Sludge curing agent as well as preparation method and application thereof

The preparation of sludge curing agents through cement, granulated blast furnace slag powder, fly ash and other materials has solved the problem of stabilization and resource utilization of soft soil silt produced by silting, achieved rapid curing and strength improvement of silt, and reduced construction Cost and pollution have good environmental benefits.

CN118978368APending Publication Date: 2024-11-19HAINAN LANDAO ENVIRONMENTAL PROTECTION IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411059716.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Traditional methods cannot effectively stabilize and resource utilization of soft soil silt produced by silting, resulting in high pollution and construction costs, and the existing sludge curing agent materials are complex and the application conditions are harsh.

Method used

Sludge curing agent is prepared by materials such as cement, granulated blast furnace slag powder, fly ash and curing agent masterbatch (limestone, iron powder, composite mineralizer). It is prepared by dry powder stirring method, and the dosage is increased to more than 45%, so as to achieve Rapid curing and strength increase of sludge.

Benefits of technology

It has achieved in-situ solidification of sludge, reduced construction costs, met the construction requirements of highway engineering, and used industrial solid waste in resource utilization to reduce pollution, which has good environmental and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979763740000061
    Figure BDA0004979763740000061
  • Figure BDA0004979763740000062
    Figure BDA0004979763740000062
  • Figure BDA0004979763740000071
    Figure BDA0004979763740000071
Patent Text Reader

Abstract

The invention provides a sludge curing agent and a preparation method and application thereof, and belongs to the technical field of curing agents and solid waste resource utilization, the curing agent comprises the following raw materials by mass: 45%-65% of cement, 18%-30% of mineral powder, 9%-20% of fly ash and 8%-10% of curing agent master batch. Solid waste materials such as mineral powder and coal ash are used for achieving solidification and stabilization of the mud flat sludge, no special additive needs to be added, and the method has the advantages of being low in price and simple in material. Besides, the solid wastes such as the fly ash and the green mud recovered from the pulping alkali of the paper pulp mill are subjected to resource utilization, so that the economic benefit is increased, and meanwhile, the pollution problem of the ecological environment is relieved; meanwhile, sludge can be cured in situ, the curing speed is high, the construction period can be greatly shortened, the construction cost is reduced, and the method is suitable for large-scale sludge and soft foundation treatment; and the prepared sludge solidified soil meets the construction requirements of highway engineering, and has excellent compression resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of curing agent and solid waste resource utilization, and in particular relates to a sludge curing agent and a preparation method and application thereof. Background Art

[0002] Soft soil refers to fine-grained soil with high natural water content, large porosity, high compressibility and low shear strength. It generally refers to soft clay, silt soil, silt peat soil, peat and other soft soils. The definition of highway roadbed is: clay soil with standard penetration number less than 4, unconfined compressive strength less than 50kPa, water content greater than 50% and sandy soil with standard penetration number less than 10 and water content greater than 30% are collectively called soft soil. According to the Technical Specifications for Design and Construction of Highway Soft Soil Foundation Embankment (JTJ017-96), soft soil meets the three indicators of natural water content ≧35% or liquid limit, natural porosity ≧1.0, and cross-plate shear strength <35kPa.

[0003] Silt is a soft soil with a high natural water content and a porosity ratio of ≧1.5. It has rheological and thixotropic properties. It is a modern sediment formed in a static water or slow-flowing environment with the participation of microorganisms. It is rich in organic matter, often gray-black in color, and has the properties of low strength, high compressibility, high permeability, low shear strength, and poor seismic resistance. If there is silt in the foundation, it will easily cause the building to sink.

[0004] With the increase in the amount of highway infrastructure construction in my country, the construction of highways in coastal cities involves silt and soft soil sections, resulting in a huge amount of silt generated by dredging of rivers and waterways and soft soil silt generated by highway construction. The traditional method of dealing with these silts generated by dredging is to use sea dumping and soil replacement backfill construction, but after soil replacement, the original silt needs to be stored in another place, causing new pollution; and the soft soil silt generated by dredging cannot meet the requirements of highway construction due to its own properties and cannot be directly utilized as a resource; therefore, the stabilization and harmless treatment of dredged soft soil silt has become an engineering problem that needs to be solved urgently.

[0005] A curing agent is a material that uses chemical or biological methods to cement soil particles. By adding a curing agent to the soil, the purpose of increasing soil strength, reducing soil deformation, and reducing soil permeability can be achieved within the required time. At present, there are many research results on sludge curing agents, but most of them use complex materials, and the application conditions are relatively harsh and the process flow is complicated.

[0006] In order to solve this problem, the present invention provides a curing agent for soft soil silt in highway engineering construction, which has the advantages of simple materials and low price. The silt in the construction section is then cured in situ, so that the compressive strength and bearing ratio of the cured silt can meet the requirements of highway engineering construction, and can be used in the original site and can also be used for other civil engineering projects. At the same time, when preparing the curing agent, industrial solid waste fly ash, mineral powder, etc. can be utilized as waste resources, which does not cause pollution and saves engineering costs, and has important social benefits and application value. Summary of the invention

[0007] In order to solve the above technical problems, the present invention proposes a sludge solidifying agent and a preparation method and application thereof, which can increase the total amount of fly ash and granulated blast furnace slag powder solid waste to 45%, play a role in the resource recycling of industrial waste, produce good environmental benefits, energy saving and environmental protection, and low price; the prepared solidifying agent can increase the speed and strength of sludge solidification, can achieve the requirements of in-situ solidification of large-scale sludge, reduce construction costs, and at the same time the solidified soil meets the actual needs of highway engineering construction.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] One of the technical solutions of the present invention:

[0010] A sludge solidifying agent, wherein the raw materials include, by weight percentage:

[0011] Cement 45%-65%, mineral powder 18%-30%, fly ash 9%-20% and curing agent masterbatch 8%-10%.

[0012] Preferably, the cement is pozzolanic silicate cement;

[0013] The mineral powder is granulated blast furnace slag powder;

[0014] The preparation process of the mineral powder is as follows: water-quenched blast furnace slag is dried, ball-milled, and then dried and dehydrated by a dryer to obtain high-fineness and high-activity granulated blast furnace slag powder, also known as mineral powder;

[0015] The fly ash is fly ash from a power plant and belongs to first-class fly ash.

[0016] Preferably, the curing agent masterbatch comprises the following raw materials: limestone, iron powder, fly ash and composite mineralizer.

[0017] Furthermore, the mass ratio of the limestone, iron powder, fly ash and composite mineralizer is 65:2:30:3.

[0018] Furthermore, the composite mineralizer is desulfurized gypsum and fluorite, and the mass ratio of the two is 3:1.

[0019] Preferably, the preparation method of the curing agent masterbatch is: uniformly mixing the above raw materials, sintering at high temperature, and ball milling to obtain the curing agent masterbatch.

[0020] Furthermore, the specific conditions of the high temperature sintering are: high temperature sintering at 1400°C-1500°C for 2.5-3.5h.

[0021] Preferably, the ball milling in the preparation process of the mineral powder and the ball milling in the preparation method of the curing agent masterbatch both use one or a combination of a vertical roller mill system, a vibration mill or a Raymond mill; the ball milling time is 25 to 30 minutes, the fineness of the powder is 250 to 350 mesh and the moisture content is less than 0.5%.

[0022] The second technical solution of the present invention:

[0023] A method for preparing a sludge solidifying agent comprises the following steps:

[0024] The above raw materials are mixed evenly, and a sludge solidifying agent is prepared by a dry powder stirring method.

[0025] Preferably, the specific steps of the dry powder stirring method are: stirring the raw materials at a low speed of 140±5r / min for 30 to 40min.

[0026] The third technical solution of the present invention:

[0027] The above-mentioned sludge solidifying agent is used in solidifying soft soil sludge in highway engineering construction and / or green mud for pulping alkali recovery in pulp mill.

[0028] Preferably, the dosage of the sludge solidifying agent is 5% to 10% of the total mass of the soft soil sludge from highway construction and the green mud for alkali recovery from pulping in a pulp mill.

[0029] The role of each raw material component in the sludge solidifying agent of the present invention in the sludge solidification process is as follows:

[0030] Cement: Cement mineral phases C3S, C2S, C3A, C4AF and calcium sulfate undergo hydration reactions to generate CSH, CAH, AFm, AFt, CH and other hydration products. The cementation between the powder, sand and gravel particles of different sizes forms a structural whole with a certain strength, which improves the strength of the solidified soil. Cement and the water in the silt react with CaO+H2O→Ca(OH)2, and the OH generated by the ionization of the generated Ca(OH)2 - The ions effectively neutralize the acidic substances in the sludge, increase the pH, and provide an alkaline environment for the sludge solidification process.

[0031] Mineral powder: slag is industrial waste discharged after mineral processing or smelting, which contains a large amount of glass and has great potential activity, but needs to be ground into powder to stimulate its activity; the mineral powder mainly based on the CaO-Al2O3-SiO2 system adopts the method of physical excitation (mechanical grinding) in the present invention, aiming to reduce the particle fineness, increase the specific surface area, increase its glass phase content and volcanic ash reaction activity, thereby increasing the rate and intensity of reaction with sludge. Among them, mineral powder can fill the pores in the sludge, reduce the porosity, and improve the density of the sludge.

[0032] Fly ash: Fly ash is industrial solid waste discharged from coal-fired power plants. In the early stage, fly ash has low activity and can only be used for filling. As its age increases, the soluble substances it contains gradually react with Ca(OH)2 to form a gelling substance with a certain strength.

[0033] Limestone: CaO reacts with the water in the sludge to form Ca(OH)2, which can undergo ion exchange with clay particles and adsorb between particles to form solids. During the solidification process of sludge, Ca(OH)2 in the hardened material will recrystallize and carbonize to form CaCO3, which can make the material harder and increase the solidification strength during the solidification of sludge. The alkaline components of limestone can effectively increase the pH of sludge, thereby promoting the decomposition of organic matter and the solidification of harmful substances, and improving the strength of solidification.

[0034] Iron powder: C3S and C2S are generated during high-temperature calcination. Iron powder can increase the liquid limit, promote C2S to absorb f-CaO to form C3S, increase the hardening speed of cement clinker and enhance the bonding effect. After reacting with water in the sludge, it can form a hardened body with high strength and good durability, thereby improving the solidification strength of the sludge.

[0035] Composite mineralizer: SO3 in gypsum can reduce the liquid limit viscosity of cement, increase the liquid limit, and is conducive to the formation of C3S. On the other hand, it can form 2C2S·CaSO4 and C4A3S, which is an early strength mineral that can effectively improve the speed and strength of sludge solidification.

[0036] CaF2 in fluorite can produce hydrofluoric acid under high temperature to generate SiF4 and CaF. The reaction promotes the decomposition of carbonates and destroys the SiO2 lattice. CaF2 and other components generate calcium fluorosilicate, calcium fluoroaluminate, etc. through solid phase reaction, which effectively generates C2S and C3S, enhances the solidification reaction, and improves the strength and crack resistance of sludge solidification.

[0037] Compared with the prior art, the present invention has the following advantages and technical effects:

[0038] The sludge solidifying agent disclosed in the present invention can solidify and stabilize the sludge generated by dredging of rivers and waterways and soft soil sludge in highway engineering construction; the raw materials used by the solidifying agent are simple in type and widely in source, including solid waste slag, fly ash, etc. On the one hand, it realizes the comprehensive resource treatment of waste materials such as slag, fly ash, and green mud recovered from pulping alkali in pulp mills, saving resources and producing good environmental benefits; on the other hand, the sludge itself does not need to be added with special additives or special process environment treatment. In the face of sludge under different natural conditions, the solidifying agent can be proportioned and deployed so that the solidification speed and strength can meet the actual engineering needs. That is, large-scale sludge can be solidified and treated in situ, the construction method is simple, the total project cost is saved, and the problems of water and soil environmental pollution are solved at the same time. DETAILED DESCRIPTION

[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0040] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0044] The invention discloses a curing agent for soft soil sludge in highway engineering construction. The curing agent comprises the following raw materials in terms of mass percentage: 45% to 65% of cement, 18% to 30% of mineral powder (granulated blast furnace slag powder), 9% to 20% of fly ash and 8% to 10% of curing agent masterbatch.

[0045] In some preferred embodiments, the cement is pozzolanic silicate cement with a strength of 32.5 MPa and a specific surface area of ​​393.8 m 2 / kg.

[0046] In some preferred embodiments, the granulated blast furnace slag powder has a specific surface area of ​​372.0 m 2 / kg.

[0047] In some preferred embodiments, fly ash is the main solid waste discharged from coal-fired power plants, with a specific surface area of ​​409.8 m 2 / kg, which is first-grade fly ash.

[0048] In some preferred embodiments, the curing agent masterbatch has a specific surface area of ​​440.4 m 2 / kg; wherein, the curing agent masterbatch includes the following raw materials, according to the mass ratio, limestone: iron powder: fly ash: desulfurized gypsum: fluorite = 65: 2: 30: 2.25: 0.75. The chemical composition and content (wt.%) of each raw material are shown in Table 1 below:

[0049] Table 1

[0050] raw material CaO SiO2 <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SO3]]> <![CDATA[CaF2]]> limestone 52.26 3.10 0.94 0.57 0.68 0 0 Iron Fan 8.11 17.80 5.95 65.84 0.93 0 0 Fly ash 5.60 48.40 37.31 5.12 2.22 0 0 Desulfurization gypsum 32.12 2.72 1.40 4.59 2.18 40.12 0 fluorite 11.56 11.10 1.40 0.50 1.90 0 56.12

[0051] The invention discloses a method for preparing a curing agent for soft soil sludge in highway engineering construction, which specifically comprises the following steps:

[0052] Step 1. According to the mass ratio, limestone, iron powder, fly ash and composite mineralizer (desulfurized gypsum and fluorite) are weighed, the raw materials are mixed evenly, and then sintered at 1400°C to 1500°C for 2.5 to 3.5 hours. The obtained material is ball-milled into powder to obtain a curing agent masterbatch, which is sealed and stored for standby use;

[0053] Step 2. The water-quenched blast furnace slag is dried, ball-milled, and then dried and dehydrated in a dryer to obtain high-fineness and high-activity granulated blast furnace slag powder, also known as ore powder, which is sealed and stored for later use;

[0054] Step 3. Accurately weigh the powder of each component according to the mass percentage, place the raw material components (curing agent masterbatch, cement, mineral powder, fly ash) in a cement mortar mixer, and stir at a low speed of 140±5r / min for 30-40min to make the powder mix evenly, and obtain a powder density of 2.82g / cm 3Sludge solidifying agent;

[0055] In addition, the present invention also discloses the application of the above-mentioned curing agent in soft soil sludge of highway engineering, specifically: the sludge excavated from the construction section, the green mud recovered from pulping alkali in the pulp mill and the curing agent are evenly mixed, and the mixture is naturally cured in situ;

[0056] The mass proportion of the curing agent is 5% to 10% of the total mass of the sludge and pulping alkali recovery green mud.

[0057] All raw materials used in the examples of the present invention are commercially available.

[0058] Unless otherwise specified, the “parts” used in the embodiments of the present invention are “parts by weight”.

[0059] The technical solution of the present invention is further illustrated by the following embodiments.

[0060] Example 1

[0061] (A) A method for preparing a curing agent, comprising the following steps:

[0062] Step 1. According to the mass ratio, limestone, iron powder, fly ash and composite mineralizer (desulfurized gypsum and fluorite) are weighed, the raw materials are mixed evenly, and then sintered at 1400°C for 3.0 hours. The obtained material is ball-milled (the ball-milling time is 30 minutes, the fineness is 350 mesh, and the moisture content is 0.44%) to become powder to obtain a curing agent masterbatch, which is sealed and stored for standby use;

[0063] Step 2. The water-quenched blast furnace slag is dried (drying temperature is 250°C, time is 1.5h), ball milled (ball milling time is 30min, fineness is 325 mesh, moisture content is 4.50%), and then dried and dehydrated in a dryer (drying temperature is 105°C, dehydrated to a moisture content of 0.48%) to obtain high-fineness and high-activity slag micropowder, also known as mineral powder, which is sealed and stored for standby use;

[0064] Step 3. According to the mass percentage, 45.46% of raw cement, 27.27% of granulated blast furnace slag powder, 18.18% of fly ash and 9.09% of curing agent masterbatch are stirred at a low speed of 140±5r / min for 40min to make the powders evenly mixed to obtain sludge curing agent 1.

[0065] (ii) The steps of solidifying sludge and green mud are:

[0066] At room temperature of 25°C, a mixture of pulp mill alkali recovery green mud (water content of 97.7%, the same below) and sludge 1 (various test indexes of sludge 1 are shown in Table 2) was solidified using sludge solidifier 1. The dosage of sludge solidifier 1 was 5% of the total mass of sludge 1 and pulp mill alkali recovery green mud (wherein the mass ratio of sludge 1 to green mud was 90:10). Obvious solidification was observed within 48 hours, indicating that the sludge solidification test was fast.

[0067] Note: The method of solidifying silt and chlorite in the above step (ii) refers to 2.2 Silt Solidification Method for Solidifying Silt and Chlorite in the paper "Solidification Test and Filling Performance Analysis of Ultra-High Moisture Content Lake Phase Silt" in Wang Jiangying Silicate Bulletin.

[0068] Table 2

[0069]

[0070] Example 2

[0071] The difference from Example 1 is that

[0072] The various test indexes of the sludge 2 used for solidification in step (ii) are shown in Table 3.

[0073] Other conditions are consistent with those in Example 1.

[0074] Table 3

[0075]

[0076]

[0077] Example 3

[0078] The difference from Example 1 is that

[0079] The raw material types and dosage ratios of the curing agent in step (i) are: 63.64% cement, 18.18% granulated blast furnace slag powder, 9.09% fly ash and 9.09% curing agent masterbatch.

[0080] And the various test indexes of the sludge 3 used for solidification in step (ii) are shown in Table 4.

[0081] Other conditions are consistent with those in Example 1.

[0082] Table 4

[0083]

[0084] Example 4

[0085] The difference from Example 1 is that

[0086] The various test indexes of the sludge 4 used for solidification in step (ii) are shown in Table 5.

[0087] Other conditions are consistent with those in Example 1.

[0088] Table 5

[0089]

[0090]

[0091] Example 5

[0092] The difference from Example 3 is that

[0093] The various test indexes of the sludge 5 used for solidification in step (ii) are shown in Table 6.

[0094] Table 6

[0095]

[0096] Comparative Example 1

[0097] The only difference from Example 1 is that no mineral powder is added to the curing agent ratio in step 3, and the cement, fly ash and curing agent masterbatch are accurately weighed and uniformly mixed according to the mass percentages of 62.50%, 25.00% and 12.50% respectively to obtain the sludge curing agent. Other conditions are the same as in Example 1.

[0098] Comparative Example 2

[0099] The only difference from Example 5 is that no curing agent masterbatch is added to the curing agent ratio in step 3, and cement, mineral powder and fly ash are prepared in a mass percentage ratio of 62.50%, 25.00% and 12.50%. The three materials are accurately weighed and uniformly mixed to obtain a sludge curing agent. Other conditions are the same as in Example 5.

[0100] Effect verification

[0101] The unconfined compressive strength test of the silt-solidified soil obtained in Examples 1 to 5 was carried out using an electronic universal testing machine (microcomputer controlled). According to the T0134-2019 bearing ratio CBR test method in the JTG 3430-2020 "Highway Geotechnical Test Code" standard, the test was carried out using a bearing ratio tester. Table 7 below shows the test results when the number of blows is 50.

[0102] Table 7

[0103]

[0104]

[0105] Conclusion: The above data show that the compressive strength, bearing ratio and other data of the silt-solidified soil of Examples 1 to 5 can meet the strength requirements of the construction of the highway subbase; among them, the obtained silt-solidified soil has high strength and good stability, which can meet the requirements of the highway subbase construction. For the silt of 5 different working conditions in the actual construction section, the optimal curing agent ratio scheme required by each is developed, which also achieves the ultimate purpose of the present invention, provides data guarantee for subsequent on-site construction, and can also be applied to other civil engineering projects.

[0106] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A sludge solidifying agent, characterized in that: In terms of mass percentage, the raw materials include: Cement 45%-65%, mineral powder 18%-30%, fly ash 9%-20% and curing agent masterbatch 8%-10%.

2. A sludge solidifying agent according to claim 1, characterized in that: The curing agent masterbatch comprises the following components: limestone, iron powder, fly ash and composite mineralizer.

3. A sludge solidifying agent according to claim 2, characterized in that: The mass ratio of the limestone, iron powder, fly ash and composite mineralizer is 65:2:30:

3.

4. A sludge solidifying agent according to claim 2, characterized in that: The composite mineralizer is desulfurized gypsum and fluorite, and the mass ratio of the two is 3:

1.

5. A sludge solidifying agent according to claim 2, characterized in that: The preparation method of the curing agent masterbatch is: uniformly mixing the above raw materials, sintering at high temperature, and ball milling to obtain the curing agent masterbatch.

6. A sludge solidifying agent according to claim 5, characterized in that: The specific conditions of the high temperature sintering are: high temperature sintering at 1400° C.-1500° C. for 2.5 to 3.5 hours.

7. A method for preparing a sludge solidifying agent, characterized in that: The following steps are involved: The raw materials described in any one of claims 1 to 6 are mixed uniformly, and a sludge solidifying agent is prepared by a dry powder stirring method.

8. The method for preparing a sludge solidifying agent according to claim 7, characterized in that: The specific steps of the dry powder stirring method are: stirring the raw materials at a low speed of 140±5r / min for 30 to 40min.

9. Use of the sludge solidifying agent according to any one of claims 1 to 6 in solidifying soft soil sludge in highway construction and green mud for alkali recovery in pulping in pulp mills.