 g of intermediate D was transferred to a vacuum degasser and vacuum degassed for 15 min to remove bubbles in the intermediate D to obtain 500 g of Example 1;
[0032] Table 1, reagent parameters used in Example 1
[0033] Drug Name source model parameter Bisphenol A epoxy resin Langfang Senqiang Environmental Protection Technology Co., Ltd. E-44 1kg glacial acetic acid Shandong Baijing New Materials Co., Ltd. 7452 25kg Chitin Shaanxi Xupeptide Biotechnology Co., Ltd. XTZ343 1kg Epoxyphenylacetone Aladdin P16034 1kg
[0034] Example 2
[0035] 1: Add 200g of epoxyphenol resin and 800ml of glacial acetic acid to 1L of deionized water, heat in a three-necked flask equipped with a thermometer and a magnetic stirrer, adjust the reaction temperature to 65°C, set the speed to 1000rpm, and stir for 1.5h to obtain 1.8L of intermediate A;
[0036] 2: Add 360g of chitin to intermediate A, use a high-pressure reactor equipped with a stirrer, a thermometer and a condenser, adjust the temperature to 150°C, the pressure to 15Mpa, and the stirring rate to 700rpm, and stir the reaction for 30min. Then, turn on the condenser to heat and reflux the product. Heat and reflux for 6h to obtain 2L of intermediate B;
[0037] 3: Transfer 2L of intermediate B to a high shear mixer, add 200ml of epoxypropiophenone, adjust the reaction temperature to 80°C, the speed of the device to 1000rpm, and stir for 1.5h to make the epoxypropiophenone evenly dispersed in the resin matrix to obtain 2L of intermediate C;
[0038] 4: Transfer 2L of intermediate C to a distillation tower, distill under high pressure, adjust the temperature of the distillation tower to 150°C and the pressure to 0.5 atm, collect the distillation bottom product after distillation for 5 hours, transfer the distillation bottom product to room temperature and cool for 2 hours to obtain 500g of intermediate D;
[0039] 5: 500 g of intermediate D was transferred to a vacuum degasser and vacuum degassed for 15 min to remove bubbles in intermediate D to obtain 500 g of Example 2;
[0040] Table 2, reagent parameters used in Example 2
[0041] Drug Name source model parameter Epoxy phenol resin Guangzhou Konari New Materials Co., Ltd. NPEF-170 500L glacial acetic acid Shandong Baijing New Materials Co., Ltd. 7452 25kg Chitin Shaanxi Xupeptide Biotechnology Co., Ltd. XTZ343 1kg Epoxyphenylacetone Aladdin P16034 1kg
[0042] Example 3
[0043] 1: 100 g of Example 1 and 40 g of polyurethane resin were mixed in a reaction kettle, stirred at 65° C. and 1200 rpm for 30 min, then 2 g of ethyl propionate, 2 g of polyether silane and 2 g of polyvinyl pyrrolidone were added, the reaction temperature was adjusted to 90° C., stirred at 1200 rpm for 1.5 h, then vacuum filtered, and the filter cake was washed to obtain 140 g of product 1;
[0044] 2: Add 1 g of γ-epoxypropyltriethoxysilane, 1 ml of γ-vinyltriethoxysilane and 1 ml of γ-aminopropyltriethoxysilane to 140 g of product 1, transfer the reactor to an air bath, heat to 80 ° C with steam, heat for 30 min, add a magnetic rotor to the reactor, transfer the air bath to a magnetic rotor stirrer, set the speed to 1000 rpm, magnetically stir for 30 min, then remove the magnetic rotor to obtain 140 g of product 2;
[0045] 3: Add 6 g of polyacrylic acid, 6 g of polystyrene sulfonate, 4 g of polyvinyl alcohol and 4 g of ethyl benzoate to 140 g of product 2, adjust the temperature of the air bath to 60 ° C, set the speed of the magnetic rotor stirrer to 800 rpm, stir at a low speed for 2 h to fully mix the components in the product, then transfer the product to an oil bath, adjust the temperature of the oil bath to 120 ° C, set the speed to 400 rpm and stir for 1.5 h to obtain 160 g of product 3;
[0046] 4: Add 4 g of dye to 160 g of product 3 and stir evenly with a glass rod to obtain product 4;
[0047] 5: Transfer product 4 to a vacuum degasser and perform vacuum degassing for 15 min to remove bubbles in product 3 to obtain Example 3.
[0048] Table 3, reagent parameters used in Example 3
[0049]
[0050]
[0051] Example 4
[0052] 1: 100 g of Example 2 and 40 g of polyurethane resin were mixed in a reaction kettle, stirred at 55° C. and 1000 rpm for 30 min, then 2 g of ethyl propionate, 2 g of polyether silane and 2 g of polyvinyl pyrrolidone were added, the reaction temperature was adjusted to 90° C., stirred at 1200 rpm for 1.5 h, then vacuum filtered, and the filter cake was washed to obtain 140 g of product 1;
[0053] 2: Add 1 g of γ-epoxypropyltriethoxysilane, 1 ml of γ-vinyltriethoxysilane and 1 ml of γ-aminopropyltriethoxysilane to 140 g of product 1, transfer the reactor to an air bath, heat to 75 ° C with steam, heat for 30 min, add a magnetic rotor to the reactor, transfer the air bath to a magnetic rotor stirrer, set the speed to 1000 rpm, magnetically stir for 30 min, then remove the magnetic rotor to obtain 140 g of product 2;
[0054] 3: Add 6 g of polyacrylic acid, 6 g of polystyrene sulfonate, 4 g of polyvinyl alcohol and 4 g of ethyl benzoate to 140 g of product 2, adjust the temperature of the air bath to 60 ° C, set the speed of the magnetic rotor stirrer to 700 rpm, stir at a low speed for 2 h to fully mix the components in the product, then transfer the product to an oil bath, adjust the temperature of the oil bath to 120 ° C, set the speed to 500 rpm and stir for 1.5 h to obtain 160 g of product 3;
[0055] 4: Add 4 g of dye to 160 g of product 3 and stir evenly with a glass rod to obtain product 4;
[0056] 5: Transfer product 4 to a vacuum degasser and perform vacuum degassing for 15 min to remove bubbles in product 3 to obtain Example 4.
[0057] Table 4, reagent parameters used in Example 4
[0058]
[0059] Comparative Example 1
[0060] Example 1 of Chinese patent publication number CN108729262A was selected as comparative example 1.
[0061] Comparative Example 2
[0062] Example 1 of the Chinese patent with publication number CN118109080A was selected as comparative example 2.
[0063] Physical and chemical properties test:
[0064] Example 3, Example 4, Comparative Example 1 and Comparative Example 2 were placed in a 60° C. oven and a 0° C. refrigerator for 14 days, respectively, and the physicochemical properties were tested.
[0065] Table 5, Physical and chemical properties test results
[0066] 60℃ after 14 days 0℃ after 14 days Precipitation phenomenon Example 3 No change Unchanged No precipitation Example 4 Unchanged No change No precipitation Comparative Example 1 No change No change No precipitation Comparative Example 2 Unchanged No change A small amount of particle precipitation
[0067] From the analysis of Table 5, it can be seen that the inkjet printing inks prepared in Examples 3 and 4 did not undergo any changes in physical and chemical properties after being placed in a 60°C oven and a 0°C refrigerator for 14 days, and no precipitation was generated.
[0068] Washability test:
[0069] Example 3, Example 4, Comparative Example 1 and Comparative Example 2 were respectively applied to pure cotton fabric inkjet printing, and the color fastness and washing fixation rate of the fabric were measured.
[0070] Table 6, Washability Test Results
[0071]
[0072] From the analysis of Table 6, it can be seen that the inkjet printing inks prepared in Examples 3 and 4 have better color fastness to washing and color fastness to rubbing, and the color fixation rate after washing is above 96.5%.
[0073] Physical performance test:
[0074] Example 3, Example 4, Comparative Example 1 and Comparative Example 2 were printed on acrylic plates to form patterns, and the patterns were wiped with a paper towel under a pressure of 0.5 kg to test the surface smoothness; the adhesion test was carried out with reference to the cross-cut test of paint and varnish film in GB / T 9286-1988. The test result of grade 0 indicates that the coating cut edge is completely smooth and no grid falls off; grade 3 indicates that the coating falls off partially or completely in large fragments along the cut edge, or falls off partially or completely at different parts of the grid, which is significantly greater than 15%, but the affected area is significantly less than 35%; with reference to GB 6739-1986 "Coating Hardness Pencil Determination Method" measures hardness, 6H is the hardest, and from hard to soft are 5H, 4H, 3H, 2H, H, HB, B, 2B, 3B, 4B, 5B, 6B; wipe the pattern with a paper towel soaked in alcohol under a pressure of 1KG, and observe whether the paper towel is stained to test the surface's alcohol wiping resistance; use a rotational viscometer to test the viscosity of the ink; use the Wilhelmy disk method to test the surface tension, hang a platinum sheet on a torsion balance, and measure the pressure when the bottom parallel surface of the platinum sheet just touches the liquid surface, which is the surface tension.
[0075] Table 7, Physical properties test results
[0076]
[0077] By analyzing Table 7, it can be seen that the inkjet printing inks prepared in Example 3 and Example 4 have better performance in surface smoothness, adhesion, hardness, alcohol resistance, viscosity and surface tension.
[0078] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A water-based UV inkjet printing ink for textiles, characterized in that: The invention is composed of the following percentage components: 20-30% polyurethane resin, 1-3% ethyl propionate, 35-50% modified UV light curing resin, 2-5% dye, 1-3% polyether silane, 1-3% polyvinyl pyrrolidone, 0.5-1% γ-epoxypropyl triethoxy silane, 0.5-1% γ-vinyl triethoxy silane, 0.5-1% γ-aminopropyl triethoxy silane, 3-5% polyacrylic acid, 3-5% polystyrene sulfonate, 2-5% polyvinyl alcohol and 2-5% ethyl benzoate; The preparation method of the modified UV light-curable resin comprises the following steps: A1: Add epoxy resin and glacial acetic acid into deionized water, heat in a three-necked flask equipped with a thermometer and a magnetic stirrer, adjust the reaction temperature to 65-85°C, set the speed to 1000-1200 rpm, and stir for 1.5-2 hours to obtain intermediate A; A2: Add chitin to the intermediate A, use a high-pressure reactor equipped with a stirrer, a thermometer and a condenser, adjust the temperature to 120-150°C, the pressure to 10-15 MPa, and the stirring rate to 600-800 rpm, and stir the reaction for 30 minutes, then open the condenser to heat and reflux the product, and heat and reflux for 5-6 hours to obtain the intermediate B; A3: Transfer intermediate B to a high shear mixer, add epoxy propiophenone, adjust the reaction temperature to 65-85°C, the speed of the device to 1000-1200 rpm, and stir for 1.5-2 hours to evenly disperse the epoxy propiophenone in the resin matrix to obtain intermediate C; A4: Transfer intermediate C to a distillation tower, distill under high pressure and temperature, and collect the distillation bottom product after distillation for 3-5 hours; transfer the distillation bottom product to room temperature and cool it for 1-2 hours to obtain intermediate D; A5: Transfer intermediate D to a vacuum degasser and perform vacuum degassing for 15 minutes to remove bubbles in intermediate D to obtain a modified UV light-curable resin.
2. The method for preparing a water-based UV inkjet printing ink for textiles according to claim 1, characterized in that: The following steps are involved: B1: Preparation of modified UV light-curing resin; B2: The modified UV light-curable resin and the polyurethane resin were mixed in a reaction kettle, stirred at 55-65°C and 800-1200 rpm for 30 min, then ethyl propionate, polyether silane and polyvinyl pyrrolidone were added, the reaction temperature was adjusted to 80-90°C, stirred at 800-1200 rpm for 1.5 h, then vacuum filtered, and the filter cake was washed to obtain product 1; B3: Add γ-epoxypropyltriethoxysilane, γ-vinyltriethoxysilane and γ-aminopropyltriethoxysilane to product 1, transfer the reactor to an air bath, heat to 65-80°C with steam, heat for 30 minutes, add a magnetic rotor to the reactor, transfer the air bath to a magnetic rotor stirrer, set the speed to 900-1000 rpm, magnetically stir for 30 minutes, then remove the magnetic rotor to obtain product 2; B4: Add polyacrylic acid, polystyrene sulfonate, polyvinyl alcohol and ethyl benzoate to product 2, adjust the temperature of the air bath to 55-60°C, set the speed of the magnetic rotor stirrer to 600-800 rpm, stir at a low speed for 2 hours to fully mix the components in the product, then transfer the product to an oil bath, adjust the temperature of the oil bath to 120-150°C, set the speed to 400-600 rpm and stir for 1.5 hours to obtain product 3; B5: Add dye to product 3 and stir evenly with a glass rod to obtain product 4; B6: The product 4 was transferred to a vacuum degasser and vacuum degassed for 15 minutes to remove the bubbles in the product 3 to obtain a water-based UV inkjet printing ink for textiles.
3. The aqueous UV inkjet printing ink for textiles according to claim 1, characterized in that: The epoxy resin is one or two of bisphenol A epoxy resin, bisphenol F epoxy resin, epoxyphenol resin, propylene oxide resin, aliphatic epoxy resin, glycidyl epoxy resin or dimer acid modified epoxy resin.
4. The aqueous UV inkjet printing ink for textiles according to claim 1, characterized in that: The concentration of the glacial acetic acid in step A1 is 9%; the mass ratio of the epoxy resin, glacial acetic acid and deionized water is 1:4:
5.
5. The aqueous UV inkjet printing ink for textiles according to claim 1, characterized in that: The chitin described in step A2 is a 80-mesh water-soluble powder; the mass ratio of the intermediate A to chitin is 5:
1.
6. The aqueous UV inkjet printing ink for textiles according to claim 1, characterized in that: The mass ratio of the intermediate B and epoxypropiophenone described in step A3 is 10:
1.