Early-strength low-shrinkage cementing material and preparation method thereof
By using clinker minerals such as anhydrous calcium sulfaluminate, dicalcium silicate and calcium sulfate, combined with the iron phase high-temperature calcination and grinding process, early-strength low-shrinkage gelling materials were prepared, and sulfaluminate gelling was solved. The problems of material's strength decrease and production costs after age have achieved high early strength and continuous growth of the material in the later stage, avoiding the problem of shrinkage.
Patent Information
- Application Number
- CN202411053326.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The strength of sulfur aluminate gelling materials no longer increases after reaching a certain age, and even have problems of strength reduction. Their production relies on a large amount of high-grade bauxite to increase costs, limiting their large-scale application.
Anhydrous calcium sulfaluminate, dicalcium silicate and calcium sulfate are used as the main clinker minerals, and early-strength low-shrinkage clinker is prepared through high-temperature calcination and grinding, combined with iron to stimulate each other, forming early high strength and later-stage continuous The gelling material with the characteristics of growth avoids the shrinkage problem of material.
It realizes that gelled materials have high strength and easy construction in the early stage, while avoiding later strength retracting and material shrinkage, meeting engineering needs and reducing production costs.
Smart Images

Figure BDA0004975576090000091 
Figure BDA0004975576090000101 
Figure BDA0004975576090000111
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and in particular relates to an early-strength low-shrinkage gelling material and a preparation method for its industrial production. Background Art
[0002] Sulphoaluminate cementitious material is a cementitious material system independently invented in my country. It has low firing temperature, good grindability, low limestone consumption, and significantly lower carbon emissions than silicate cementitious materials. It is of great significance for energy conservation and emission reduction in the cementitious materials industry.
[0003] However, after reaching a certain age, the strength of sulphoaluminate cementitious materials no longer increases, and even decreases, which is called late strength shrinkage. The hydration products of sulphoaluminate cementitious materials will undergo a crystal transformation in the later stage, from metastable monocalcium aluminate hydrate and dicalcium aluminate hydrate to stable hydrogarnet and alumina. During this transformation process, the relative density of the hydration products increases, resulting in an increase in porosity and structural instability, which causes strength shrinkage. Late strength shrinkage not only affects the performance and service life of the sulphoaluminate cementitious materials themselves, but may also pose a potential threat to the safety and stability of building structures.
[0004] Secondly, anhydrous calcium sulfoaluminate minerals are the main clinker minerals in sulfoaluminate cementitious materials, and its clinker production requires a large amount of high-grade bauxite. As a key target of macro-control and supervision and management of mineral resources, bauxite has been included in the catalog of strategic minerals. The annual increase in the price of bauxite ore has led to a significant increase in the production cost of sulfoaluminate cementitious materials, limiting the large-scale application of sulfoaluminate cementitious materials and becoming an important bottleneck restricting the development of sulfoaluminate cementitious materials.
[0005] Reducing the aluminum content in cementitious material clinker and increasing the silicon content is an important way to alleviate the dependence of sulphoaluminate cementitious materials on bauxite. However, as the content of anhydrous calcium sulphoaluminate with higher activity decreases and the content of belite with lower activity increases, the overall hydration of cementitious materials slows down, and the most distinctive advantage of sulphoaluminate cementitious materials, fast hardening and early strength, is lost, making it difficult to meet the use requirements.
[0006] To this end, many scholars have begun to study the activation of belite to improve the strength of low-aluminum, high-silicon sulfoaluminate cementitious materials, such as: (1) stabilizing the high-temperature variant of belite to prevent the transformation of the more active belite to the less active crystal form; (2) reducing the belite grain size and increasing the lattice distortion. At present, the above goals are mainly achieved through three methods: rapid cooling, low-temperature crystallization, and chemical doping. The above methods can improve the activity of belite to a certain extent, but there is still an urgent need to seek efficient and economical technical methods to improve the activity of belite.
[0007] Therefore, developing a material that can retain the early strength characteristics of sulphoaluminate cementitious materials while absorbing the performance characteristics of belite minerals, so that the cementitious material has the performance characteristics of early strength while also having the characteristics of continuous growth in strength in the later stage, avoiding the shrinkage problem caused by the volume change of the material in the later stage, is a long-awaited but unrealized dream of the cementitious materials and construction industries at home and abroad, and it is also a major technical problem in the professional field of cementitious materials at home and abroad. Summary of the invention
[0008] Based on the technical problems existing in the background technology, the present invention proposes an early-strength, low-shrinkage cementitious material and a preparation method thereof, which takes anhydrous calcium sulfoaluminate and dicalcium silicate as main clinker minerals, and adds appropriate amounts of calcium sulfate and iron to stimulate each other, breaking through the constraints of clinker ingredients of sulfoaluminate cementitious materials at home and abroad, and preparing an early-strength, low-shrinkage clinker, and then using the clinker to design an early-strength, low-shrinkage cementitious material and a preparation method thereof, thereby achieving an early-strength, low-shrinkage cementitious material that has the performance characteristics of early strength, continuous growth in strength in the later period, and avoids the problem of shrinkage in the later period.
[0009] The first object of the present invention is to provide an early strength low shrinkage clinker for use in cementitious materials to alleviate the technical problem of low early strength of existing high-belite cementitious materials.
[0010] The second object of the present invention is to provide a method for preparing early-strength and low-shrinkage clinker, which has the advantages of simple process flow and suitability for industrial production.
[0011] The third object of the present invention is to provide an early-strength low-shrinkage cementitious material, which has the advantages of high early strength and easy construction.
[0012] The fourth object of the present invention is to provide a method for preparing an early-strength, low-shrinkage gelling material, which has the advantages of simple process flow and suitability for industrial production.
[0013] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0014] The invention provides an early-strength low-shrinkage clinker, which comprises the following clinker minerals: anhydrous calcium sulphoaluminate, dicalcium silicate, calcium sulfate and an iron phase, the sum of the mass percentages of the anhydrous calcium sulphoaluminate and the dicalcium silicate is 70% to 90%, the mass ratio of the anhydrous calcium sulphoaluminate to the dicalcium silicate is 0.85 to 1.2, and the mass percentage of the calcium sulfate is 5% to 20%.
[0015] Preferably, the mass ratio of anhydrous calcium sulphoaluminate to dicalcium silicate is 0.87 to 1.15.
[0016] More preferably, the mass ratio of anhydrous calcium sulphoaluminate to dicalcium silicate is 0.9 to 1.1.
[0017] Preferably, the content of anhydrous calcium sulphoaluminate is 33% to 50%, and the content of dicalcium silicate is 33% to 50%.
[0018] More preferably, the content of anhydrous calcium sulphoaluminate is 33.5% to 47%, and the content of dicalcium silicate is 33.5% to 47%.
[0019] More preferably, the content of anhydrous calcium sulphoaluminate is 35% to 45%, and the content of dicalcium silicate is 35% to 45%.
[0020] Preferably, the mass percentage of calcium sulfate is 7% to 15%.
[0021] More preferably, the mass percentage of calcium sulfate is 8% to 12%.
[0022] An early strength low shrinkage cementitious material prepared from early strength low shrinkage clinker comprises the following components by weight percentage: 30% to 100% of early strength low shrinkage clinker and 0% to 70% of cementitious material mixture.
[0023] Preferably, the early strength and low shrinkage cementitious material comprises 100% by weight of early strength and low shrinkage clinker.
[0024] Preferably, an early strength low shrinkage cementitious material comprises the following components by weight percentage: 40% to 90% of early strength low shrinkage clinker and 10% to 60% of cementitious material mixture.
[0025] Further preferably, an early strength low shrinkage cementitious material comprises the following components by weight percentage: 50% to 80% of early strength low shrinkage clinker and 20% to 50% of cementitious material mixture.
[0026] Preferably, the early-strength, low-shrinkage gelling material further comprises 0 to 20% of gypsum by weight.
[0027] Preferably, the cementitious material admixture is any one of granulated blast furnace slag, fly ash, steel slag, limestone, or sandstone, or a combination of at least two thereof.
[0028] Preferably, the gypsum is any one of dihydrate gypsum, anhydrite, hemihydrate gypsum, and desulfurized gypsum, or a combination of at least two thereof.
[0029] A method for preparing early-strength low-shrinkage clinker comprises the following specific steps: firstly grinding and homogenizing the mixed raw materials, and then calcining them at a high temperature of 1250°C±100°C to prepare the early-strength low-shrinkage clinker.
[0030] The mixed raw material is a composition consisting of any two or more of limestone, alkali slag, steel slag, carbide slag, bauxite, high-iron bauxite, garbage fly ash, aluminum ash, bauxite tailings, coal gangue, kaolin, boiling furnace slag, clay, anhydrite, dihydrate gypsum, desulfurized gypsum, hemihydrate gypsum, phosphogypsum, fluorite, desulfurized ash, iron ore, selected iron ore powder, fly ash or granulated blast furnace slag.
[0031] A method for preparing an early strength low shrinkage cementitious material, comprising the steps of: mixing the raw materials and grinding them together to a specific surface area of 200 m 2 / g~800m 2 / g powder to obtain early strength low shrinkage gelling material; or grind each raw material separately to a specific surface area of 200m 2 / g~1000m 2 / g of powder, and then mixed to obtain an early strength and low shrinkage gelling material.
[0032] Preferably, the raw materials are mixed and ground together to a specific surface area of 300m 2 / g~600m 2 / g of powder to obtain the early strength and low shrinkage gelling material.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] Belite is one of the main minerals in silicate cementitious material clinker and sulphoaluminate cementitious material clinker. It has a low calcium content and requires little limestone during firing. It is a low-carbon mineral. However, the belite activity in existing silicate cementitious material clinker and sulphoaluminate cementitious material clinker is low and the hydration rate is slow, resulting in too low early strength of cementitious materials with high belite content. At present, the contradiction between high belite content and low early strength in cementitious materials has not been resolved.
[0035] The inventors have found that calcium sulfate can be used to activate dicalcium silicate during the high-temperature calcination of clinker. When calcium sulfate exists, that is, when the weight percentage of calcium sulfate in the clinker is 5% to 20%, as the calcination temperature rises to 950°C, free calcium and silicon dioxide react with calcium sulfate to form calcium sulfosilicate; as the calcination temperature continues to rise, the remaining calcium sulfate gradually melts to form a liquid phase; when the temperature rises to 1150°C, calcium sulfosilicate decomposes into calcium sulfate and highly active dicalcium silicate in the calcium sulfate liquid phase, and the highly active dicalcium silicate is a mixture of α-type dicalcium silicate and amorphous dicalcium silicate, which has a smaller grain size and higher activity; during the clinker cooling stage, the calcium sulfate liquid phase gradually condenses and solidifies the dicalcium silicate, preventing the transformation of highly active α-type dicalcium silicate and amorphous dicalcium silicate to low-activity β-type dicalcium silicate, thereby preventing the transformation to inactive γ-type dicalcium silicate, and ensuring the final activity of the dicalcium silicate.
[0036] In addition, when calcium sulfate is present, dicalcium silicate, anhydrous calcium sulfoaluminate and calcium sulfate will react together to form ettringite (C6AS3H 32 ), calcium silicate hydrate gel (CSH) and aluminum gel (AH3), among which calcium silicate hydrate and aluminum gel are colloids. The content and proportion of crystal colloidal products determine the strength of cement-based materials after hydration and hardening. When the crystal / colloid ratio is too low, the compressive strength is low and the shrinkage is large; when the crystal / colloid ratio is too high, the material expands too much and cracks, and the flexural / tensile strength decreases significantly, and the compressive strength will also decrease to a certain extent. The weight ratio of dicalcium silicate and anhydrous calcium sulfoaluminate in the clinker determines the amount of crystals and colloidal products generated in the hydration product. Therefore, by regulating the content of dicalcium silicate and anhydrous calcium sulfoaluminate, the mechanical properties of cement-based materials can be optimized. Studies have shown that when the sum of the weight percentages of dicalcium silicate and anhydrous calcium sulfoaluminate in the clinker is 70% to 90%, both the early strength and the later strength are high; further, the mass ratio of anhydrous calcium sulfoaluminate to dicalcium silicate is 0.85 to 1.2, and the shrinkage and expansion of the material are small.
[0037]
[0038] The early-strength low-shrinkage clinker of the present invention has the characteristics of high activity and fast hydration reaction. The cementitious material prepared from the clinker has technical advantages such as high early and late strength and low shrinkage, which can alleviate the technical problem of low early strength of existing high-belite cementitious materials and meet engineering needs. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is described in detail below through specific embodiments.
[0040] Example 1: An early strength and low shrinkage clinker
[0041] Limestone and carbide slag are mixed according to the clinker mineral mass ratio of 35% anhydrous calcium sulphoaluminate, 38.5% dicalcium silicate and 12% calcium sulfate, and the remainder is mixed mineral components. Put it into a grinder and crush it to a particle size of 500μm. After homogenization, it is calcined at a high temperature of 1250℃ to prepare early strength and low shrinkage clinker.
[0042] Example 2: An early strength low shrinkage clinker
[0043] Bauxite, fly ash and aluminum ash are mixed according to the clinker mineral mass ratio of 45% anhydrous calcium sulphoaluminate, 39.2% dicalcium silicate and 8% calcium sulfate, and the remainder is mixed mineral components. Put them into a grinder and crush them to a particle size of 400μm. After homogenization, they are calcined at 1300℃ to prepare early strength and low shrinkage clinker.
[0044] Example 3: An early strength and low shrinkage clinker
[0045] The coal gangue, kaolin and boiling furnace slag are mixed according to the clinker mineral mass ratio of 37% anhydrous calcium sulphoaluminate, 41.2% dicalcium silicate and 9% calcium sulfate, and the rest is mixed mineral components. Put them into a grinder and crush them to a particle size of 300μm. After homogenization, they are calcined at a high temperature of 1350℃ to prepare early strength and low shrinkage clinker.
[0046] Example 4: An early strength low shrinkage clinker
[0047] Limestone, kaolin and selected iron ore powder are mixed according to the clinker mineral mass ratio of 41.5% anhydrous calcium sulphoaluminate, 38% dicalcium silicate and 9.5% calcium sulfate, and the remainder is mixed mineral components. Put them into a grinder and crush them to a particle size of 300μm. After homogenization, they are calcined at a high temperature of 1300℃ to prepare early strength and low shrinkage clinker.
[0048] Example 5: An early strength and low shrinkage clinker
[0049] The garbage fly ash, aluminum ash, bauxite tailings and anhydrite are mixed according to the clinker mineral mass ratio of 37% anhydrous calcium sulphoaluminate, 42.5% dicalcium silicate and 15% calcium sulfate, and the remainder is mixed mineral components. Put it into a grinder and crush it to a particle size of 400μm. After homogenization treatment, it is calcined at a high temperature of 1250℃ to prepare early strength and low shrinkage clinker.
[0050] Example 6: An early strength low shrinkage gelling material
[0051] The clinker of Example 1: the cementitious material mixture (blast furnace slag + fly ash): dihydrate gypsum in a mass ratio of 70%: 25%: 5% were put into a grinder and ground to a specific surface area of 300m 2 / g of powder to obtain an early-strength, low-shrinkage gelling material.
[0052] Example 7: An early strength low shrinkage gelling material
[0053] The clinker of Example 2: cementitious material mixture (fly ash + limestone): anhydrite in a mass ratio of 80%:16%:4% were put into a grinder and ground to a specific surface area of 400m 2 / g of powder to obtain an early-strength, low-shrinkage gelling material.
[0054] Example 8: An early strength low shrinkage gelling material
[0055] The clinker of Example 3: the cementitious material mixture (limestone + sandstone): the semi-hydrated gypsum in a mass ratio of 60%: 30%: 10% were put into a grinder and ground to a specific surface area of 500m 2 / g of powder to obtain an early-strength, low-shrinkage gelling material.
[0056] Example 9: An early-strength, low-shrinkage gelling material
[0057] The clinker of Example 4: the cementitious material mixture (blast furnace slag + steel slag): the desulfurized gypsum in a mass ratio of 75%: 21%: 4% were put into a grinder and ground to a specific surface area of 550 m 2 / g of powder, and then mix them evenly to obtain early strength and low shrinkage gelling material.
[0058] Example 10: An early strength low shrinkage gelling material
[0059] The clinker of Example 5 and dihydrate gypsum were put into a grinder at a mass ratio of 90%:10% and ground to a specific surface area of 500m 2 / g of powder to obtain an early-strength, low-shrinkage gelling material.
[0060] Comparative Example 1: An early strength and low shrinkage clinker
[0061] Limestone and carbide slag are mixed according to the clinker mineral mass ratio of 42% anhydrous calcium sulphoaluminate, 47% dicalcium silicate and 4% calcium sulfate, and the remainder is mixed mineral components. The mixture is put into a grinder and crushed to a particle size of 500 μm. After homogenization treatment, the mixture is calcined at a high temperature of 1250°C to prepare an early strength and low shrinkage clinker.
[0062] Comparative Example 2: An early strength and low shrinkage clinker
[0063] Limestone and carbide slag are mixed according to the clinker mineral mass ratio of 32.5% anhydrous calcium sulphoaluminate, 36.5% dicalcium silicate, 21% calcium sulfate, and 7% iron phase, and the remainder is mixed mineral components. Put it into a grinder and crush it to a particle size of 500μm. After homogenization treatment, it is calcined at a high temperature of 1250℃ to prepare an early strength and low shrinkage clinker.
[0064] Comparative Example 3: An early strength low shrinkage gelling material
[0065] The clinker of Comparative Example 1: cementitious material mixture (blast furnace slag + fly ash): dihydrate gypsum in a mass ratio of 70%: 25%: 5% were put into a grinder and ground to a specific surface area of 300m 2 / g of powder to obtain an early-strength, low-shrinkage gelling material.
[0066] Comparative Example 4: An early-strength low-shrinkage gelling material
[0067] The clinker of comparative example 2: cementitious material mixture (fly ash + limestone): anhydrite in a mass ratio of 80%:16%:4% were put into a grinder and ground to a specific surface area of 400m 2 / g of powder to obtain an early-strength, low-shrinkage gelling material.
[0068] (I) Strength test
[0069] The strength test was carried out using the GB / T 17671-2021 clinker strength test method (ISO method) using a flexural and compression machine. The test results are shown in Table 1 below.
[0070] Table 1
[0071]
[0072] The shrinkage test method of JC / T 603-2004 was used to test the shrinkage of the clinker. The test results are shown in Table 2 below.
[0073] Table 2
[0074]
[0075] In Table 1 and Table 2, C1 is sulphoaluminate clinker, and C2 is high-belite sulphoaluminate clinker. It can be seen from Table 1 that in Comparative Example 1, due to the high content of anhydrous calcium sulphoaluminate and dicalcium silicate, the flexural / compressive strength of 1d and 3d is high, but due to the low content of calcium sulfate, the flexural / compressive strength of 28d is significantly lower than that of the embodiment, and the shrinkage rate is greater than that of the embodiment. In Comparative Example 2, due to the excessively high content of calcium sulfate, the flexural / compressive strength of 1d and 3d is high, and due to the excessively high content of calcium sulfate, the flexural / compressive strength of 28d is significantly lower and lower than that of the embodiment, and the shrinkage rate is greater than that of the embodiment. The flexural / compressive strength of 1d, 3d and 28d of Examples 1-5 is significantly higher than that of C1 and C2, and the shrinkage rate is less than that of C1 and C2.
[0076] The strength test of mortar was carried out using the flexural and compression machine in accordance with GB / T 17671-2021 cementitious material mortar strength test method (ISO method). The test results are shown in Table 3 below.
[0077] Table 3
[0078]
[0079] The shrinkage test method of JC / T 603-2004 was used to test the shrinkage of the cementitious material. The test results are shown in Table 4 below.
[0080] Table 4
[0081]
[0082] In Table 3 and Table 4, D1 is a sulphoaluminate cementitious material, and D2 is a high-belite sulphoaluminate cementitious material. It can be seen from Table 3 that in Comparative Example 3, due to the high content of anhydrous calcium sulphoaluminate and dicalcium silicate, the flexural / compressive strength of 1d and 3d is high, but due to the low content of calcium sulfate, the flexural / compressive strength of 28d is significantly lower than that of the embodiment, and the shrinkage rate is greater than that of the embodiment. In Comparative Example 4, due to the excessively high content of calcium sulfate, the flexural / compressive strength of 1d and 3d is high, and due to the excessively high content of calcium sulfate, the flexural / compressive strength of 28d is significantly lower than that of the embodiment, and the shrinkage rate is greater than that of the embodiment. The flexural / compressive strength of 1d, 3d and 28d of Examples 6-10 is significantly higher than that of D1 and D2, and the shrinkage rate is less than that of D1 and D2.
[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An early strength low shrinkage clinker, the clinker comprising the following clinker minerals: anhydrous calcium sulphoaluminate, dicalcium silicate and calcium sulfate, Features The sum of the mass percentages of anhydrous calcium sulphoaluminate and dicalcium silicate is 70% to 90%, the mass ratio of anhydrous calcium sulphoaluminate to dicalcium silicate is 0.85 to 1.2, and the mass percentage of calcium sulfate is 5% to 20%.
2. The early strength and low shrinkage clinker according to claim 1, Features The mass ratio of anhydrous calcium sulphoaluminate to dicalcium silicate is 0.87 to 1.
15.
3. The early strength and low shrinkage clinker according to claim 2, Features The mass ratio of anhydrous calcium sulphoaluminate to dicalcium silicate is 0.9 to 1.
1.
4. The early strength and low shrinkage clinker according to claim 3, Features : The content of anhydrous calcium sulphoaluminate is 33% to 50%, and the content of dicalcium silicate is 33% to 50%.
5. The early strength and low shrinkage clinker according to claim 4, Features The content of anhydrous calcium sulphoaluminate is 33.5% to 47%, and the content of dicalcium silicate is 33.5% to 47%.
6. The early strength and low shrinkage clinker according to claim 5, Features The content of anhydrous calcium sulphoaluminate is 35% to 45%, and the content of dicalcium silicate is 35% to 45%.
7. The early strength and low shrinkage clinker according to claim 1, Features : The mass percentage of calcium sulfate is 7% to 15%.
8. The early strength and low shrinkage clinker according to claim 7, Features : The mass percentage of calcium sulfate is 8% to 12%.
9. An early-strength, low-shrinkage cementitious material prepared from the early-strength, low-shrinkage clinker according to any one of claims 1 to 8, comprising the following components by weight percentage: 30% to 100% of the early-strength, low-shrinkage clinker and 0% to 70% of a cementitious material admixture.
10. The early strength and low shrinkage gelling material according to claim 9, Features : Early strength and low shrinkage clinker with a weight percentage of 100%.
11. The early-strength, low-shrinkage gelling material according to claim 9, Features: Calculated by weight percentage, it includes the following components: 40% to 90% of early strength and low shrinkage clinker and 10% to 60% of cementitious material admixture.
12. The early strength and low shrinkage gelling material according to claim 11, Features: Calculated by weight percentage, it includes the following components: 50% to 80% of early strength and low shrinkage clinker and 20% to 50% of cementitious material admixture.
13. An early strength low shrinkage gelling material according to any one of claims 9 to 12, Features: Calculated by weight percentage, it also includes 0-20% gypsum.
14. An early strength low shrinkage gelling material according to any one of claims 9, 11, 12 or 13, Features The cementitious material mixture is any one of granulated blast furnace slag, fly ash, steel slag, limestone or sandstone, or a combination of at least two of them.
15. The early strength and low shrinkage gelling material according to claim 13, Features The gypsum is any one of dihydrate gypsum, anhydrite, hemihydrate gypsum and desulfurized gypsum, or a combination of at least two of them.
16. A method for preparing the early-strength low-shrinkage clinker according to any one of claims 1 to 8, the specific steps being: firstly grinding and homogenizing the mixed raw materials, and then calcining them at a high temperature of 1250°C±100°C to prepare the early-strength low-shrinkage clinker. The mixed raw material is a composition consisting of any two or more of limestone, alkali slag, steel slag, carbide slag, bauxite, high-iron bauxite, garbage fly ash, aluminum ash, bauxite tailings, coal gangue, kaolin, boiling furnace slag, clay, anhydrite, dihydrate gypsum, desulfurized gypsum, hemihydrate gypsum, phosphogypsum, fluorite, desulfurized ash, iron ore, selected iron ore powder, fly ash or granulated blast furnace slag.
17. A method for preparing an early strength low shrinkage gelling material according to any one of claims 9 to 15, comprising the steps of: mixing the raw materials and grinding them together to a specific surface area of 200 m 2 / g~800m 2 / g powder to obtain the early strength low shrinkage gelling material; or grind each raw material separately to a specific surface area of 200m 2 / g~1000m 2 / g of powder, and then mixing to obtain the early strength and low shrinkage gelling material.
Citation Information
Cited By
Early-strength anti-cracking solid-waste-based belite cementing material and preparation method thereof
CN120504506A