Preparation method of low-basis-weight high-density fiber material
By filling the battery separator material with ultrafine powder and setting a hot melt powder layer, the problem of excessive thickness and insufficient tensile strength of the battery separator material prepared by the wet papermaking process is solved, and low thickness, high density and high safety are achieved battery separator material.
Patent Information
- Application Number
- CN202410980084.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The thickness of the battery separator material prepared by the existing wet papermaking process is too high, resulting in poor tensile strength and cannot meet the thickness requirements of power lithium batteries. At the same time, it lacks sufficient safety, especially in the automatic cutting off current function during heating. .
Using the preparation method of low-quantity high-density fiber material, the thermally closed holes of the material are enhanced by filling the fiber layer with ultrafine powder and setting a hot melt powder layer on one side of the fiber layer. Function, improve safety. Specific steps include mixed slurry molding, hydrospinning reinforcement, dehydration, rolling and coating of hot melt powder layers, controlling the thickness and density of the fiber layer.
The low thickness, high density and high porosity of the battery separator material are achieved, the fracture strength and safety of the material are improved, the use requirements of power lithium batteries are met, and the problems of excessive thickness and insufficient tensile strength of the existing materials are solved. .
Smart Images

Figure CN118958042A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nonwoven materials, and in particular relates to a method for preparing a low-quantity high-density fiber material. Background Art
[0002] In recent years, the rapid development of the new energy vehicle industry has driven the rapid growth of the battery separator field. At present, the separator materials of power batteries are mostly non-renewable polyolefin materials. The initial investment cost of producing such materials is high, and the performance and safety of the battery are also affected to a certain extent due to the poor wettability and thermal dimensional stability of such materials. Based on this, seeking a solution to solve the wettability and thermal dimensional stability of polyolefin materials has become an important topic in this field.
[0003] At present, battery separators prepared by wet papermaking process have been widely used in alkaline manganese, nickel-metal hydride and lead-acid batteries, but the thickness of the separator is generally above 100 microns, which is much higher than the thickness of less than 40 microns required for power lithium batteries. Therefore, the key to further application and expansion of wet papermaking and similar processes in the field of battery separators is how to reduce the thickness of the material and how to have better tensile strength and air permeability at low thickness.
[0004] The Chinese patent document with publication number CN108933217A discloses a method for preparing an ultra-fine polyester fiber non-woven lithium-ion battery separator. The separator is made of ultra-fine short polyester fibers through wet non-woven technology, with a thickness of 20-50 μm and a surface density of 10-35 g / m 2 The preparation steps include dispersing extremely fine and short polyester fibers in water containing a fiber dispersant to form a fiber dispersion slurry, and then using a wet non-woven fabric manufacturing device similar to a papermaking machine to sequentially filter, paper, dehydrate, dry, hot roll and other processes to form a non-woven fabric type lithium-ion battery separator. Compared with conventional polyolefin microporous membrane type lithium-ion battery separators, this separator has higher temperature resistance and higher porosity, can provide a larger liquid absorption capacity and lower resistance, and can give the battery better electrical performance and safety performance.
[0005] However, the extremely fine and short polyester fibers used in this material cannot provide good strength for the material, and it does not have the function of automatically cutting off the current when the battery heats up, and is not sufficiently safe. Summary of the invention
[0006] In order to overcome the technical problems of the battery diaphragm material prepared by the wet papermaking process in the prior art being too thick and the poor tensile strength caused by the reduced thickness; one object of the present invention is to provide a method for preparing a low-quantity high-density fiber material, by filling ultrafine powder in the fiber layer so that the fiber layer has the characteristics of multiple voids, small pore size, and uniform distribution, and a hot-melt powder layer is arranged on one side of the fiber layer so that the fiber material has a thermal closed-pore function, thereby increasing the safety of the battery diaphragm.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme: a method for preparing a low-quantity high-density fiber material, wherein the fiber material comprises a fiber layer and a hot-melt powder layer arranged on one side of the fiber layer; the fiber layer is filled with ultrafine powder; the method for preparing the fiber material comprises the following steps:
[0008] (1) mixing polyvinyl alcohol ultra-short fibers and hydrophobic polyester ultra-fine ultra-short fibers to prepare a first slurry with a concentration of 0.5-1%;
[0009] (2) preparing hydrophilic fine-denier ultra-short cellulose fibers into a fiber slurry with a concentration of 0.5-2%, and then sending the fiber slurry into a refiner for refining to prepare a second slurry with a beating degree of 60°SR-85°SR;
[0010] (3) mixing the first slurry and the second slurry into a mixed slurry, and then conveying the mixed slurry to an inclined wire former through a slurry pump to form a wet-laid fiber web;
[0011] (4) feeding the wet-laid fiber web into a hydroentanglement system to reinforce the front and back sides to form an intermediate material, and the hydroentanglement pressure is configured according to the processing sequence of low pressure, high pressure, and low pressure (40kg, 60kg, 90kg, 90kg, 70kg, and 70kg);
[0012] (5) dehydrating the intermediate material after spunlacing by negative pressure suction, and then sending the intermediate material into a hot water bath at 40° C. to 90° C. to dissolve the polyvinyl alcohol ultrashort fibers;
[0013] (6) subjecting the intermediate material obtained in step (5) to a first-stage rolling process, so that the material reaches a first thickness of 0.15-0.25 mm;
[0014] (7) preparing the ultrafine powder into a suspension, and then immersing the intermediate material after the first stage rolling into the suspension to fill the ultrafine powder into the intermediate material;
[0015] (8) drying the impregnated intermediate material, and then subjecting it to a second rolling process, and controlling the rolling temperature to 80-120° C., so that the material reaches a second thickness of 0.08-0.15 mm, thereby forming the fiber layer;
[0016] (9) preparing a hot-melt powder into a suspension slurry, and then coating and fixing the suspension slurry onto one side of the fiber layer to form the hot-melt powder layer;
[0017] (10) subjecting the fiber layer coated with the hot-melt powder layer to a third-level rolling process, controlling the material to reach a third thickness of 0.02-0.04 mm;
[0018] (11) Finally, the fiber material is manufactured.
[0019] The length and fineness of the fiber directly affect the porosity and pore size in the fiber material. The fiber layer in this solution is composed of ultra-short fibers connected to each other. The purpose of this arrangement is to obtain a smaller pore size in the fiber layer; and the ultra-fine powder is filled in the fiber layer to make the pore size distribution in the fiber layer more uniform and further reduce the pore size in the fiber layer, so as to meet the technical requirements of multiple voids, small pore size and uniform distribution required by the battery separator;
[0020] The purpose of providing the hot-melt powder layer on one side of the fiber layer is to enable the fiber material to have a thermal pore-closing function and meet the safety requirements of the battery separator.
[0021] Furthermore, the total mass of the hot-melt powder layer accounts for 3-8% of the total mass of the fiber material; the total mass of the ultrafine powder accounts for 4-12% of the total mass of the fiber layer; the mass of the fine denier ultrashort cellulose fibers accounts for 0%-30% of the total mass of the fiber layer, and the remainder is the polyester ultrafine and ultrashort fibers.
[0022] The polyester ultrafine and ultrashort fibers are used according to the use requirements of the battery separator to enable the product to obtain higher breaking strength, and the purpose of adding the hydrophilic fine denier ultrashort cellulose fibers to the polyester ultrafine and ultrashort fibers is to improve the wetting properties of the battery separator and enhance the wetting ability of the electrolyte to the material.
[0023] Furthermore, the ultrafine powder is composed of one or more combinations of alumina, silica, zirconium oxide, titanium oxide, and nanocellulose; and the particle size of the ultrafine powder is 0.1 μm-0.6 μm.
[0024] Specifically, when the mass of the polyester ultrafine and ultrashort fibers is greater than 90% of the total mass of the fiber layer, the ultrafine powder includes nanocellulose.
[0025] When the polyester ultrafine and ultrashort fibers account for a high proportion (i.e., >90%), in order to improve wettability, the ultrafine powder filled needs to be hydrophilic; filling the fiber layer with the ultrafine powder can adjust the porosity and pore size distribution of the material, wherein the nanocellulose can also enhance the material's wetting properties to the electrolyte.
[0026] Furthermore, the material of the hot-melt powder layer is polypropylene or polyethylene, which is used to ensure the safety of the battery separator product.
[0027] Specifically, in step (1), the mass proportion of the polyester ultrafine and short fibers is 50%-70%; the remainder is the polyvinyl alcohol ultrafine and short fibers.
[0028] The polyvinyl alcohol ultra-short fibers are mainly used to adjust the pores of the material and reduce the mass per unit area of the material.
[0029] Preferably, the length of the polyvinyl alcohol ultra-short fibers is 1-4 mm, and the linear density is 0.5 dtex-2.5 dtex; the linear density or length of the polyvinyl alcohol ultra-short fibers is at least two specifications.
[0030] Preferably, the polyester ultrafine and short fibers include at least two fiber lengths; the polyester ultrafine and short fibers have a fineness of 0.05 dtex-0.5 dtex and a length of 5-10 mm.
[0031] Battery separators require pores smaller than 0.5μm. Compared with ordinary fibers, the polyester ultrafine short fibers will bring smaller pores and pores. By controlling the length ratio of the fibers, you can obtain materials with good uniformity and better material strength. When the length of the polyester ultrafine short fibers is less than 5mm, the breaking strength of the material shows a sharp decline as the fiber length decreases.
[0032] Preferably, the cross-sectional shape of the polyester ultrafine and ultrashort fibers is a combination of one or more of circular, rectangular and triangular shapes.
[0033] The cross-sectional shape of the fibers will affect the mutual entanglement between the fibers; using fibers with different cross-sections can improve the entanglement efficiency of the fibers in the fiber layer, so that the material can obtain better breaking strength.
[0034] Preferably, the fine denier ultra-short cellulose fibers are one or more combinations of viscose fibers, modal fibers, and lyocell fibers; the fineness of the fine denier ultra-short cellulose fibers is 0.1 dtex-1.0 dtex, and the length is 3-7 mm.
[0035] Battery separator materials have high requirements for pore size, generally requiring the pore size to be controlled below 0.5μm. Compared with ordinary fibers, ultrafine fibers will bring smaller pores and pore sizes.
[0036] Preferably, the fine denier cellulose fiber is lyocell (tencel) fiber; the lyocell (tencel) fiber will have a fibrillation effect after being treated, and fine fluff will be generated on the fiber surface, which can bring smaller pores and pore sizes.
[0037] Preferably, the mass per unit area of the fiber material is 10-30 g / m 2 ;
[0038] Preferably, the fiber packing density of the fiber material is 0.5-1 g / cm 3 .
[0039] Preferably, the thickness of the fiber material is 0.02-0.04 mm. The thickness of the battery separator material directly affects the performance of the battery. On the premise of ensuring the material properties, the thickness of the battery separator material is required to be as low as possible.
[0040] The solution is as follows: the thickness of the battery separator material is required to be less than 40μm, and the basic requirement is that the gram weight is less than 30 grams; the material pore size is required to be smaller, that is, the fiber stacking density is higher than that of ordinary materials.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) The present invention adds polyvinyl alcohol ultra-short fibers to the polyester ultra-fine and ultra-short fiber slurry and reasonably sets the water dissolution temperature, which is not only beneficial to wet web forming and fiber web reinforcement, but also, because the polyvinyl alcohol ultra-short fibers are dissolved in the subsequent hot water bath, the unit area mass of the material is reduced, thereby solving the problem that the existing fiber materials cannot be applied to battery separator materials due to their high quantitativeness.
[0043] (2) The present invention fills the fiber layer with ultrafine powder, reduces the pore size in the fiber layer, and plays a role in increasing the material density at a low quantitative level, solving the problem that the existing non-woven materials cannot be applied to battery separators due to the large pore size. At the same time, the thermal pore-closing effect of ultrafine powder can ensure the safety of battery separator products.
[0044] (3) The present invention applies and fixes a hot-melt powder layer to one side of the fiber layer surface, further reducing the pore size on the material surface and further increasing the material density at a low quantity, thereby improving the material's breaking strength, meeting the use requirements of battery separators, and solving the problem that existing ordinary fiber materials cannot be applied to battery separators.
[0045] (4) During the product preparation process, the present invention performs the first stage rolling and the second stage rolling on the intermediate material respectively, and reasonably sets the second stage rolling temperature, thereby gradually reducing the material thickness, increasing the material density, and improving the material breaking strength, so that the final product can achieve the technical requirements of low quantity, high density and high porosity, thereby solving the problem that the existing fiber materials cannot meet the requirements for use in battery separators. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 It is a schematic diagram of the structure of the fiber material of the present invention;
[0047] Figure 2 It is a schematic diagram of the preparation process of the fiber material of the present invention.
[0048] In the figure: 1. Fiber layer; 2. Ultrafine powder; 3. Hot-melt powder layer. DETAILED DESCRIPTION
[0049] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.
[0050] In the description of the present invention, it should be noted that directional words, such as the terms "center", "lateral", "longitudinal", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc., indicating directions and positional relationships are based on the directions or positional relationships shown in the accompanying drawings, which are only for the convenience of narrating the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and cannot be understood as limiting the specific scope of protection of the present invention.
[0051] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features. Therefore, the definition of "first" and "second" features can explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "several" is two or more, unless otherwise clearly and specifically defined.
[0052] In the present invention, unless otherwise specified and limited, the terms "setting", "installation" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can also be a mechanical connection; it can be directly connected, or it can be connected through an intermediate medium, or the two elements can be internally connected. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0053] See also Figure 1-Figure 2 A method for preparing a low-quantity high-density fiber material, the fiber material comprises a fiber layer 1 and a hot-melt powder layer 3 arranged on one side of the fiber layer 1; the fiber layer 1 is filled with ultrafine powder 2; the fiber layer 1 is formed by ultrashort fibers entangled and fixed with each other; the ultrafine powder 2 is attached to the ultrashort fibers; the method for preparing the fiber material comprises the following steps:
[0054] (1) mixing polyvinyl alcohol ultra-short fibers and hydrophobic polyester ultra-fine ultra-short fibers to prepare a first slurry with a concentration of 0.5-1%;
[0055] (2) preparing hydrophilic fine-denier ultra-short cellulose fibers into a fiber slurry with a concentration of 0.5-2%, and then sending the fiber slurry into a refiner for refining to prepare a second slurry with a beating degree of 60°SR-85°SR;
[0056] (3) mixing the first slurry and the second slurry into a mixed slurry, and then conveying the mixed slurry to an inclined wire former through a slurry pump to form a wet-laid fiber web;
[0057] (4) feeding the wet-laid fiber web into a hydroentanglement system to reinforce the front and back sides to form an intermediate material, and the hydroentanglement pressure is configured according to the processing sequence of low pressure, high pressure, and low pressure (40kg, 60kg, 90kg, 90kg, 70kg, and 70kg);
[0058] (5) dehydrating the intermediate material after spunlacing by negative pressure suction, and then sending the intermediate material into a hot water bath at 40° C. to 90° C. to dissolve the polyvinyl alcohol ultrashort fibers;
[0059] (6) subjecting the intermediate material of step (5) to a first-stage rolling process, so that the material reaches a first thickness of 0.15-0.25 mm;
[0060] (7) preparing the ultrafine powder into a suspension, and then immersing the intermediate material after the first stage rolling into the suspension to fill the ultrafine powder into the intermediate material;
[0061] (8) drying the impregnated intermediate material, and then subjecting it to a second rolling process, and controlling the rolling temperature to 80-120° C., so that the material reaches a second thickness of 0.08-0.15 mm, thereby forming the fiber layer;
[0062] (9) preparing a hot-melt powder into a suspension slurry, and then coating and fixing the suspension slurry onto one side of the fiber layer to form the hot-melt powder layer;
[0063] (10) subjecting the fiber layer coated with the hot-melt powder layer to a third-level rolling process, controlling the material to reach a third thickness of 0.02-0.04 mm;
[0064] (11) Finally, the fiber material is manufactured.
[0065] Among them, in the step (1), if the concentration of the first slurry is too high, the fibers will be easily entangled during the slurry transportation process, resulting in uneven cloth surface; if the concentration of the first slurry is too low, it will affect the production efficiency; the linear density or length of the polyvinyl alcohol ultra-short fibers is at least two specifications, for example: 1.5dtex*1.5mm and 2dtex*2.5mm are mixed; the water solubility temperature of the polyvinyl alcohol ultra-short fibers is greater than 70°C.
[0066] In the step (1), the mass proportion of the polyester ultrafine and short fibers is 50%-70%; the remainder is the polyvinyl alcohol ultrafine and short fibers.
[0067] There are two purposes for adding the polyvinyl alcohol ultra-short fibers into the raw materials. First, the low-quantity fiber web is not easy to transfer. Adding the polyvinyl alcohol fibers is conducive to the transfer of the fiber web and increases production efficiency. Second, the surface of the polyester ultra-fine short fibers will be very dense after hydroentanglement, which is not conducive to impregnation and sizing. The added polyvinyl alcohol fibers will have pores after being dissolved in hot water, which is conducive to the impregnation of the ultra-fine powder. The polyvinyl alcohol fibers with a water dissolution temperature of >70°C are used to prevent the fibers from being water-soluble during processing.
[0068] In the step (4), the hydroentanglement system adopts a processing sequence of low pressure, high pressure, and low pressure to effectively reduce the hydroentanglement marks on the surface of the material and improve the uniformity of the material. Hydroentanglement reinforcement causes the ultra-short fibers to interweave and embrace, and the fibers are arranged in three dimensions, forming a larger porosity.
[0069] The combination of hydroentanglement reinforcement and two rolling processes can make the material have a higher breaking strength and meet the use requirements of battery separators. At the same time, the hydroentanglement consolidation material will be relatively loose and thick, with more pores and uniform pore size, so that the material has enough space for the impregnation liquid to penetrate into the material and allow the ultrafine powder to be adsorbed on each fiber; the second stage uses high-temperature rolling to compact the impregnated material, which can make the pores in the material more uniform and dense; coating the hot-melt powder layer on one side of the material can make the material have a thermal pore-closing function.
[0070] Thermal closure function is a special diaphragm technology that can provide additional safety protection for lithium-ion batteries. The main parameters of this function are thermal closure temperature and thermal rupture temperature. The closure temperature is the temperature at which the micropores inside the diaphragm are closed. When the battery cell is in an abnormal environment such as thermal abuse, overcharging, external short circuit, etc., the temperature inside the battery cell rises rapidly. Since the diaphragm material is a thermoplastic polymer, when the temperature approaches the melting point of the polymer, the micropores inside the diaphragm are thermally closed, the lithium ion transmission channel is blocked, and a short circuit is formed inside the battery cell, thereby protecting the battery.
[0071] The total mass of the hot-melt powder layer accounts for 3-8% of the total mass of the fiber material; the total mass of the ultrafine powder accounts for 4-12% of the total mass of the fiber layer; the mass of the fine denier ultrashort cellulose fibers accounts for 0%-30% of the total mass of the fiber layer, and the remainder is the polyester ultrafine and ultrashort fibers.
[0072] If the content of the hot melt powder layer is too low, it will affect the thermal pore closing function, and if the content is too high, it will affect the wettability of the material and increase the thickness of the material. If the content of the ultrafine powder is too low, it will be unfavorable to control the pore size of the material, and if it is too high, it will reduce the porosity of the material and reduce the ion conduction efficiency.
[0073] The ultrafine powder is composed of one or more combinations of aluminum oxide, silicon dioxide, zirconium oxide, titanium oxide, and nanocellulose; and the particle size of the ultrafine powder is 0.1 μm-0.6 μm.
[0074] Generally, battery separators require the pore size in the material to be less than 0.5 μm. If the particle size of the ultrafine powder is too large, it is not conducive to controlling the pore size in the material. If the particle size of the ultrafine powder is too small, it is not only not conducive to its fixation on the ultrashort fibers, but also reduces the ion conduction efficiency.
[0075] When the mass of the polyester ultrafine and ultrashort fibers is greater than 90% of the total mass of the fiber layer, the ultrafine powder includes nanocellulose.
[0076] The material of the hot-melt powder layer is polypropylene or polyethylene; the particle size of the hot-melt powder is 0.3 μm-0.8 μm;.
[0077] The length of the polyvinyl alcohol ultra-short fibers is 1-4 mm, and the linear density is 0.5 dtex-2.5 dtex; the linear density or length of the polyvinyl alcohol ultra-short fibers is at least two specifications.
[0078] The polyester ultra-fine short fibers include at least two fiber lengths; the polyester ultra-fine short fibers have a fineness of 0.05 dtex-0.5 dtex and a length of 5-10 mm; and the cross-sectional shape of the polyester ultra-fine short fibers is one or more combinations of circular, rectangular, and triangular.
[0079] The fine denier ultra-short cellulose fiber is one or more combinations of viscose fiber, modal fiber, and lyocell fiber; the fineness of the fine denier ultra-short cellulose fiber is 0.1dtex-1.0dtex, and the length is 3-7mm; preferably, the fine denier cellulose fiber is lyocell (Tencel) fiber; the lyocell (Tencel) fiber will have a fibrillation effect after treatment, and fine fluff will be produced on the fiber surface, which can bring smaller pores and pore sizes.
[0080] Example 1
[0081] A low-quantity high-density fiber material, wherein the fiber layer is composed of PET fiber (polyethylene terephthalate fiber, i.e., the specific selection of the polyester ultrafine and ultrashort fiber), lyocell fiber and nanocellulose powder, wherein the PET fiber accounts for 75% of the total mass of the fiber layer, with a linear density of 0.1dtex and a length of 5mm; the lyocell fiber accounts for 20% of the total mass of the fiber layer, with a linear density of 0.6dtex and a length of 4mm; the nanocellulose powder accounts for 5% of the total mass of the fiber layer, with a powder particle size of 0.1μm. The hot-melt powder layer is provided on the outer surface of the fiber layer, and the hot-melt powder layer is composed of polyethylene powder, with an average powder particle size of 0.5μm. The overall gram weight of the material is 28g / m 2 , thickness is 0.035mm.
[0082] A method for preparing a low-quantity high-density fiber material comprises the following steps:
[0083] (1) PET fibers and polyvinyl alcohol ultra-short fibers are mixed to prepare a first slurry having a concentration of 0.5%;
[0084] (2) preparing the lyocell cellulose fibers into a second slurry with a slurry concentration of 0.5% and a beating degree of 60° SR;
[0085] (3) mixing the first slurry and the second slurry into a mixed slurry, wherein the mass ratio of PET fiber, polyvinyl alcohol ultra-short fiber and lyocell cellulose fiber in the mixed slurry is 4:5:1; and then forming a wet-laid fiber web from the mixed slurry;
[0086] (4) hydroentangle the fibers in the wet-laid fiber web to form an intermediate material;
[0087] (5) placing the intermediate material into a hot water bath to dissolve the polyvinyl alcohol ultrashort fibers; and then subjecting the intermediate material to a first-stage rolling process to a material thickness of 0.2 mm;
[0088] (6) filling the ultrafine powder into the intermediate material obtained in step (5);
[0089] (7) subjecting the intermediate material filled with ultrafine powder to a second-stage rolling process to a material thickness of 0.12 mm;
[0090] (8) applying and fixing a hot melt powder layer to one side of the intermediate material;
[0091] (9) The intermediate material coated with the hot-melt powder is subjected to a third-stage rolling process to make the material thickness reach 0.035 mm, thereby obtaining the fiber material.
[0092] Example 2
[0093] A low-basis-weight high-density fiber material, which is different from Example 1 only in that the length of the PET fiber in the fiber layer is 10 mm.
[0094] Example 3
[0095] A low-quantity high-density fiber material, which is different from Example 1 only in that the nanocellulose powder is replaced by titanium oxide.
[0096] Comparative Example 1
[0097] A low-quantity high-density fiber material, which is different from Example 1 only in that: the fiber layer does not contain ultrafine powder, and the PET fiber mass accounts for 80% of the fiber layer.
[0098] Comparative Example 2
[0099] A low-quantity high-density fiber material, which is different from Example 1 only in that the content of nano-cellulose powder in the fiber layer is 15%, and the weight of PET fibers in the fiber layer accounts for 65%.
[0100] Comparative Example 3
[0101] A low-basis-weight high-density fiber material, which is different from Example 1 only in that the outer surface of the fiber layer does not contain a hot-melt powder layer.
[0102] Comparative Example 4
[0103] A low-quantity high-density fiber material, which is different from Example 3 only in that: the PET fiber accounts for 95% of the fiber layer, and does not contain hydrophilic fibers, that is, does not contain lyocell cellulose fibers.
[0104] Comparative Example 5
[0105] A low-basis-weight high-density fiber material, which is different from Example 1 only in that the length of the PET fiber in the fiber layer is 15 mm.
[0106] Comparative Example 6
[0107] A low-basis-weight high-density fiber material, which is different from Example 1 only in that the length of the PET fibers in the fiber layer is 3 mm.
[0108] Test Case
[0109] Test purpose: To determine the suitability of the test material for battery separator applications by testing the material's breaking strength, maximum pore size, porosity and contact angle.
[0110] Test method:
[0111] (1) Breaking strength: in accordance with ISO 9073-3 Textiles - Test methods for nonwovens - Part 3: Determination of breaking strength and elongation.
[0112] (2) Average pore size: in accordance with ASTM F316-03 standard.
[0113] (3) Porosity: This shall be carried out in accordance with GB / T21650.2-2008 “Determination of pore size distribution and porosity of solid materials by mercury intrusion and gas adsorption method Part 2: Analysis of mesopores and macropores by gas adsorption method”.
[0114] (4) Contact angle: in accordance with DB44 / T 1872-2016 standard.
[0115] (5) Thermal closing temperature: in accordance with INASA TM 2010-216099 standard.
[0116] The test results are shown in Table 1
[0117] Comparison table of nonwoven fabric performance test data in various embodiments and comparative examples
[0118]
[0119] Test result analysis:
[0120] 1) From the comparison of the data of Example 1, Example 2, Comparative Example 5 and Comparative Example 6, it can be seen that the length of the PET fibers in the fiber layer is in the range of 5-10 mm. Increasing the fiber length will increase the breaking strength of the material, but the pore size and porosity will become larger due to the uneven distribution of the long fibers during the web-forming process; when the fiber length is too long, the breaking strength of the material is significantly improved, but the pore size and porosity of the material will be too large, which cannot meet the requirements as a battery separator material; when the fiber length is too short, the breaking strength of the material is too low, causing the material to break easily.
[0121] 2) From the comparison between Example 1 and Example 3, it can be seen that after the nanocellulose powder is replaced with titanium oxide powder, the contact angle of the material to the electrolyte increases and the wetting performance decreases.
[0122] 3) From the comparison between Example 1 and Comparative Example 1, it can be seen that the ultrafine powder filled in the fiber layer can effectively improve the pore size and porosity of the material. The increase in pore size makes the material more susceptible to the growth of ion dendrites in the electrolyte piercing the diaphragm, thereby causing safety problems such as short circuit or even explosion.
[0123] 4) From the comparison between Example 1 and Comparative Example 2, it can be seen that excessive filling of ultrafine powder in the fiber layer will reduce the pore size and porosity. Too small pore size will limit the permeability of ions in the electrolyte, thereby increasing the internal resistance of the battery and reducing the overall performance of the battery.
[0124] 5) From the comparison between Example 1 and Comparative Example 3, it can be seen that the hot-melt powder layer coated on the outside of the fiber layer can play a role in thermal pore closure.
[0125] 6) From the comparison between Example 3 and Comparative Example 4, it can be seen that the hydrophilic fibers and nanocellulose powder in the material can effectively reduce the contact angle between the material and the electrolyte and increase its infiltration speed into the electrolyte.
[0126] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0127] The above description is only a specific embodiment of the present invention, but the technical features of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are included in the patent scope of the present invention.
Claims
1. A method for preparing low-quantity high-density fiber material, Features: The fiber material comprises a fiber layer and a hot-melt powder layer arranged on one side of the fiber layer; the fiber layer is filled with ultrafine powder; and the preparation method of the fiber material comprises the following steps: (1) mixing polyvinyl alcohol short fibers and polyester ultrafine short fibers to prepare a first slurry with a concentration of 0.5-1%; (2) preparing hydrophilic fine-denier ultra-short cellulose fibers into a fiber slurry with a concentration of 0.5-2%, and then sending the fiber slurry into a refiner for refining to prepare a second slurry with a beating degree of 60°SR-85°SR; (3) mixing the first slurry and the second slurry to form a mixed slurry, and then making the mixed slurry into a wet-laid fiber web; (4) feeding the wet-laid fiber web into a hydroentanglement system to reinforce the front and back surfaces to form an intermediate material; (5) dehydrating the intermediate material after spunlacing by negative pressure suction, and then sending the intermediate material into a hot water bath at 40° C. to 90° C. to dissolve the polyvinyl alcohol ultrashort fibers; (6) subjecting the intermediate material obtained in step (5) to a first-stage rolling process, so that the material reaches a first thickness of 0.15-0.25 mm; (7) preparing the ultrafine powder into a suspension, and then immersing the intermediate material after the first stage rolling into the suspension to fill the ultrafine powder into the intermediate material; (8) drying the impregnated intermediate material, and then subjecting it to a second rolling process, and controlling the rolling temperature to 80-120° C., so that the material reaches a second thickness of 0.08-0.15 mm, thereby forming the fiber layer; (9) preparing a hot-melt powder into a suspension slurry, and then coating and fixing the suspension slurry onto one side of the fiber layer to form the hot-melt powder layer; (10) subjecting the fiber layer coated with the hot-melt powder layer to a third-level rolling process, controlling the material to reach a third thickness of 0.02-0.04 mm; (11) Finally, the fiber material is manufactured.
2. The preparation method according to claim 1, Features: The total mass of the hot-melt powder layer accounts for 3-8% of the total mass of the fiber material; the total mass of the ultrafine powder accounts for 4-12% of the total mass of the fiber layer; the mass of the fine denier ultrashort cellulose fibers accounts for 0%-30% of the total mass of the fiber layer, and the remainder is the polyester ultrafine and ultrashort fibers.
3. The preparation method according to claim 2, Features: The ultrafine powder is composed of one or more combinations of aluminum oxide, silicon dioxide, zirconium oxide, titanium oxide, and nanocellulose; and the particle size of the ultrafine powder is 0.1 μm-0.6 μm.
4. The preparation method according to claim 3, Features: When the mass of the polyester ultrafine and ultrashort fibers is greater than 90% of the total mass of the fiber layer, the ultrafine powder includes nanocellulose.
5. The preparation method according to any one of claims 1 to 4, Features: The material of the hot-melt powder layer is polypropylene or polyethylene.
6. The preparation method according to any one of claims 1 to 4, Features: In the step (1), the mass proportion of the polyester ultrafine and short fibers is 50%-70%; the remainder is the polyvinyl alcohol ultrafine and short fibers.
7. The preparation method according to any one of claims 1 to 4, Features: The length of the polyvinyl alcohol ultra-short fibers is 1-4 mm, and the linear density is 0.5 dtex-2.5 dtex; the linear density or length of the polyvinyl alcohol ultra-short fibers is at least two specifications.
8. The preparation method according to any one of claims 1 to 4, Features: The polyester ultra-fine and ultra-short fibers include at least two fiber lengths; the polyester ultra-fine and ultra-short fibers have a fineness of 0.05dtex-0.5dtex and a length of 5-10mm.
9. The preparation method according to any one of claims 1 to 4, Features: The cross-sectional shape of the polyester ultrafine and ultrashort fibers is one or more combinations of circular, rectangular and triangular.
10. The preparation method according to any one of claims 1 to 4, Features: The fine denier ultra-short cellulose fibers are one or more combinations of viscose fibers, modal fibers, and lyocell fibers; the fineness of the fine denier ultra-short cellulose fibers is 0.1 dtex-1.0 dtex, and the length is 3-7 mm.
Citation Information
Patent Citations
Battery and capacitor diaphragm filter material formed by wet nonwoven fabrics and preparation method of filter material
CN103100264A
A method for preparing a non-woven fabric type lithium ion battery separating membrane made of ultrafine polyester fibers
CN108933217A
Wet-process molded battery diaphragm with controllable pore diameter and preparation method thereof
CN109326762A
Method for preparing fiber lithium ion battery diaphragm,
CN110429227A
Ultrafine fiber bundle and method for producing the same
JP2003253555A