Single-component UV curable conformal coating with moisture secondary curing function
By using isocyanate-functional acrylate polyurethane composition, the problem of poor protection effect and high viscosity of conformal coating after aging in high temperature environment is solved, and the improvement of thermal shock resistance at high temperature is achieved and coating effect.
Patent Information
- Application Number
- CN202380032104.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-04
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-15
AI Technical Summary
The existing conformal coating compositions exhibit adverse changes in properties after aging under high temperature environments, resulting in insufficient protection of circuit boards or electronic components, and the high viscosity of the double cured polyurethane resin makes it difficult to contour shapes. Evenly coat, affecting the protection effect.
Isocyanate-functional acrylated polyurethane compositions containing 25-65% by weight of isocyanate-functional acrylated polyurethane, 30-65% by weight of acrylic monomers, 3.5-5.5% by weight of a photoinitiator, 0.1-1% by weight of defoaming agent, 0.5-1.5% by weight of dehydrating agent, 0.2-1.5% by weight of wetting agent and 0.5-2.5% by weight of coupling agent can maintain improved characteristics at 130°C and reduce Glass transition temperature and internal stress improve elasticity and heat shock resistance.
The composition maintains improved heat shock resistance and elasticity at high temperatures, ensuring the protection effect of the circuit board, while providing better protection performance due to the low viscosity characteristics.
Smart Images

Figure CN118974126A_ABST
Abstract
Description
[0001] The present invention relates to conformal coating compositions, methods for conformally coating substrates using the compositions, and substrates coated with the compositions.
[0002] Conformal coating materials are thin polymer films that conform to the contours of a printed circuit board to protect the board's components. Typically applied at a thickness of 25 μm to 250 μm, they are applied to electronic circuits to protect from moisture, dust, chemicals and extreme temperatures.
[0003] Coatings can be applied in a variety of ways, including brushing, spraying, dispensing, and dipping. In addition, many materials can be used as conformal coatings, such as acrylics, silicones, polyurethanes, and parylene. Polyurethane coatings are a popular choice for conformal coatings due to their high chemical resistance, flexibility, and hardness.
[0004] Coatings that can be cured by actinic radiation (e.g., "UV coatings") can be used as conformal coatings because such coatings can be cured relatively quickly by exposure to a radiation source (usually UV, including traditional UV (arc and microwave types) and UV-LED light sources). Rapid curing allows manufacturers to increase production. However, because circuit boards and other electronic components have highly contoured surfaces, such UV coatings suffer from the following phenomenon when used as conformal coatings: areas of the coating that cannot be easily exposed to UV light due to the contours (i.e., "shadow" areas) remain uncured.
[0005] US 4,424,252 describes the problem of "shadow cure" and solves this problem using dual cure resins. Such resins cure by two mechanisms: a) exposure to UV light; and b) curing by atmospheric moisture. Atmospheric moisture reacts with free isocyanate groups in the dual cure resin to form amine groups. The amine groups react with other isocyanate groups to form polyureas. Curing by atmospheric moisture allows areas of the coating that are in the "shadow" to cure completely.
[0006] However, dual cure polyurethane resins have disadvantages due to their relatively high viscosity. This problem is particularly relevant for conformal coatings due to the contoured shape of the substrate. From a flowability point of view, low viscosity resins are more advantageous, i.e., low viscosity resins flow more easily around the contours of the circuit board and can coat such circuit boards more evenly.
[0007] Previous attempts to reduce the viscosity of dual cure polyurethane resins have involved adding significant amounts of reactive diluents to the dual cure polyurethane resins. While the addition of reactive diluents acts to reduce the viscosity of the resin, it also reduces the weight % of free isocyanate groups in the resin. This in turn has the effect of reducing the effectiveness of the moisture cure mechanism, particularly in shadowed areas, which results in coatings having insufficient hardness and / or solvent resistance in such areas.
[0008] US 9,932,492 describes a one-component, dual-cure conformal coating composition containing an isocyanate-functional polyurethane acrylate and a polyisocyanate containing allophanate and / or uretdione groups. The composition is described as providing a coating having high hardness and solvent resistance. Conformal coating compositions are also disclosed in US2014 / 199491A1, CN109321125A, CN111548726A, and CN111471337A.
[0009] To date, conventional conformal coating compositions have exhibited adverse changes in their properties after aging at elevated temperatures. This can result in the conformal coating providing inadequate protection to circuit boards or electronic components due to stress cracking when used in high temperature environments.
[0010] The present invention seeks to solve at least some of the problems associated with the prior art or at least provide a commercially acceptable alternative solution to the prior art. In addition, the present invention discloses the construction / manufacture of new assemblies, devices and components using the disclosed materials and processes.
[0011] In a first aspect, the present invention provides a UV and moisture curable conformal coating composition comprising:
[0012] 25 to 65 wt % of an isocyanate functional acrylated polyurethane;
[0013] 30 to 65 wt % of acrylic monomers;
[0014] 3.5 to 5.5 wt % photoinitiator;
[0015] 0.1 to 1 wt % of a defoaming agent;
[0016] 0.5 to 1.5 wt % of a dehydrating agent;
[0017] 0.2 wt % to 1.5 wt % of a wetting agent; and
[0018] 0.5 wt% to 2.5 wt% coupling agent.
[0019] Each aspect or embodiment as defined herein may be combined with any other aspect or embodiment unless clearly indicated to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature indicated as being preferred or advantageous.
[0020] The present inventors have surprisingly found that the compositions of the present invention exhibit improved retention of properties during heat aging testing at 130°C compared to conventional conformal coating compositions. Advantageously, this can result in improved thermal shock resistance compared to the prior art. Without being bound by theory, it is believed that this is due to the combination of the amounts of acrylated polyurethane, acrylic monomer, and photoinitiator.
[0021] The composition may result in a glass transition temperature (T g ) and advantageously high elasticity (low modulus) conformal coating formation. This can be particularly useful for protecting circuit boards during use. Without being bound by theory, it is believed that this is due to the combination of the amounts of acrylated polyurethane and acrylic monomers.
[0022] Advantageously, the compositions of the present invention may undergo a slower and more controlled polymerization process during UV curing compared to conventional conformal coating compositions. This may result in a reduction in internal stress levels and thus improve the ability to withstand stress fractures during thermal shock excursions. However, curing may still be fast enough to be used in conventional conformal coating production processes and assembly lines. Without being bound by theory, it is believed that this is due to the combination of the amounts of acrylated polyurethane, acrylic monomer, and photoinitiator.
[0023] As used herein, the term "conformal coating composition" may encompass compositions used to form a conformal coating, for example, on a circuit board.
[0024] The composition comprises an isocyanate-functional acrylated polyurethane (an acrylated polyurethane comprising isocyanate functional groups). As used herein, the term "polyurethane" may encompass a class of polymers consisting of organic units connected by carbamate (urethane) bonds. As used herein, the term "acrylated polyurethane" may encompass polyurethanes comprising acrylate functional groups in addition to free isocyanate functional groups. Acrylate functional groups may also include methacrylate functional groups. The isocyanate-functional acrylated polyurethane is preferably in the form of an oligomer.
[0025] The composition is both UV curable and moisture curable. The composition contains a second moisture curing functionality to ensure curing in areas that are shielded from exposure to actinic radiation. When exposed to actinic radiation (usually UV), the photoinitiator can cause a reaction between the acrylate functional groups on the acrylated polyurethane and the acrylic monomer. When exposed to moisture (usually moisture contained in the air), the isocyanate functional groups can form amine groups, which in turn can react with other isocyanate groups to form polyureas.
[0026] The composition comprises 0.1 wt % to 1.0 wt % of an antifoaming agent. The presence of the antifoaming agent in the amount described can inhibit the generation of bubbles during storage and / or use.
[0027] The composition comprises 0.5 wt % to 1.5 wt % of a dehydrating agent. The presence of the dehydrating agent in the amount described above can inhibit the composition from undesired moisture curing during storage.
[0028] The composition comprises 0.2 wt % to 1.5 wt % of a wetting agent. The presence of the wetting agent in the amount described can improve the ability of the composition to "wet" a substrate (e.g., a circuit board) to which the composition is applied. In particular, the composition can "wet" all parts of a circuit board.
[0029] The composition comprises 0.5 wt % to 2.5 wt % of a coupling agent. The presence of the coupling agent in such an amount can improve the adhesion of the final conformal coating to the substrate to which it is applied.
[0030] The composition is preferably a "one-component" composition.
[0031] The composition preferably comprises 30 to 50 wt % of isocyanate functional acrylated polyurethane, more preferably 35 to 45 wt % of isocyanate functional acrylated polyurethane. The presence of isocyanate functional acrylated polyurethane in such amounts can lead to further improvements in the properties of retention of properties during heat aging, advantageously low glass transition temperature, advantageously high elasticity, and a slower and more controlled polymerization process during UV curing.
[0032] The isocyanate functional acrylated polyurethane is preferably thermoplastic. The isocyanate functional acrylated polyurethane is preferably an elastomer. The isocyanate functional acrylated polyurethane is preferably an isocyanate functional acrylated thermoplastic polyurethane elastomer. This can result in a particularly advantageous low glass transition temperature and / or high elasticity of the conformal coating formed from the composition.
[0033] The isocyanate functional acrylated polyurethane preferably has a ratio of acrylate functional groups to isocyanate functional groups of 2: 1 to 1: 2. Such a ratio can result in a particularly favorable amount of crosslinking during the curing process, i.e., not too little to result in inadequate curing, nor too much to result in a hard, inflexible coating.
[0034] The isocyanate functional acrylated polyurethane is preferably the reaction product of reactants comprising:
[0035] at least one polyol, preferably an amorphous hydrophobic polyol;
[0036] at least one diisocyanate, preferably a branched diisocyanate; and
[0037] At least one hydroxyalkyl acrylate.
[0038] Typically, a diisocyanate is reacted with a polyol to give an isocyanate terminated "prepolymer" which is then further reacted with a hydroxyalkyl acrylate in a second stage to form an isocyanate functional acrylated polyurethane.
[0039] The polyol (preferably an amorphous hydrophobic polyol) preferably comprises:
[0040] One or more of hydroxyl-terminated polybutadiene, hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated polyisoprene, hydroxyl-terminated polyolefin, hydroxyl-terminated polyfarnesene, hydroxyl-terminated hydrogenated polyfarnesene, castor oil, hydrogenated castor oil and dimer acid-based polyester polyol (preferably C36), more preferably one or more of hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated hydrogenated polyfarnesene, hydrogenated castor oil and dimer acid-based polyester polyol; and / or
[0041] The diol is selected from 2-ethyl-1,3-hexanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, isosorbide, C 18 One or more of dimer glycol, 2-butyl-2-ethyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol and 2,2-diethyl-1,3-propanediol, preferably 2-ethyl-1,3-hexanediol, C 18 One or more of dimer glycol and 2-butyl-2-ethyl-1,3-propanediol; and / or
[0042] The triol is selected from one or more of trimethylolpropane, triethanolamine, diethanolamine, 1,2,6-hexanetriol, phloroglucinol (1,3,5-trihydroxybenzene) and glycerol, more preferably 1,2,6-hexanetriol.
[0043] In contrast, prior art isocyanate-functional acrylated polyurethanes are typically formed from polyether polyols, polyester polyols, polycaprolactone polyols, polycarbonate polyols, and polylactone polyols. It has been demonstrated in the past that polyether and polyester polyols give poor results when formulated into conformal coatings because their electrical properties, particularly surface insulation resistance (SIR), are poor in high temperature / high humidity (“harsh”) environments (e.g., 85% RH, 85°C, conditions typically used to test conformal coatings for automotive applications). Polyurethane acrylate oligomers based on polyether and polyester polyols are susceptible to degradation under these automotive test conditions, primarily through oxidation and hydrolysis. In addition, their low temperature performance is generally unacceptable for use in conformal coatings. Conformal coatings for automotive and aerospace applications need to remain flexible at temperatures as low as -60°C. For the automotive industry, -40°C is an acceptable standard test temperature for evaluating low temperature performance. Current conformal coatings using polyurethane acrylate oligomers based on polyester polyols do not easily retain their mechanical properties (elongation (flexibility), tensile strength, modulus) at subambient temperatures, especially when they have been aged at elevated temperatures. Relatively low initial elongation values of about 50% (samples aged and tested at ambient temperature) are reduced to unacceptable levels when thermally aged / tested at subambient temperatures. As observed by the inventors of the present application, elongation values of less than 50% generally translate into early failure of the conformal coating when subjected to thermal shock testing. When the flexibility of the conformal coating is lost, extensive fracture of the coating is evident, typically after only a few hundred cycles.
[0044] The glass transition temperature of the final conformal coating is also very important. Glass transition temperatures significantly above -40°C can also lead to stress fractures during thermal shock testing. The isocyanate-functional acrylated polyurethanes of the present application formed from the polyols listed above can exhibit properties superior to commercially available polyurethane acrylate oligomers (recommended for and / or used in current radiation-curable conformal coatings) due to their unique composition and low glass transition temperature. In particular, compositions containing isocyanate-functional acrylated polyurethanes formed from the polyols listed above can exhibit particularly excellent flexibility and low temperature properties, as well as improved SIR performance. The composition can still be cured by the primary curing mechanism (UV / UV-LED photopolymerization of acrylate groups) in the "sight" area of the circuit board, and cured by the secondary curing mechanism (isocyanate-moisture reaction) in the "shadow area" of the circuit board.
[0045] The polyol preferably has 500 gmol -1 Up to 3000 gmol -1 , more preferably 1000 gmol -1 Up to 2000 gmol -1, even more preferably about 2000 gmol -1 The number average molar mass.
[0046] The polyols preferably have a functionality of 1.9 to 2.5 and / or a hydroxyl number of 50 to 250 mg KOH / g.
[0047] The diisocyanates preferably include 1,3-bis(1-isocyanato-1-methylethyl)benzene (TMXDI, tetramethylxylene diisocyanate), 5-isocyanato-1-(isocyanatomethyl)-1,3,3-trimethylcyclohexane (IPDI, isophorone diisocyanate), 1,6-diisocyanato-2,2,4(2,4,4)-trimethylhexane (TMDI, trimethylhexamethylene diisocyanate), 1,6-diisocyanatohexane (HDI, hexamethylene diisocyanate), 4,4'-diisocyanatodicyclohexylmethane (HDI, hexamethylene diisocyanate), 1,6-diisocyanatohexane ... 12 MDI) and 1,5-diisocyanatopentane (PDI, 1,5-pentamethylene diisocyanate), preferably one or more of 1,6-diisocyanato-2,2,4(2,4,4)-trimethylhexane (TMDI, trimethylhexamethylene diisocyanate). This can result in a cured composition exhibiting particularly excellent flexibility and low temperature properties, as well as improved SIR. Prior art isocyanate functional acrylated polyurethanes are typically formed from aromatic diisocyanates (e.g. TDI, toluene diisocyanate). This exacerbates the problem of poor tensile property retention / poor thermal shock (also due to the type of polyols in the prior art) because the aromatic character of the resulting polymers means that they are more susceptible to oxidative decomposition during aging at elevated temperature / humidity.
[0048] The hydroxyalkyl acrylate preferably includes one or more of 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate and 4-hydroxybutyl methacrylate, more preferably 4-hydroxybutyl acrylate. Such hydroxyalkyl acrylates have longer carbon chains than the hydroxyalkyl acrylates of conventional isocyanate-functional acrylated polyurethanes used to form conformal coatings. This can result in the cured composition exhibiting particularly excellent flexibility and low temperature performance, as well as improved SIR.
[0049] In particularly preferred embodiments, the isocyanate functional acrylated polyurethane is the reaction product of reactants comprising:
[0050] Hydroxyl terminated hydrogenated polybutadiene, hydroxy terminated hydrogenated polyfarnesene, hydrogenated castor oil, polyester polyol based on dimer acid, 2-ethyl-1,3-hexanediol, C 18 One or more of dimer diol and 1,2,6-hexanetriol;
[0051] 1,6-diisocyanato-2,2,4(2,4,4)-trimethylhexane (TMDI, trimethylhexamethylene diisocyanate); and
[0052] 4-Hydroxybutyl acrylate.
[0053] In order to form an isocyanate-functional acrylated polyurethane from the reaction product of the above-mentioned substances, a catalyst is preferably used to increase the speed and / or selectivity of the reaction or to reduce the temperature that may be required. Suitable catalysts are known in the art, such as metal complexes and tertiary amines. Among metal-based catalysts, organotin compounds (such as DBTL, DOTL, tin carboxylates) are very commonly used in the synthesis of polyurethanes. They provide very good performance, but have unfavorable toxicity characteristics. Other metal catalysts have been developed that show similar performance / reactivity to tin-based materials while being more user- and environmentally friendly. Notable examples are compounds of zirconium, zinc, and bismuth. Preferred catalysts include bismuth carboxylates to catalyze the reaction of isocyanates with hydroxyl-containing reagents. Commercial examples of such catalysts include K-Kat XC-B221, K-Kat XK651, and K-Kat 6212 from King Industries; and Tibkat 716 and Tibkat 720 from Tib Chemicals.
[0054] The composition preferably comprises 45 to 60 wt % of acrylic monomers, more preferably 50 to 60 wt % of acrylic monomers. The presence of acrylic monomers in such amounts can lead to further improvements in the properties of retention during heat aging, advantageously low glass transition temperature, advantageously high elasticity, and a slower and more controlled polymerization process during UV curing. Acrylic monomers can be considered as reactive diluents.
[0055] The acrylic monomer preferably comprises a linear alkyl acrylate containing 4 to 12 carbon atoms, more preferably 6 to 12 carbon atoms, even more preferably 8 to 10 carbon atoms. Preferably, the linear alkyl acrylate comprises octadecyl acrylate.
[0056] In addition to the linear alkyl acrylate, the acrylic monomer may also preferably include a diacrylate, more preferably a diacrylate selected from one or both of 1,6-hexanediol diacrylate and 3-methyl-1,5-pentanediol diacrylate. Such materials are particularly effective reactive diluents in combination with other components of the composition.
[0057] Acrylic monomers may also include cyclic acrylates, more preferably tetrahydrofurfuryl acrylate, cyclic trimethylolpropane formal acrylate, tert-butyl cyclohexanol acrylate, 3,3,5-trimethylcyclohexyl acrylate, isobornyl acrylate, and 2-phenoxyethyl acrylate, even more preferably tetrahydrofurfuryl acrylate. Such materials are particularly effective reactive diluents in combination with the other components of the composition.
[0058] The photoinitiator preferably comprises:
[0059] α-hydroxyketone based photoinitiators; and / or
[0060] Phenylphosphine oxide based photoinitiators; and / or
[0061] Ethyl benzoylformate type photoinitiator.
[0062] More preferably, the photoinitiator comprises:
[0063] α-Hydroxyketone based photoinitiators;
[0064] phenylphosphine oxide based photoinitiators; and
[0065] Ethyl benzoylformate type photoinitiator.
[0066] Combinations of such photoinitiators can result in a particularly controlled polymerization process during UV curing. Photoinitiators based on α-hydroxyketones can result in surface curing of the composition. Commercial examples of suitable α-hydroxyketone-based photoinitiators include Darocur TM / Irgacure 1173 TM and Double cure TM 173. Phenylphosphine oxide based photoinitiators can result in full cure / deep cure of the composition. Commercial examples of suitable phenylphosphine oxide based photoinitiators include Irgacure TM 819 and Doublecure TM 1819. Methyl benzoylformate-type photoinitiators can be particularly effective in varying the extent of cure to minimize internal stresses during cure and to prevent yellowing and excessive odor after cure. A commercial example of a methyl benzoylformate-type photoinitiator is Doublecure TM 200.
[0067] The α-hydroxyketone based photoinitiator preferably includes 2-hydroxy-2-methyl-1-phenyl-1-propanone. Such photoinitiators are particularly effective in causing surface curing of the composition.
[0068] The phenylphosphine oxide based photoinitiator preferably includes phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, ethyl(2,4,6-trimethylbenzoyl)phenylphosphonate and / or diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide. Such photoinitiators are particularly effective in causing full cure / deep cure of the composition.
[0069] Ethyl benzoylformate type photoinitiators preferably include methyl benzoylformate.Such photoinitiators can be particularly effective in modifying the cure rate to minimize internal stress during cure and prevent yellowing and excessive odor after cure.
[0070] The photoinitiator preferably comprises: a thioxanthone-type initiator, preferably comprising 2-isopropylthioxanthone; and a tertiary amine synergist, preferably comprising ethyl 4-(dimethylamino)benzoate. The photoinitiator and synergist combination can be particularly effective in causing a good balance of surface and full (depth) curing of the composition. Commercial examples of thioxanthone-type photoinitiators and synergists are Ominrad TM ITX, Speedcure TM ITX and Omnirad TM EDB.
[0071] The composition preferably comprises 3.8 to 5.2 wt% photoinitiator, more preferably 4 to 4.5 wt% photoinitiator.
[0072] The defoamer preferably comprises a polyether siloxane.Polyether siloxanes are particularly effective defoamers when used in conjunction with the other components of the composition.
[0073] The composition preferably comprises 0.2 to 0.8 wt% of an antifoaming agent, more preferably 0.3 to 0.7 wt% of an antifoaming agent.
[0074] The dehydrating agent preferably comprises p-toluenesulfonyl isocyanate.P-toluenesulfonyl isocyanate is a particularly effective dehydrating agent when used in combination with the other components of the composition.
[0075] The composition preferably comprises 0.7 to 1.3 wt% of the dehydrating agent, more preferably 0.8 to 1.2 wt% of the dehydrating agent.
[0076] The wetting agent preferably comprises poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-graft-poly(ethylene glycol) methyl ether. Poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-graft-poly(ethylene glycol) methyl ether is a particularly effective wetting agent when used in conjunction with the other components of the composition.
[0077] The composition preferably comprises 0.5 wt% to 1.3 wt% wetting agent, more preferably 0.8 wt% to 1.2 wt% wetting agent.
[0078] The coupling agent preferably comprises an acrylate functional silane and / or a (meth)acrylate functional silane. Such silanes are particularly effective coupling agents when used in conjunction with the other components of the composition.
[0079] The composition preferably comprises 1 to 2 wt% coupling agent, more preferably 1.0 to 1.5 wt% coupling agent.
[0080] Traditionally, lower viscosity conformal coating compositions have been thought to flow better over the surface of a PCB than higher viscosity alternatives. However, reducing the viscosity of a conformal coating composition can promote excessive flow under the component, which can make a complete secondary cure difficult.
[0081] However, the present inventors have discovered that modification of the rheological properties of the conformal coating composition, rather than just a change in viscosity, is highly beneficial. The conformal coating compositions described herein preferably contain a rheology modifier.
[0082] The rheology modifier preferably comprises a polyamide wax, preferably in the form of crystalline fibers (polyamide wax containing crystalline fibers). Advantageously, the use of polyamide wax can enable the composition to be applied to the PCB by selective spraying. This is because polyamide wax can introduce thixotropy into the system. Thixotropy is a shear-thinning property that imparts low viscosity at high shear rates and high viscosity at low shear rates. Selective spraying is a high shear process, which means that the coating is applied to the PCB with a low viscosity, thereby allowing good flow and complete fit to the PCB surface. After application, where low shear conditions prevail, the coating viscosity can undergo a time-dependent recovery to the initial high viscosity system. This minimizes excess flow (splashing, overspray) under the components and at the edges of the board, i.e. controlled flow. This feature can also ensure complete edge coverage of the components of the PCB. This is a problem that poses a problem for many conventional conformal coatings. The use of low-viscosity coating compositions generally cannot fully and well coat the sharp edges of the components / component legs, resulting in PCB failure due to these thin and fragile areas in the conformal coating. The conformal coating composition of the present invention is intended to solve this problem. Without being bound by theory, it is believed that the crystalline fibers of the polyamide wax form an interactive network within the conformal coating composition. This network can be broken down under high shear conditions, but once these shear forces are removed, it quickly reestablishes itself, returning to its original state. In this regard, the composition preferably exhibits a thixotropic index of 1.5 to 3.5. This can be achieved by using polyamide wax.
[0083] The composition preferably also comprises a UV tracer. This may cause the composition to advantageously emit blue light under a black light.
[0084] The UV tracer preferably comprises 2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole). 2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole) is a particularly effective UV tracer in combination with the other components of the composition.
[0085] The composition preferably comprises 0.1 wt% to 0.5 wt% UV tracer, more preferably 0.2 wt% to 0.4 wt% UV tracer.
[0086] The composition preferably comprises an odour masking agent. This may make the composition more pleasant to use.
[0087] The odor masking agent preferably comprises one or both, preferably both, of dimethyl-7-octen-2-ol and p-tert-butylcyclohexyl acetate. Such materials are particularly effective odor masking agents in combination with other components of the composition.
[0088] In another aspect, the present invention provides a method for conformally coating a substrate, the method comprising:
[0089] Providing a substrate,
[0090] Providing the compositions described herein;
[0091] depositing the composition on at least a portion of the substrate; and
[0092] The coated substrate is exposed to actinic radiation.
[0093] The advantages and preferred features of the first aspect also apply to this aspect.
[0094] Depositing the composition onto at least a portion of the substrate may include one or more of brushing, spraying, dispensing, and dipping.
[0095] The actinic radiation preferably comprises UV, such as a UV-LED.
[0096] The substrate preferably comprises a circuit board or an electronic component.
[0097] In another aspect, the present invention provides a substrate coated with a composition as described herein. The advantages and preferred features of the first aspect also apply to this aspect.
[0098] In another aspect, the present invention provides a UV and moisture curable conformal coating composition comprising an isocyanate functional acrylated polyurethane which is the reaction product of reactants comprising:
[0099] polyol, preferably an amorphous polyol;
[0100] A diisocyanate, preferably a branched diisocyanate; and
[0101] Hydroxyalkyl acrylate.
[0102] The advantages and preferred features of the first aspect also apply to this aspect.
[0103] In another aspect, the present invention provides a UV and moisture curable conformal coating composition comprising:
[0104] 25 to 65 wt % of an isocyanate functional acrylated polyurethane;
[0105] 30 to 65 wt % of acrylic monomers;
[0106] and optionally one or more of the following:
[0107] 3.5 to 5.5 wt % photoinitiator;
[0108] 0.1 to 1 wt % of a defoaming agent;
[0109] 0.5 to 1.5 wt % of a dehydrating agent;
[0110] 0.2 wt % to 1.5 wt % of a wetting agent;
[0111] 0.5 wt % to 2.5 wt % of a coupling agent; and
[0112] 0.1 wt% to 2.5 wt% rheology modifier.
[0113] The advantages and preferred features of the first aspect also apply to this aspect.
[0114] The present invention will now be further described with reference to the following numbered clauses:
[0115] 1. A UV and moisture curable conformal coating composition comprising:
[0116] 52 to 75 weight percent of an isocyanate functional acrylated polyurethane;
[0117] 20 to 43 wt% acrylic monomers;
[0118] 3.5 to 5.5 wt % photoinitiator;
[0119] 0.5 to 1 wt % of a defoaming agent;
[0120] 0.2 wt % to 0.5 wt % of a dehydrating agent;
[0121] 0.3 wt % to 0.5 wt % of a wetting agent; and
[0122] 0.1 wt% to 0.3 wt% coupling agent.
[0123] 2. The composition according to clause 1, comprising 55 to 70 wt% of the isocyanate functional acrylated polyurethane, preferably 57 to 65 wt% of the isocyanate functional acrylated polyurethane.
[0124] 3. The composition according to clause 1 or clause 2, wherein the isocyanate functional acrylated polyurethane is thermoplastic.
[0125] 4. A composition according to any preceding clause, wherein the isocyanate functional acrylated polyurethane is an elastomer.
[0126] 5. A composition according to any preceding clause, comprising 25 to 41 wt% acrylic monomer, preferably 30 to 40 wt% acrylic monomer.
[0127] 6. A composition according to any preceding clause, wherein the photoinitiator comprises:
[0128] α-hydroxyketone based photoinitiators; and / or
[0129] Phenylphosphine oxide based photoinitiators; and / or
[0130] Ethyl benzoylformate type photoinitiator.
[0131] 7. A composition according to any preceding clause, wherein the photoinitiator comprises:
[0132] α-Hydroxyketone based photoinitiators;
[0133] phenylphosphine oxide based photoinitiators; and
[0134] Ethyl benzoylformate type photoinitiator.
[0135] 8. The composition according to clause 6 or clause 7, wherein the α-hydroxyketone based photoinitiator comprises 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0136] 9. The composition according to any one of clauses 6 to 8, wherein the phenylphosphine oxide-based photoinitiator comprises phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.
[0137] 10. The composition according to any one of clauses 6 to 9, wherein the ethyl benzoylformate-type photoinitiator comprises methyl benzoylformate.
[0138] 11. A composition according to any preceding clause, wherein the defoaming agent comprises a polyether-modified siloxane.
[0139] 12. A composition according to any preceding clause, wherein the dehydrating agent comprises p-toluenesulfonyl isocyanate.
[0140] 13. A composition according to any preceding clause, wherein the wetting agent comprises poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-graft-poly(ethylene glycol) methyl ether.
[0141] 14. A composition according to any preceding clause, wherein the coupling agent comprises an acrylate functional silane.
[0142] 15. A composition according to any preceding clause, further comprising a reactive diluent.
[0143] 16. The composition according to clause 15, wherein the reactive diluent comprises one or both, preferably both, of 3,3,5-trimethylcyclohexyl acrylate and tricyclodecane dimethanol diacrylate.
[0144] 17. A composition according to any preceding clause, further comprising a UV tracer.
[0145] 18. The composition according to clause 17, wherein the UV tracer comprises 2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole.
[0146] 19. A composition according to any preceding clause, further comprising an odour masking agent.
[0147] 20. The composition according to clause 19, wherein the odor masking agent comprises one or both, preferably both, of dimethyl-7-octen-2-ol and p-tert-butylcyclohexyl acetate.
[0148] 21. A method for conformally coating a substrate, the method comprising:
[0149] Providing a substrate,
[0150] Providing a composition according to any of the preceding clauses;
[0151] depositing the composition on at least a portion of the substrate; and
[0152] The coated substrate is exposed to actinic radiation.
[0153] 22. The method according to clause 21, wherein the substrate comprises a circuit board or an electronic component.
[0154] 23. A substrate coated with a composition according to any one of clauses 1 to 20.
[0155] The advantages and preferred features of the aforementioned aspects also apply to the subject matter of these clauses. Example
[0156] The present invention will now be further described with reference to the following examples:
[0157] General Synthesis of Isocyanate Functional Acrylated Polyurethane Oligomers:
[0158] In the first stage, a diisocyanate is reacted with a polyol (and / or diol / triol) at elevated temperature, under nitrogen, using a catalyst to produce an isocyanate-terminated "prepolymer". This prepolymer is further reacted with a hydroxyalkyl acrylate under air in the second stage to form an isocyanate-functional polyurethane acrylate oligomer. The elevated temperature and catalyst are used to reduce the overall reaction time, the temperature required for the reaction, and / or to improve the reaction selectivity between the isocyanate groups in the diisocyanate and the hydroxyl groups of the other reactants.
[0159] An exemplary reaction scheme is as follows:
[0160]
[0161] The above reaction scheme shows steps 1 and 2 and an idealized structure of the product - an isocyanate functional urethane acrylate oligomer.
[0162] In the reaction scheme (step 2, acrylation), the R3 group of the hydroxyalkyl acrylate can be as follows...
[0163] -CH2CH2- for 2-hydroxyethyl acrylate
[0164] -CH2CH2CH2- for 3-hydroxypropyl acrylate
[0165] -CH2CH2CH2CH2- for 4-hydroxybutyl acrylate
[0166] In the reaction scheme (step 1), representative structures of the reagents used are as follows:
[0167] Polyols / Diols :
[0168] Polyester polyols based on C36 dimer acid :
[0169]
[0170] Hydrogenated polybutadiene :
[0171]
[0172] C36 Dimer Diol :
[0173]
[0174] Isocyanate :
[0175] TMDI
[0176]
[0177] Oligomer Synthesis - Sample 1 :
[0178] 2,2,4(2,4,4)-trimethylhexamethylene diisocyanate (0.21 mol, 44.10 g) and bismuth carboxylate catalyst (0.1 wt % of the total batch) were added to a round bottom reaction flask equipped with a thermometer, stirrer and nitrogen line. Nitrogen was introduced into the flask as an initial purge, and then maintained at a constant flow rate of about 1 ml / min to maintain an inert atmosphere. A molar mass of 2000 gmol -1 C-based 36 The polyester polyol (0.1 mole, 200g) of dimer acid is added to the flask. The reaction is carried out at 80°C for 2 hours to form an isocyanate-terminated prepolymer. The endpoint of the reaction is when the theoretical % isocyanate is reached (according to ISO 14896, measured by reverse titration with di-n-butylamine), and the FTIR spectrum shows the characteristic bands for the isocyanate-terminated polyurethane prepolymer, and there is no band associated with hydroxyl. Once this stage is completed, the nitrogen pipeline is replaced with a dry air pipeline. Similarly, a constant flow of about 1ml / min is applied after the initial purge to maintain an oxygen-rich atmosphere. The temperature is reduced to 50°C from 80°C, and then 100ppm polymerization inhibitors, such as phenothiazine, MEHQ, etc. are added to the flask (to prevent the self-polymerization of acrylate groups). Once it is completely dissolved / dispersed in the isocyanate-terminated polyurethane prepolymer, 4-hydroxybutyl acrylate (0.11 mole, 15.86g) is added to the flask. The reaction was carried out at 50°C to 60°C for one hour. Again, the endpoint of the reaction was when the theoretical % isocyanate was reached, and the FTIR spectrum showed characteristic bands for isocyanate-terminated polyurethane prepolymers; this time, plus the presence of bands associated with acrylate groups. A viscous (625,000 mPa.s at 20°C), colorless isocyanate-functional polyurethane acrylate oligomer was obtained in high yield (>95%). The final isocyanate content was 1.78%, and the acrylate:isocyanate ratio was 1:1.
[0179] Oligomer Synthesis - Sample 2 :
[0180] The polyurethane acrylate oligomer was prepared using the same method as described in Example 1. 2,2,4(2,4,4)-trimethylhexamethylene diisocyanate (1.356 moles, 284.76 g) and bismuth carboxylate catalyst (0.1 wt % of the total batch) were mixed with a mass of about 540 gmol -1 C-based 36 The polyol of dimer acid (0.645 mol, 349.59 g) was reacted to form an isocyanate terminated prepolymer. 4-Hydroxybutyl acrylate (0.71 mol, 102.41 g) was then added to the flask and reacted to form a polyurethane acrylate oligomer. A viscous (103,000 mPa.s at 20°C), straw-colored, isocyanate functional polyurethane acrylate oligomer was obtained in high yield (>95%). The final isocyanate content was 4.31% and the acrylate:isocyanate ratio was 1:1.
[0181] Oligomer Synthesis - Sample 3 :
[0182] The polyurethane acrylate oligomer was prepared using the same method as described in Example 1. 2,2,4(2,4,4)-trimethylhexamethylene diisocyanate (0.21 mole, 44.10 g) and bismuth carboxylate catalyst (0.01 wt % of the total batch) were mixed with a molar mass of about 2000 gmol -1 Hydrogenated polybutadiene polyol (0.1 mol, 200 g) was reacted to form an isocyanate terminated prepolymer. 2-Hydroxyethyl acrylate (0.11 mol, 12.77 g) was then added to the flask and reacted to form a polyurethane acrylate oligomer. A viscous (750,000 mPa.s at 20° C.), straw-colored, isocyanate functional polyurethane acrylate oligomer was obtained in high yield (>95%). The final isocyanate content was 1.73% and the acrylate:isocyanate ratio was 1:1.
[0183] Testing of Isocyanate Functional Acrylated Polyurethane Oligomers:
[0184] Improved surface insulation resistance (SIR)
[0185] This is a critical property of conformal coatings and is routinely evaluated under harsh conditions to examine (a) initial SIR values, (b) any trends in SIR values over time, and (c) any evidence of corrosion on the PCB, etc. A downward trend indicates degradation of the conformal coating, leading to premature failure of the PCB via corrosion, dendrite formation, tin whiskers, etc.
[0186] Laboratory testing of oligomer samples 1-3 showed that SIR values higher than commercially available oligomers (by an order of magnitude) could be achieved. The SIR test results for sample 1 and two commercially available oligomers are shown in Figure 1 Commercial Example 1 is an isocyanate aliphatic functional urethane acrylate. Commercial Example 2 is an oligomer with UV, isocyanate, and siloxane functionalities. As can be seen, Sample 1 achieves an average SIR value of 9.31 with a stable linear response during the test, indicating that the coating performed well and did not show any signs of degradation. The two commercial oligomers returned lower average SIR values of 8.42 and 7.98 for Commercial Example 1 and Commercial Example 2, respectively. In addition, the response of these oligomers was not stable, showing a clear downward trend. The stable response of Sample 1 at 85% relative humidity and 85°C is excellent. The minimum SIR value accepted for automotive applications is 8 Log 10 , Sample 1 exceeds this value by some margin. Conversely, the two commercial oligomers perform poorly in this test and, based on the downward trend over time, will not meet this standard over an extended testing period.
[0187] Improved retention of tensile properties
[0188] The tensile properties of Samples 1-3 oligomers and commercial examples were measured initially (after primary and secondary cure) and after aging at 130°C. Testing was performed at ambient temperature and at -40°C. Sample 1 initially showed higher elongation and lower modulus values and maintained these initial properties to a higher degree after aging. The elongation and modulus values are shown in Figure 2 and Figure 3 In terms of elongation, samples 1, 2, and 3 showed higher levels of elasticity / flexibility than the two commercial materials when initially tested. They maintained their elasticity after heat aging and when tested below ambient temperature. When these two conditions were combined, samples 1-3 performed exceptionally well.
[0189] The oligomer of Commercial Example 2, despite having a lower initial elongation value, did tend to be better in terms of retention of this elongation upon heat aging. However, the combination of heat aging and testing below ambient did return poor results, with the elongation dropping by about 50%. The oligomer of Commercial Example 1 performed far worse than Samples 1-3 in terms of elastic retention. The initial elongation value of about 50% dropped 10-fold (to about 5%) after heat aging and testing at below ambient temperatures. The test sample broke almost immediately upon initiation of testing.
[0190] When tested at subambient temperatures, Commercial Examples 1 and 2 appear to exhibit primarily plastic deformation, with no discernible recovery (return to original sample dimensions) when returned to room temperature. Samples 1-3 exhibit significant elastic deformation and rapid recovery (samples return to original dimensions in less than a minute at room temperature).
[0191] In terms of modulus (a measure of the "stiffness" of a sample), the higher the modulus, the stiffer and less elastic the material. All of the oligomers tested had very low moduli to begin with, indicating soft, elastic materials. After aging, samples 1-3 did show a modest increase in modulus values of an order of magnitude, from 0.5 MPa-1.0 MPa to 15 MPa-45 MPa, but as mentioned above, this did not appear to significantly affect elasticity / recovery.
[0192] However, both commercial materials showed a significant increase in modulus when tested below ambient temperature, an increase that was exacerbated when aged at elevated temperatures prior to testing. When the unaged specimens were tested at -40°C (stored at 25°C prior to testing), a two-order-of-magnitude increase was returned, which increased to two orders of magnitude for the aged specimens at the same test temperature.
[0193] This is manifested as increased stiffness and poor recovery for these samples. Without being bound by theory, it is likely that the changes in these tensile properties are due to the increased crystallinity (and associated intermolecular bonding) of the commercial material when compared to the sample 1-3 oligomers. This would also explain the poor thermal shock performance. The above test protocol was designed to simulate what a conformal coating (in this case, an oligomer) would be subjected to under actual use conditions.
[0194] Improved thermal shock resistance
[0195] Thermal shock testing showed that samples 1-3 exhibited improved thermal shock resistance compared to the commercial oligomers.
[0196] Reduction of Tg (glass transition temperature)
[0197] Tg tests show that samples 1-3 exhibit lower Tg temperatures compared to commercially available oligomers.
[0198] The above detailed description has been provided by way of explanation and illustration and is not intended to limit the scope of the appended claims. Many variations of the preferred embodiments of the invention shown herein will be apparent to those of ordinary skill in the art and are still within the scope of the appended claims and their equivalents.
Claims
1. A UV and moisture curable conformal coating composition comprising: 25 to 65 weight percent of an isocyanate functional acrylated polyurethane; 30 to 65 wt % of acrylic monomers; 3.5 to 5.5 wt % photoinitiator; 0.1 to 1 wt % of a defoaming agent; 0.5 to 1.5 wt % of a dehydrating agent; 0.2 wt % to 1.5 wt % of a wetting agent; and 0.5 wt% to 2.5 wt% coupling agent.
2. The composition according to claim 1, comprising 30 to 50 wt% of the isocyanate functional acrylated polyurethane, preferably 35 to 45 wt% of the isocyanate functional acrylated polyurethane.
3. The composition of claim 1 or claim 2, wherein the isocyanate functional acrylated polyurethane is thermoplastic.
4. A composition according to any preceding claim wherein the isocyanate functional acrylated polyurethane is an elastomer.
5. The composition of any preceding claim, wherein the isocyanate functional acrylated polyurethane has a ratio of acrylate functional groups to isocyanate functional groups of from 2:1 to 1:
2.
6. The composition of any preceding claim, wherein the isocyanate functional acrylated polyurethane is the reaction product of reactants comprising: a polyol, preferably an amorphous hydrophobic polyol; A diisocyanate, preferably a branched diisocyanate; and Hydroxyalkyl acrylate.
7. The composition of claim 6, wherein the polyol comprises: One or more of hydroxyl-terminated polybutadiene, hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated polyisoprene, hydroxyl-terminated polyolefin, hydroxyl-terminated polyfarnesene, hydroxyl-terminated hydrogenated polyfarnesene, castor oil, hydrogenated castor oil and dimer acid-based polyester polyol (preferably C36), preferably one or more of hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated hydrogenated polyfarnesene, hydrogenated castor oil and dimer acid-based polyester polyol; and / or The diol is selected from 2-ethyl-1-hexanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, isosorbide, C 18 One or more of dimer glycol, 2-butyl-2-ethyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol and 2,2-diethyl-1,3-propanediol, preferably 2-ethyl-1,3-hexanediol, C 18 One or more of dimer glycol and 2-butyl-2-ethyl-1,3-propanediol; and / or The triol is selected from one or more of trimethylolpropane, triethanolamine, diethanolamine, 1,2,6-hexanetriol, phloroglucinol (1,3,5-trihydroxybenzene) and glycerol, preferably 1,2,6-hexanetriol.
8. A composition according to claim 6 or claim 7, wherein the polyol has a molecular weight of 500 gmol -1 Up to 3000 gmol -1 , preferably 1000 gmol -1 Up to 2000 gmol -1 , more preferably about 2000 gmol -1 The molar mass of .
9. The composition according to any one of claims 6 to 8, wherein the polyol has a functionality of 1.9 to 2.5 and / or a hydroxyl value of 50 to 250 mg KOH / g.
10. The composition according to any one of claims 6 to 9, wherein the diisocyanate comprises 1,3-bis(1-isocyanato-1-methylethyl)benzene (TMXDI, tetramethylxylene diisocyanate), 5-isocyanato-1-(isocyanatomethyl)-1,3,3-trimethylcyclohexane (IPDI, isophorone diisocyanate), 1,6-diisocyanato-2,2,4(2,4,4)-trimethylhexane (TMDI, trimethylhexamethylene diisocyanate), 1,6-diisocyanatohexane (HDI, hexamethylene diisocyanate), 4,4'-diisocyanatodicyclohexylmethane (HDI, hexamethylene diisocyanate), 12 MDI) and one or more of 1,5-diisocyanatopentane (PDI, 1,5-pentamethylene diisocyanate), preferably 1,6-diisocyanato-2,2,4(2,4,4)-trimethylhexane (TMDI, trimethylhexamethylene diisocyanate).
11. The composition according to any one of claims 6 to 10, wherein the hydroxyalkyl acrylate comprises one or more of 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate and 4-hydroxybutyl methacrylate, preferably 4-hydroxybutyl acrylate.
12. A composition according to any preceding claim comprising 45 to 60 wt% acrylic monomers, preferably 50 to 60 wt% acrylic monomers.
13. A composition according to any preceding claim, wherein the acrylic monomer comprises a linear alkyl acrylate containing from 4 to 12 carbon atoms, preferably from 6 to 12 carbon atoms, more preferably from 8 to 10 carbon atoms.
14. A composition according to any preceding claim, wherein the acrylic monomer comprises one or both of 1,6-hexanediol diacrylate and 3-methyl-1,5-pentanediol diacrylate.
15. A composition according to any preceding claim, wherein the acrylic monomer comprises a cyclic acrylate, preferably tetrahydrofurfuryl acrylate, cyclic trimethylolpropane formal acrylate, tert-butyl cyclohexanol acrylate, 3,3,5-trimethylcyclohexyl acrylate, isobornyl acrylate and 2-phenoxyethyl acrylate, more preferably tetrahydrofurfuryl acrylate.
16. A composition according to any preceding claim, wherein the photoinitiator comprises: α-hydroxyketone based photoinitiators; and / or Photoinitiators based on phenylphosphine oxide; and / or Ethyl benzoylformate type photoinitiator.
17. A composition according to any preceding claim, wherein the photoinitiator comprises: α-Hydroxyketone based photoinitiators; Photoinitiators based on phenylphosphine oxide; and Ethyl benzoylformate type photoinitiator.
18. A composition according to claim 16 or claim 17, wherein the alpha-hydroxyketone based photoinitiator comprises 2-hydroxy-2-methyl-1-phenyl-1-propanone.
19. The composition of any one of claims 16 to 18, wherein the phenylphosphine oxide-based photoinitiator comprises phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, ethyl(2,4,6-trimethylbenzoyl)phenylphosphonate and / or diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide.
20. The composition of any one of claims 16 to 19, wherein the ethyl benzoylformate-type photoinitiator comprises methyl benzoylformate.
21. The composition of any one of claims 16 to 20, wherein the photoinitiator comprises: A thioxanthone-type initiator, preferably comprising 2-isopropylthioxanthone; and Tertiary amine synergists preferably include ethyl 4-(dimethylamino)benzoate.
22. A composition according to any preceding claim comprising 3.8 to 5.2 wt% photoinitiator, preferably 4 to 4.5 wt% photoinitiator.
23. A composition according to any preceding claim, wherein the defoaming agent comprises a polyether siloxane.
24. A composition according to any preceding claim comprising 0.2 to 0.8 wt% anti-foaming agent, preferably 0.3 to 0.7 wt% anti-foaming agent.
25. A composition according to any preceding claim, wherein the dehydrating agent comprises p-toluenesulfonyl isocyanate.
26. A composition according to any preceding claim comprising 0.7 to 1.3 wt% dehydrating agent, preferably 0.8 to 1.2 wt% dehydrating agent.
27. A composition according to any preceding claim, wherein the wetting agent comprises poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-graft-poly(ethylene glycol) methyl ether.
28. A composition according to any preceding claim comprising 0.5 to 1.3 wt% wetting agent, preferably 0.8 to 1.2 wt% wetting agent.
29. A composition according to any preceding claim, wherein the coupling agent comprises an acrylate or methacrylate functional silane.
30. A composition according to any preceding claim comprising from 1 to 2 wt% coupling agent, preferably from 1.3 to 1.8 wt% coupling agent.
31. A composition according to any preceding claim further comprising a rheology modifier.
32. The composition of claim 31 , wherein the rheology modifier comprises a polyamide wax.
33. A composition according to claim 31 or 32 comprising 0.1 wt% to 2.5 wt% rheology modifier, preferably 0.2 wt% to 0.8 wt% rheology modifier, more preferably 0.3 wt% to 0.7 wt% rheology modifier.
34. A composition according to any preceding claim further comprising a UV tracer.
35. The composition of claim 34, wherein the UV tracer comprises 2,5-thiophenediylbis(5-tert-butyl-1,3-benzoxazole.
36. A composition according to claim 34 or claim 35 comprising 0.1 wt% to 0.5 wt% UV tracer, preferably 0.2 wt% to 0.4 wt% UV tracer.
37. A composition according to any preceding claim further comprising an odour masking agent.
38. A composition according to claim 37, wherein the odour masking agent comprises one or both, preferably both, of dimethyl-7-octen-2-ol and p-tert-butylcyclohexyl acetate.
39. A method for conformally coating a substrate, the method comprising: Providing a substrate, Providing a composition according to any preceding claim; depositing the composition on at least a portion of the substrate; as well as The coated substrate is exposed to actinic radiation.
40. The method of claim 39, wherein the substrate comprises a circuit board or an electronic component.
41. A substrate coated with a composition according to any one of claims 1 to 38.
Citation Information
Cited By
Toughening type UV moisture dual-curing conformal coating and preparation method thereof
CN119955401A
A toughened UV and moisture dual-curing three-proof paint and its preparation method
CN119955401B
High-stability UV moisture dual-curing conformal coating and preparation method thereof
CN120505034A
High-stable UV-moisture dual-curing three-protection paint and preparation method thereof