Preparation method of deep eutectic solvent doped polyvinylidene fluoride solid electrolyte
Through the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte, the liquid leakage and thermal runaway problems of liquid electrolyte in lithium-ion batteries are solved, and a lithium-ion battery with high safety and long life is achieved. Polymer polarity and ionic conductivity improve the cycle life and mechanical strength of the battery.
Patent Information
- Application Number
- CN202411143334.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-15
AI Technical Summary
The liquid organic electrolytes used in existing lithium-ion batteries have liquid leakage, thermal runaway, and instability between the interface between the electrolyte and the positive and negative electrodes, which affects the performance and safety of the battery. In addition, the electrolyte curing in low-temperature environments affects ion transmission and shortens the battery life.
Polyvinylidene fluoride-trifluoroethylene solid electrolyte doped with deep eutectic solvents is used to enhance the polarity of the polymer through a lithium-based deep eutectic solvent composed of hydrogen bond donor and acceptor, forming organic polymer-enhanced phases and ions. The conductive phase improves the conductivity and mechanical strength to prepare a solid electrolyte with excellent electrochemical stability and thermal stability.
The high safety, stability and long life of lithium-ion batteries are achieved, and the polarity of polymer is enhanced through the induction of deep eutectic solvents, the ion transport capability is improved, the growth of Li+ dendrites is inhibited, electrolyte cracks and short circuits are avoided, and the The battery cycle life and safety are provided.
Smart Images

Figure CN118970166A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer electrolytes, and specifically relates to a preparation method of a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte, and application of the solid electrolyte in lithium ion batteries. Background Art
[0002] With the development of science and technology, the rapid growth of smart wearable devices, electric vehicles and static energy storage has continuously promoted the development of energy technology, and the demand for fossil fuels has greatly increased. However, the use of large amounts of fossil fuels will not only cause environmental pollution, but will also accelerate the depletion of non-renewable energy. Although some green energy can currently supply energy in some areas, its performance is greatly affected by the natural environment. Therefore, there is an urgent need for green, reliable, and low-energy energy storage devices to balance the supply. Since its first development by Exxon and Moli Energy in the late 1970s, lithium-ion battery technology has undergone significant development. Lithium-ion batteries have the advantages of high voltage, high energy density, long life, and fast charging, so they are considered to be one of the most promising energy storage technologies. However, the current commercial lithium-ion batteries use liquid organic electrolytes, which have potential risks such as leakage and even fire and explosion. In addition, in low-temperature environments, the electrolyte inside the battery may have solidification problems, affecting the ion transport performance of the battery. More importantly, liquid electrolytes are prone to accelerate the growth of lithium dendrites, destroy the solid electrolyte interface (SEI) film inside the battery, shorten the cycle life of the battery, and even cause the battery to short-circuit. Therefore, developing a highly safe and stable solid electrolyte is a key link in improving the overall performance of lithium-ion batteries.
[0003] Deep eutectic solvents (DESs) are binary or ternary systems composed of hydrogen bond donors (such as polyols, urea and carboxylic acids) and hydrogen bond acceptors (such as quaternary ammonium salts, such as choline chloride). They are easy to synthesize and have good thermal and chemical stability. The presence of deep eutectic solvents can not only improve the electrolyte-electrode interface contact and enhance battery safety, but also provide important guidance for the development of high-performance solid electrolytes due to their excellent electrochemical stability.
[0004] Organic polymer electrolytes have been widely studied because of their good flexibility, good contact with electrodes, and better ion transmission at the polymer-electrode interface. Traditional polymer electrolytes have slow chain segment movement at room temperature, which is not conducive to the transmission of lithium ions, resulting in reduced battery performance. Although the composite solid electrolyte formed after adding inorganic fillers can improve ion conductivity, it will cause a decrease in the flexibility of the polymer electrolyte. The polarity of the polymer has a great influence on its residual polarization, and the size of the residual polarization will affect the degree of dissociation of the lithium salt. Therefore, increasing the polarity of the polymer will help promote the dissociation of the lithium salt, thereby achieving the purpose of improving conductivity. Polyvinylidene fluoride-trifluoroethylene shows an all-trans high polarity conformation. The addition of DES can further improve the polarity of polyvinylidene fluoride-trifluoroethylene. The prepared solid electrolyte has considerable ionic conductivity and migration number, excellent mechanical strength and thermal stability, and can better inhibit Li + Dendrite growth. Deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene electrolyte has the advantages of simple synthesis, excellent thermal stability and electrochemical stability. By adjusting the preparation temperature and the type of deep eutectic solvent, the prepared solid electrolyte has great application potential in lithium-ion batteries. Summary of the invention
[0005] In view of the technical defects of existing lithium-ion batteries, such as leakage of organic electrolyte, thermal runaway, instability of the electrolyte and the interface between the positive and negative electrodes, the purpose of the present invention is to provide a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium-ion electrolyte and its preparation method and use it in lithium-ion batteries. The polarity of polyvinylidene fluoride-trifluoroethylene polymer is enhanced by induction of deep eutectic solvent, the dissociation of lithium in DES is increased, and by dispersing the ion conductive phase in polyvinylidene fluoride-trifluoroethylene, excellent conductivity and mechanical strength are given to construct a stable solid electrolyte.
[0006] Specifically, the present invention is achieved through the following solutions: A deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte comprises an organic polymer reinforcement phase and an ion conductive phase, wherein the organic polymer reinforcement phase is polyvinylidene fluoride-trifluoroethylene; the ion conductive phase is a lithium-based deep eutectic solvent, which is composed of a hydrogen bond donor and a hydrogen bond acceptor; the hydrogen bond donor is at least one of trifluoroacetamide, ethylene glycol, and choline chloride; the hydrogen bond acceptor is at least one of lithium bis(trifluoromethanesulfonyl imide), lithium chloride, and lithium trifluoromethanesulfonate.
[0007] To achieve the above solution, a method for preparing a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte is provided, characterized in that the technical solution comprises the following steps: (1) mixing a hydrogen bond acceptor and a hydrogen bond donor in a certain proportion, heating at a certain temperature for a period of time, and obtaining a lithium-based deep eutectic solvent; (2) Add PVDF-TrFE into an organic solvent in a certain proportion, heat and stir to obtain a uniform and transparent solution; (3) adding the lithium-based deep eutectic solvent obtained in step (1) into step (2) in a certain proportion, and continuing to heat and stir until a stable, uniform, transparent solution is formed; (4) Pour the uniform transparent solution obtained in step (3) into a polytetrafluoroethylene mold and place it in an oven to dry, remove excess solvent, and obtain a polyvinylidene fluoride-trifluoroethylene-DES composite solid electrolyte.
[0008] The preparation method of the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte described in the above technical scheme, the hydrogen bond donor is at least one of trifluoroacetamide, ethylene glycol, and choline chloride; the hydrogen bond acceptor is at least one of lithium bis(trifluoromethanesulfonyl imide), lithium chloride, and lithium trifluoromethanesulfonate. The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:1 to 1:3. As a further improvement of the present invention, the preferred hydrogen bond donor is trifluoroacetamide, and the hydrogen bond acceptor is lithium bis(trifluoromethanesulfonyl imide), and the molar ratio of the two is 2:1.
[0009] Furthermore, in step (1), the heating temperature is 60-80°C, and the heating reaction time is 1-4 h. Preferably, the heating temperature is 50°C, and the heating reaction time is 2.5 h.
[0010] In the method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte described in the above technical scheme, the amount of polyvinylidene fluoride-trifluoroethylene added is 5-10% of the total mass fraction. As a further improvement of the present invention, the preferred amount added is 10% of the total mass fraction.
[0011] Furthermore, in step (2), the heating temperature is 40-70°C, the heating time is 3-5 h, and the organic solvent is one of N,N-dimethylformamide, N-methylpyrrolidone, and N,N-dimethylacetamide. Preferably, the heating temperature is 50°C, the heating time is 5 h, and the organic solvent is N,N-dimethylformamide.
[0012] In the method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte described in the above technical scheme, the mass ratio of the amount of lithium-based DES added to polyvinylidene fluoride-trifluoroethylene in step (3) is (1-3):1, preferably, the mass ratio is 1.3:1. In the method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte described in the above technical scheme, in step (4), the oven is in a vacuum state and the temperature is 40~120°C. Preferably, the solvent evaporation rate is selected to be 100°C.
[0013] The preparation method of the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte described in the above technical scheme, the solid electrolyte is a thin film electrolyte with a film thickness of 0.03~0.1 mm.
[0014] A further object of the present invention is to provide a lithium-ion solid-state battery with a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene electrolyte, comprising a positive electrode, an electrolyte, and a negative electrode, characterized in that the electrolyte is obtained by the preparation method in the above technical solution.
[0015] Preferably, the positive electrode is at least one of lithium iron phosphate, spinel nickel manganese oxide, lithium cobalt oxide, and high nickel ternary materials; the negative electrode is at least one of graphite, metallic lithium, tin-based materials, lithium titanate, and silicon-based negative electrodes.
[0016] Preferably, the lithium-ion solid-state battery is one or more of a button battery, a soft-pack battery, and a cylindrical battery.
[0017] In general, the technical solution of the present invention has the following beneficial effects compared with the prior art: (1) The present invention uses a non-aqueous lithium-based deep eutectic solvent to replace the traditional inorganic lithium salt material, which has high flexibility, high thermal stability, and a wide electrochemical stability window. + By adjusting the solvation structure, a deep eutectic solvent electrolyte with fast ion transport capability is obtained, which can better realize the reversible deposition and stripping of lithium ions.
[0018] (2) The present invention adds a deep eutectic solvent with a solvation structure to polyvinylidene fluoride-trifluoroethylene to prepare a solid electrolyte. By properly regulating the proportion, a composite electrolyte film with excellent ionic conductivity and mechanical strength is obtained, which simplifies the battery structure and further reduces the battery volume. The polarity of polyvinylidene fluoride-trifluoroethylene is enhanced by inducing the deep eutectic solvent and controlling the preparation temperature, increasing the dissociation of lithium in DES. By dispersing the ion conductive phase in polyvinylidene fluoride-trifluoroethylene, excellent conductivity and mechanical strength are given, effectively inhibiting dendrite growth; high flexibility effectively avoids the problem of cracks or even short circuits in the electrolyte caused by stress concentration in the inorganic filler, and improves the cycle life of the battery.
[0019] (3) The deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid lithium ion electrolyte prepared by the present invention has a large number of hydrogen bonds, which fix the solvent molecules in the polymer network. At the same time, the presence of hydrogen bonds gives the solid electrolyte and the electrode material good adhesion, which is beneficial to the Li + migration and stable deposition and stripping. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] To further illustrate the technical solutions in the embodiments of the present invention, the drawings in the embodiments are briefly introduced below. Obviously, the following drawings only represent some embodiments of the present invention and are not used to limit the present invention.
[0021] Figure 1 This is a physical picture of the solid electrolyte in Example 1 of the present invention; Figure 2 Schematic diagram of the internal structure of the solid electrolyte in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] The present invention relates to a preparation method of a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte and the application of the solid electrolyte in a lithium ion battery. The purpose and technical solution of the present invention will be fully and detailedly described below in conjunction with embodiments. Obviously, the described embodiments are only part of the present invention and are only used to explain the present invention, not to limit the present invention.
[0023] Example 1 This example is to prepare a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte and use it in lithium-ion batteries. The specific steps are as follows: (1) Preparation of lithium-based deep eutectic solvent: In an argon atmosphere with water and oxygen contents both less than 0.01 ppm, trifluoroacetamide and lithium bis(trifluoromethanesulfonyl)imide in a molar ratio of 2:1 were stirred at 50°C, 500 rev / min for 1.5 h, mixed evenly, and cooled to room temperature to obtain a uniform transparent liquid, i.e., a lithium-based deep eutectic solvent; (2) Preparation of deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte: Add 10% by mass of polyvinylidene fluoride-trifluoroethylene organic reinforcement phase into 10 mL of N,N-dimethylformamide, stir evenly, dissolve 10% by mass of lithium-based deep eutectic solvent in the above solution, heat at 50°C for 5 h, pour into a polytetrafluoroethylene mold, and dry at 100°C for 2.5 h to obtain a solid electrolyte film with a thickness of 0.05 mm; (3) Preparation of polymer-based solid-state lithium-ion batteries: Use a punching machine to cut the metal lithium sheet and the lithium iron phosphate positive electrode sheet into round pieces with a diameter of 14 mm respectively; cut the above-mentioned deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte film into an electrolyte membrane with a diameter of 16 mm; use a button battery of model CR2032 to assemble the lithium-ion battery in a glove box in the order of: negative electrode shell, spring, gasket, metal lithium sheet, electrolyte membrane, lithium iron phosphate positive electrode sheet, and positive electrode shell.
[0024] Example 2 This example is to prepare a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte and use it in lithium-ion batteries. The specific steps are as follows: (1) preparing a lithium-based deep eutectic solvent: in an argon atmosphere with water and oxygen contents both lower than 0.01 ppm, stirring lithium bis(trifluoromethanesulfonyl)imide and ethylene glycol at a molar ratio of 1:3 at room temperature for 1 h, mixing them evenly to obtain a uniform and transparent liquid, i.e., a lithium-based deep eutectic solvent; (2) Preparation of deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte: Add 10% by mass of polyvinylidene fluoride-trifluoroethylene organic reinforcement phase into 10 mL of N,N-dimethylformamide, stir evenly, dissolve 15% by mass of lithium-based deep eutectic solvent in the above solution, heat at 50°C for 5 h, pour into a polytetrafluoroethylene mold, and dry at 100°C for 2.5 h to obtain a solid electrolyte film with a thickness of 0.05 mm; (3) Preparation of polymer-based solid-state lithium-ion batteries: Use a punching machine to cut the metal lithium sheet and the lithium iron phosphate positive electrode sheet into round sheets with a diameter of 14 mm respectively; cut the above-mentioned deep eutectic solvent-based polymer solid electrolyte into an electrolyte membrane with a diameter of 16 mm; use a button battery of model CR2032 to assemble the lithium-ion battery in a glove box in the order of: negative electrode shell, spring, gasket, metal lithium sheet, electrolyte membrane, lithium iron phosphate positive electrode sheet, and positive electrode shell.
[0025] Example 3 This example is to prepare a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte and use it in lithium-ion batteries. The specific steps are as follows: (1) preparing a lithium-based deep eutectic solvent: in an argon atmosphere with a water and oxygen content of less than 0.01 ppm, stirring lithium chloride and ethylene glycol at a molar ratio of 1:3 at 60° C. for 3 h, mixing them evenly, and cooling to room temperature to obtain a uniform transparent liquid, thereby obtaining a lithium-based deep eutectic solvent; (2) Preparation of deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte: Add 10% by mass of polyvinylidene fluoride-trifluoroethylene organic reinforcement phase into 10 mL of N,N-dimethylformamide, stir evenly, dissolve 10% by mass of lithium-based deep eutectic solvent in the above solution, heat at 50°C for 5 h, pour into a polytetrafluoroethylene mold, and dry at 100°C for 2.5 h to obtain a solid electrolyte film with a thickness of 0.05 mm; (3) Preparation of polymer-based solid-state lithium-ion batteries: Use a punching machine to cut the metal lithium sheet and the lithium manganese oxide positive electrode sheet into round sheets with a diameter of 14 mm respectively; cut the above-mentioned deep eutectic solvent-based polymer solid electrolyte into an electrolyte membrane with a diameter of 16 mm; use a button battery of model CR2032 to assemble the lithium-ion battery in a glove box in the order of: negative electrode shell, spring, gasket, metal lithium sheet, polymer electrolyte membrane, lithium manganese oxide positive electrode sheet, and positive electrode shell.
Claims
1. A method for preparing a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte, characterized in that: The following steps are involved: (1) Dissolving polyvinylidene fluoride-trifluoroethylene in a solvent at a certain mass ratio, heating and stirring to obtain a uniform and transparent solution; (2) mixing the hydrogen bond donor and the hydrogen bond acceptor in a specific ratio, heating and stirring at a certain temperature to obtain a uniform and transparent lithium-based deep eutectic solvent; (3) adding the lithium-based deep eutectic solvent obtained in step (2) into (1) in different proportions, and continuing to stir to obtain a transparent and uniform solution; (4) pouring the uniform solution obtained in step (3) into a polytetrafluoroethylene mold and placing it in an oven to dry, removing excess solvent, and obtaining a polyvinylidene fluoride-trifluoroethylene-deep eutectic solvent composite solid electrolyte.
2. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: In the step (1), the mass ratio of PVDF-TrFE is 5-10% of the total mass fraction.
3. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: In step (1), the solvent is selected from one of N,N-dimethylformamide (DMF) and N-methylpyrrolidone (NMP); and the amount of the solvent added is 4.5-9.5 mL.
4. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: In step (1), the heating temperature is 40-70°C, the heating time is 3-5 h, and the stirring speed is 200-500 rev / min.
5. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: In step (2), the hydrogen bond donor is selected from at least one of trifluoroacetamide, ethylene glycol, and choline chloride; the hydrogen bond acceptor is at least one of lithium bis(trifluoromethanesulfonyl imide), lithium chloride, and lithium bis(fluorosulfonyl imide); the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:1 to 1:
3. The heating temperature is 40 to 80°C, the heating time is 1 to 4 h, and the stirring speed is 100 to 400 rev / min.
6. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: The mass ratio of polyvinylidene fluoride-trifluoroethylene PVDF-TrFE and deep eutectic solvent in step (3) is 1:(1-3).
7. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: The oven in step (4) is a vacuum oven; the drying temperature is 40°C to 120°C; and the drying time is 1 to 3 hours.
8. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: The deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte is a thin film electrolyte with a film thickness of 0.04~0.1 mm.
9. The method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to claim 1, characterized in that: The solid electrolyte is prepared by the method for preparing the deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte according to any one of claims 1 to 9.
10. A lithium-ion solid-state battery based on a deep eutectic solvent-doped polyvinylidene fluoride-trifluoroethylene solid electrolyte, characterized in that: The composite solid electrolyte comprises the composite solid electrolyte according to claim 10, and one of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and nickel cobalt manganese positive electrodes; and at least one of metallic lithium, graphite, lithium alloy, lithium titanate, and silicon negative electrodes.
Citation Information
Cited By
Gel electrolyte membrane for lithium-sulfur battery, preparation method and energy storage device
CN119650834A
A gel electrolyte membrane for lithium-sulfur batteries, a preparation method and an energy storage device
CN119650834B
Composite solid-state electrolyte membrane, solid-state lithium metal battery and preparation method of solid-state lithium metal battery
CN119786717A
Preparation method of anionic coupling eutectic gel composite electrolyte