Cleaning solution for copper interconnection after polishing with cobalt as barrier layer and preparation method and application of cleaning solution

Through the combination of biodegradable polycarboxylic acid chelating agent and fatty acid potential protector, the pollution and galvanic corrosion of the copper surface after chemical mechanical polishing is solved, and the efficient and environmentally friendly cleaning effect is achieved, and the finished product rate of the integrated circuit is improved. and environmentally friendly.

CN118978959APending Publication Date: 2024-11-19SHANGHAI INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040495.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In integrated circuit manufacturing, after chemical mechanical polishing, the copper surface of cobalt as the barrier layer has pollution residues and galvanic corrosion problems, resulting in degradation of device performance and environmental pollution. The existing cleaning liquid has problems of environmental protection and high cost.

Method used

Using biodegradable polycarboxylic acid structure chelating agent and low concentration of fatty acid potential protector, combined with wetting agent, a cleaning solution for copper polishing is formed, and a solution is formed by ultrasonic stirring and pH adjustment, which is used to remove organic matter. and reduce the potential difference between copper and cobalt.

Benefits of technology

Effectively remove organic matter residues on the copper and cobalt surfaces, reduce the risk of galvanic corrosion, and improve the yield of the device. The cleaning liquid is environmentally friendly, avoiding the pollution of the environment by traditional cleaning liquids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978959A_ABST
    Figure CN118978959A_ABST
Patent Text Reader

Abstract

The invention relates to a cleaning solution for copper interconnection after polishing with cobalt as a barrier layer and a preparation method and application of the cleaning solution, and belongs to the technical field of cleaning after chemical mechanical polishing, and the cleaning solution comprises the following raw material components in percentage by mass: 0.04%-0.5% of a biodegradable chelating agent, 0.02%-0.5% of a wetting agent, 0.001%-0.2% of a potential protective agent and the balance of deionized water. Compared with the prior art, the method solves the problem that organic matters, abrasives and other pollution particles are left on the surface of a circuit after chemical mechanical polishing of copper in the manufacturing process of a large-scale high-density integrated circuit, improves the cleanliness of the polished surface of the copper wiring, reduces the galvanic corrosion risk between copper and cobalt in the cleaning process, and improves the service life of the large-scale high-density integrated circuit. A cleaner surface state is provided for subsequent processes, and the yield of chips is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of post-chemical mechanical polishing cleaning, and in particular to a post-polishing cleaning liquid for copper with cobalt as a barrier layer, and a preparation method and application thereof. Background Art

[0002] In the integrated circuit manufacturing industry, the chemical mechanical polishing (CMP) process can remove excess wiring metal overflowing from the wiring groove and achieve overall flatness of the wiring layer, barrier layer and wafer surface. However, the chemical reagent components such as abrasive particles, complexing agents, corrosion inhibitors, oxidants, pH adjusters, additives, etc. in the CMP polishing liquid will introduce contamination residues on the wafer surface after polishing. The presence of contamination residues will not only cause the adhesion of subsequent deposited layers to decrease, but also reduce the reliability of the device, resulting in a decrease in device yield and even safety issues. Therefore, based on the requirement to keep the surface clean after CMP to reduce the number of impurity defects, post-CMP cleaning is an indispensable step. The yield of electronic devices can be improved through the post-CMP cleaning process.

[0003] The main cleaning targets of post-CMP cleaning are organic matter, abrasive particles and other impurity ions. Benzotriazole BTA is a common corrosion inhibitor in copper and cobalt CMP processes and is widely used in the CMP process of metal surfaces. However, after CMP, BTA, as the main organic residue, will cause serious drying problems and poor adhesion to the stack due to its high hydrophobicity, which seriously affects the reliability of device performance. Therefore, it is extremely important to remove organic impurities BTA during the post-CMP cleaning process of copper and cobalt barrier layers.

[0004] Most of the chelates used in the market are chelated with amino structures, but amino compounds have a high vapor pressure and are easy to evaporate into the environment. In addition, ammonia substances can deteriorate the photolithography process in semiconductor manufacturing units. Therefore, in industrial applications, complex and costly filtration systems are required to remove these substances from clean room air, resulting in higher costs and more maintenance. Strong alkaline ammonia substances represented by TMAH may cause serious health problems if inhaled or absorbed through the skin. Therefore, the semiconductor industry prefers to use non-amino chemicals in all applications. At present, EDTA and its reaction products are widely used in polishing and cleaning because they can form stable water-soluble complexes with copper and cobalt ions. However, the release of EDTA into the environment will lead to the reactivation of metal ions and form a toxic environment. At the same time, it will also increase the nitrogen content and the solubility of phosphates in the environment, resulting in eutrophication of water quality. In addition, EDTA has poor degradability, which makes it easy to remain in the environment and cause long-term damage. Ecological safety has always been and will continue to be a concern. At present, increasingly stringent legislation has been proposed and implemented in China to control the emission of chelating agents such as EDTA in the environment and to find new eco-friendly and biodegradable chelating agents to replace traditional chelating agents that are unsafe for the environment. In addition, in most polishing and cleaning fluids, when cobalt is used as a barrier layer for interconnected copper, the electrode potential difference between copper and cobalt is relatively large (Cu 2+ / Cu and Co 2 + The standard equilibrium potentials of the copper / Co pair are +0.34V and -0.28V respectively. Post-polishing cleaning has the risk of galvanic corrosion, which reduces the service life and yield rate of integrated circuits. Therefore, how to make the post-polishing cleaning of copper interconnects with cobalt as a barrier layer more efficient, environmentally friendly and with lower surface quality damage is the main technical challenge currently. Summary of the invention

[0005] The purpose of the present invention is to provide a cleaning solution for copper post-polishing with cobalt as a barrier layer and its preparation method and application in order to overcome at least one of the defects of the above-mentioned prior art. Specifically, in order to solve the technical problem of cleaning copper interconnects after chemical mechanical polishing in the presence of a cobalt barrier layer, the present invention provides a green and environmentally friendly cleaning solution for removing copper after chemical mechanical polishing with cobalt as a barrier layer.

[0006] The present invention provides a cleaning liquid for cleaning copper after chemical mechanical polishing of high-density integrated circuits. One of the effective ingredients is a biodegradable chelating agent, which is an organic molecule with a polycarboxylic acid structure and has a good chelating effect on metals. The pollutants can be stripped from the copper and cobalt surfaces by the principle of root cutting to achieve the purpose of cleaning the pollutants. The addition of a wetting agent can reduce the surface tension of the solid-liquid surface, which is beneficial to the contact of the cleaning liquid with the copper and cobalt surfaces, and improves the cleaning effect and efficiency. The addition of a potential protective agent can selectively adsorb copper and cobalt to form a surface film to change the charge distribution of the interface, adjust the potential difference between copper and cobalt, and achieve the purpose of reducing the galvanic corrosion between copper and cobalt.

[0007] Long-chain fatty acids in existing cleaning solutions are mostly used as surfactants, but through our research we have found that low-concentration long-chain fatty acids have a good effect in adjusting the copper-cobalt potential difference and thus solving the copper-cobalt galvanic corrosion. The present invention selects fatty acids including but not limited to oleic acid, lauric acid, palmitic acid, and one or more of octadecyl fatty acids as potential protective agents.

[0008] In order to more gently and effectively remove organic contamination on the surface of the metal circuit, the present invention provides a chelating agent which is alkaline in itself and has an excellent cleaning effect, and can completely clean the organic residues on the surface.

[0009] The purpose of the present invention can be achieved by the following technical solutions:

[0010] One of the purposes of the present invention is to provide a cleaning solution for copper interconnect after polishing with cobalt as a barrier layer, which comprises the following raw material components by mass fraction: 0.04%-0.5% of a biodegradable chelating agent, 0.02%-0.5% of a wetting agent, 0.001%-0.2% of a potential protective agent, and the rest being deionized water.

[0011] Preferably, the cleaning solution of the present invention satisfies the following conditions: the mass fraction of the biodegradable chelating agent is preferably 0.10% to 0.3%; the mass fraction of the wetting agent is preferably 0.10% to 0.3%; the mass fraction of the potential protective agent is preferably 0.001% to 0.1%.

[0012] Furthermore, the chelating agent is selected from one or more of the biodegradable chelating agents tetrasodium iminodisuccinate, tetrasodium glutamate diacetate, methylglycine diacetic acid or ethylenediamine disuccinic acid.

[0013] Furthermore, the wetting agent is selected from one or more of anionic surfactant sodium secondary alkyl sulfonate series or nonionic surfactant fatty alcohol polyoxyethylene ether series.

[0014] Furthermore, the potential protective agent is a fatty acid potential protective agent. Preferably, the potential protective agent is selected from one or more of oleic acid, lauric acid, palmitic acid or octadecyl fatty acid.

[0015] The second object of the present invention is to provide a method for preparing a copper interconnect post-polishing cleaning solution with cobalt as a barrier layer as described above, comprising the following steps: adding a biodegradable chelating agent, a wetting agent and a potential protective agent to deionized water, stirring the solution uniformly by ultrasonic stirring, and then adjusting the pH value of the solution to alkaline with a pH regulator to obtain a copper interconnect post-polishing cleaning solution with cobalt as a barrier layer.

[0016] Furthermore, the pH regulator is sodium hydroxide; after adding the pH regulator, the pH of the solution is adjusted to 10-11.

[0017] The third object of the present invention is to use the above-mentioned cleaning solution for cleaning copper interconnects after polishing with cobalt as a barrier layer, characterized in that the cleaning solution is used for cleaning copper interconnects after chemical mechanical polishing with cobalt as a barrier layer.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] (1) The present invention solves the problem of residual organic matter, abrasives and other contaminant particles on the surface of the circuit after copper chemical mechanical polishing in the process of large-scale high-density integrated circuit manufacturing, improves the cleanliness of the surface of the copper wiring after polishing, solves the problem of residual contaminants on the surface of the copper wiring, provides a cleaner surface state for subsequent processes, and improves the yield rate of chips.

[0020] (2) The present invention solves the problem of galvanic corrosion between copper and cobalt during the cleaning process. The fatty acid carbon chain used can selectively adsorb with copper and cobalt to form an isolation film covering the metal surface, thereby reducing the potential difference between copper and cobalt, reducing the risk of galvanic corrosion between copper and cobalt during the cleaning process, and eliminating the problem of corrosion pits caused by potential corrosion.

[0021] (3) The chelating agent and surfactant used in the present invention are biodegradable organic substances, which are friendly to the environment and ecology, and avoid the problem that traditional strong acids and strong bases are prone to environmental pollution. At the same time, the formula in the cleaning solution is a non-amino compound, which avoids the impact on the photolithography process and subsequent processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the working process of the cleaning solution for copper interconnect after polishing using cobalt as a barrier layer according to the present invention;

[0023] Figure 2 This is a corrosion current density diagram of clean copper-cobalt and contaminated copper-cobalt in sodium sulfate solution in the present invention. DETAILED DESCRIPTION

[0024] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented under the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. If specific conditions are not specified, proceed according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0025] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0026] The invention provides a cleaning liquid for copper interconnection after polishing with cobalt as a barrier layer, comprising the following raw material components in mass fraction: 0.04%-0.5% of a biodegradable chelating agent, 0.02%-0.5% of a wetting agent, 0.001%-0.2% of a potential protective agent, and the rest being deionized water.

[0027] Preferably, the mass fraction of the biodegradable chelating agent is preferably 0.10% to 0.3%; the mass fraction of the wetting agent is preferably 0.10% to 0.3%; and the mass fraction of the potential protective agent is preferably 0.001% to 0.1%.

[0028] In some embodiments of the present invention, the chelating agent is selected from one or more of the biodegradable chelating agents tetrasodium iminodisuccinate, tetrasodium glutamate diacetate, methylglycine diacetic acid or ethylenediamine disuccinic acid.

[0029] In some embodiments of the present invention, the wetting agent is selected from one or more of the anionic surfactant sodium secondary alkyl sulfonate series or the nonionic surfactant fatty alcohol polyoxyethylene ether series, preferably one or more of sodium secondary alkyl sulfonate, hexadecanol polyoxyethylene ether or tetradecyl alcohol polyoxyethylene ether.

[0030] In some embodiments of the present invention, the potential protective agent is a fatty acid potential protective agent. Preferably, the potential protective agent is selected from one or more of oleic acid, lauric acid, palmitic acid or octadecyl fatty acid.

[0031] The present invention also provides a method for preparing the copper interconnect post-polishing cleaning solution with cobalt as a barrier layer as described above, comprising the following steps: adding a biodegradable chelating agent, a wetting agent and a potential protective agent into deionized water, stirring evenly to form a solution, and then adjusting the pH value of the solution to alkaline with a pH regulator to obtain the copper interconnect post-polishing cleaning solution with cobalt as a barrier layer. Figure 1 This is a schematic diagram of the working of the cleaning fluid.

[0032] Wherein, the pH adjuster is sodium hydroxide. After adding the pH adjuster, the pH of the solution is adjusted to 10-11.

[0033] The following is the sample processing of each embodiment and comparative example: the experiment uses copper sheets and cobalt sheets (purity of 99.995%) as samples. First, the clean and oil-free copper and cobalt are treated to remove the oxide film (the metal sheets are immersed in a 25mM citric acid solution for 5 minutes), then washed with deionized water and dried with N2 to define them as clean copper sheets and clean cobalt sheets.

[0034] In order to simulate the adsorption of organic matter during mechanical polishing, the clean sample was immersed in a 15 mM benzotriazole (BTA) solution for 10 min to contaminate the sample with BTA. The contaminated copper and cobalt were used as the experimental sample after polishing.

[0035] The following comparative examples and examples use the corrosion current density data of the samples in a neutral sodium sulfate environment to characterize the cleaning effect. First, the corrosion current (I0) of the clean sample is tested, and then the corrosion current (I s ) Then the copper-cobalt samples after the contaminated samples were cleaned with different cleaning solutions were used as electrodes to test the corrosion current (I c ). Will (I c -I s ) / (I0-I s ) as a cleaning fluid for cleaning effect.

[0036] The test method for corrosion current density is: using a saturated calomel electrode as a reference electrode, a platinum electrode as an auxiliary electrode, and copper or cobalt as a working electrode, respectively, and performing a Tafel polarization curve test in a neutral sodium sulfate solution under this three-electrode system. Figure 2 The Tafel curves of clean and contaminated samples are shown in Table 1. The calculated corrosion current density of clean copper and cobalt electrodes is shown in Table 1. Obviously, the corrosion current of copper-cobalt sheet is significantly reduced after being contaminated by BTA, indicating that BTA has contaminated the copper-cobalt surface.

[0037] The galvanic corrosion in the following comparative examples and specific embodiments is represented by the corrosion potential difference between copper and cobalt in the cleaning solution. The specific test method is: using a saturated calomel electrode as a reference electrode, a platinum electrode as an auxiliary electrode, and copper or cobalt as a working electrode, a Tafel curve test is performed in the cleaning solution under the three-electrode system to obtain the corrosion potential of the copper-cobalt electrode. corr,Cu -E corr,Co ) to determine whether there is a risk of galvanic corrosion of copper and cobalt in the cleaning solution. In the high-density integrated circuit process, if the metal potential difference between the interconnect layer and the barrier layer exceeds 20mV, it can be considered that there is a galvanic corrosion problem between the two.

[0038] Comparative Example 1;

[0039] Take 90g of deionized water, add 0.5g of sodium secondary alkyl sulfonate surfactant to the deionized water and stir to dissolve it, then add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The surfactant concentration in the solution is 0.5wt%.

[0040] The copper and cobalt sheets contaminated by BTA were immersed in the cleaning solution for cleaning, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be observed that the corrosion current density is slightly higher than that of the copper and cobalt after contamination, but compared with the corrosion current density of clean copper and clean cobalt, it is much lower than that of clean copper and cobalt, proving that the surface surfactant has a certain effect on removing organic pollution, but the cleaning is not thorough and some residues are still there. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 320.4mV, and the risk of galvanic corrosion is high.

[0041] Comparative Example 2;

[0042] Take 90g of deionized water, add 0.25g of tetrasodium glutamic acid diacetate chelating agent and 0.5g of secondary alkyl sodium sulfonate surfactant to the deionized water, stir to dissolve, then add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelating agent in the solution is 0.25wt%, and the concentration of the surfactant is 0.5wt%.

[0043] The copper sheet and cobalt sheet contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increases after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. Compared with the corrosion current density of clean copper and clean cobalt, it can be seen that after the Cu and Co electrodes are cleaned with the cleaning solution of Comparative Example 2, the corrosion current density of the Cu and Co electrode surfaces is greater than the corrosion current density of clean cobalt in the solution, and it is believed that the organic matter on the surface of Cu and Co has been completely cleaned at this time. The presence of a surface chelating agent has a good effect on the removal of organic contamination.

[0044] Comparing Comparative Example 2 with Comparative Example 1, it can be seen that the presence or absence of a chelating agent in the cleaning solution has a great influence on the cleaning effect. At this time, the potential difference between copper and cobalt in the cleaning solution increases to 570mV, indicating that the removal of organic matter on the sample surface increases the tendency of galvanic corrosion between metals.

[0045] Comparative Example 3:

[0046] Take 90g of deionized water, add 0.25g of tetrasodium glutamic acid diacetate chelating agent and 0.5g of sodium secondary alkyl sulfonate surfactant to the deionized water and stir to dissolve, add 0.02g of oleic acid potential protective agent to a beaker while stirring, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.25wt%, the concentration of the surfactant is 0.5wt%, and the concentration of the potential protective agent is 0.02wt%.

[0047] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. Compared with the corrosion current density of clean copper and clean cobalt, it can be seen that after the Cu and Co electrodes are cleaned with the cleaning solution of Comparative Example 3, the corrosion current density of the Cu and Co electrode surfaces is greater than the corrosion current density of the clean sample in the solution, and it is believed that the organic matter on the surface of Cu and Co has been completely cleaned at this time.

[0048] It was observed that the potential difference between copper and cobalt in the cleaning solution was 15mV. In the high-density integrated circuit process, the metal potential difference between the interconnect layer and the barrier layer exceeds 20mV, which can be considered to be a galvanic corrosion problem between the two. Therefore, in the presence of a potential inhibitor, the galvanic corrosion problem between copper and cobalt is greatly improved.

[0049] Comparative Example 4;

[0050] Take 90g of deionized water, add 0.02g of tetrasodium glutamic acid diacetate chelating agent and 0.5g of secondary alkyl sodium sulfonate surfactant to the deionized water and stir to dissolve, add 0.02g of oleic acid potential protective agent to a beaker while stirring, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.02wt%, the concentration of the surfactant is 0.5wt%, and the concentration of the potential protective agent is 0.02wt%.

[0051] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased slightly after cleaning with the cleaning agent, but compared with the corrosion current density of clean copper and clean cobalt, it can be seen that after the Cu and Co electrodes were cleaned with the cleaning solution of Comparative Example 4, the corrosion current density of the Cu and Co electrode surfaces was much smaller than the corrosion current density of the clean samples in the solution. It is believed that the organic matter on the surface of Cu and Co was not cleaned at this time, and the chelating agent with a lower concentration could not achieve the purpose of cleaning the organic matter.

[0052] Comparative Example 5;

[0053] Take 90g of deionized water, add 0.70g of tetrasodium glutamic acid diacetate chelating agent and 0.5g of sodium secondary alkyl sulfonate surfactant to the deionized water and stir to dissolve, add 0.02g of oleic acid potential protective agent to a beaker while stirring, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.7%, the concentration of the surfactant is 0.5wt%, and the concentration of the potential protective agent is 0.02wt%.

[0054] The copper and cobalt sheets contaminated by BTA were soaked in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased slightly after cleaning with a cleaning agent, but compared with the corrosion current density of clean copper and clean cobalt, it can be seen that after the Cu and Co electrodes were cleaned with the cleaning solution of Comparative Example 4, the corrosion current density of the Cu and Co electrode surfaces was less than the corrosion current density of the clean samples in the solution. We analyzed this result and found that when the concentration is too high, GLDA will hydrolyze and adsorb on the metal surface, which will not only cause local pits on the metal surface, but also easily cause residues on the metal surface. Therefore, the concentration of GLDA is not easy to be too high, and the cleaning purpose can be achieved at a lower concentration, saving production costs.

[0055] Embodiment 1:

[0056] Take 90g of deionized water, add 0.25g of tetrasodium glutamic acid diacetate chelating agent, 0.5g of sodium secondary alkyl sulfonate surfactant and 0.02g of oleic acid potential protective agent into the deionized water in a beaker, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.25%, the concentration of the surfactant is 0.5wt%, and the concentration of the potential protective agent is 0.02wt%.

[0057] The copper and cobalt sheets contaminated by BTA were soaked in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated copper and cobalt electrodes were placed in a three-electrode system for electrochemical testing. The Tafel curves were tested, and the test results are shown in Table 1. Compared with Comparative Example 1, it can be seen that the corrosion current increased, indicating that the organic contamination on the metal surface was washed away. The potential difference between the two in the cleaning solution was 13.2mV, which was compared with Comparative Example 2, indicating that the galvanic corrosion problem between copper and cobalt was also improved in the cleaning solution formula.

[0058] Embodiment 2:

[0059] Take 90g of deionized water, add 0.22g of methylglycine diacetic acid chelating agent, 0.5g of secondary alkyl sodium sulfonate surfactant and 0.02g of oleic acid in the deionized water in a beaker, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.22%, the concentration of the surfactant is 0.5%, and the concentration of the potential protective agent is 0.02%.

[0060] The copper and cobalt sheets contaminated by BTA were soaked in an alkaline cleaning solution for cleaning, dried with nitrogen after treatment, and the treated copper and cobalt electrodes were placed in a three-electrode system for electrochemical testing. The Tafel curves were tested, and the test results are shown in Table 1. Compared with Comparative Example 1, it can be seen that the corrosion current increased, indicating that the organic contamination on the metal surface was washed away. The potential difference between the two in the cleaning solution was 9.82mV, which was compared with Comparative Example 2, indicating that the galvanic corrosion problem between copper and cobalt was also improved in the cleaning solution formula.

[0061] Embodiment 3:

[0062] Take 90g of deionized water, add 0.28g of tetrasodium iminodisuccinate chelating agent, 0.5g of sodium secondary alkyl sulfonate surfactant and 0.02g of oleic acid potential protective agent into the deionized water in a beaker, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.28wt%, the concentration of the surfactant is 0.5wt%, and the concentration of the potential protective agent is 0.02wt%.

[0063] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated copper and cobalt electrodes were placed in a three-electrode system for electrochemical testing. The test results are shown in Table 1. Compared with the comparative example 1, the Tafel curve shows that the corrosion current increases, indicating that the organic contamination on the metal surface has been cleaned. The potential difference between the two in the cleaning solution is 16.3mV, which is compared with the comparative example 2, indicating that the galvanic corrosion problem between copper and cobalt is also improved in the cleaning solution formula.

[0064] Embodiment 4:

[0065] Take 90g of deionized water, add 0.04g of tetrasodium iminodisuccinate chelating agent, 0.5g of sodium secondary alkyl sulfonate surfactant and 0.2g of oleic acid potential protective agent into the deionized water in a beaker, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to prepare a cleaning solution. The concentration of the chelate in the solution is 0.04wt%, the concentration of the surfactant is 0.5wt%, and the concentration of the potential protective agent is 0.2wt%.

[0066] The copper and cobalt sheets contaminated by BTA were soaked in the cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is -20.4mV, and the corrosion caused by the potential difference between copper and cobalt is effectively suppressed.

[0067] Embodiment 5:

[0068] Take 90g of deionized water, add 0.1g of tetrasodium glutamic acid diacetate chelating agent, 0.1g of hexadecanol polyoxyethylene ether surfactant and 0.1g of lauric acid potential protective agent into the deionized water in a beaker, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to prepare a cleaning solution. The concentration of the chelate in the solution is 0.1wt%, the concentration of the surfactant is 0.1wt%, and the concentration of the potential protective agent is 0.1wt%.

[0069] The copper and cobalt sheets contaminated by BTA were soaked in the cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is -7.5mV. At this time, the potential of cobalt is more positive than that of copper. It can be seen that in this cleaning solution, the corrosion caused by the potential difference between copper and cobalt is effectively suppressed.

[0070] Embodiment 6:

[0071] Take 90g of deionized water, add 0.5g of methylglycine diacetic acid chelating agent, 0.02g of secondary alkyl sodium sulfonate surfactant and 0.01g of palmitic acid potential protective agent into the deionized water in a beaker, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to prepare a cleaning solution. The concentration of the chelate in the solution is 0.5wt%, the concentration of the surfactant is 0.02wt%, and the concentration of the potential protective agent is 0.01wt%.

[0072] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 19.2mV, which is further reduced compared to the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0073] Embodiment 7:

[0074] Take 90g of deionized water, add 0.2g of ethylenediamine disuccinic acid chelating agent, 0.1g of tetradecyl alcohol polyoxyethylene ether surfactant and 0.001g of octadecyl fatty acid potential protective agent into the deionized water in a beaker, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to prepare a cleaning solution. The concentration of the chelate in the solution is 0.2wt%, the concentration of the surfactant is 0.1wt%, and the concentration of the potential protective agent is 0.001wt%.

[0075] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 20.3mV, which is further reduced compared with the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0076] Embodiment 8:

[0077] Take 90g of deionized water, add 0.2g of ethylenediamine disuccinic acid, 0.1g of tetrasodium iminodisuccinate chelating agent, 0.1g of sodium secondary alkyl sulfonate, 0.1g of tetradecyl alcohol polyoxyethylene ether surfactant, 0.003g of octadecyl fatty acid and 0.004g of oleic acid into the deionized water in a beaker, stir to dissolve them, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.3wt%, the concentration of the surfactant is 0.2wt%, and the concentration of the potential protective agent is 0.007wt%.

[0078] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 17.4mV, which is further reduced compared to the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0079] Embodiment 9:

[0080] Take 90g of deionized water, add 0.1g of tetrasodium glutamate diacetate, 0.1g of tetrasodium iminodisuccinate chelating agent, 0.2g of sodium secondary alkyl sulfonate, 0.1g of tetradecyl alcohol polyoxyethylene ether surfactant, 0.003g of octadecyl fatty acid and 0.0005g of oleic acid into the deionized water in a beaker, stir to dissolve them, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.2wt%, the concentration of the surfactant is 0.3wt%, and the concentration of the potential protective agent is 0.0035wt%.

[0081] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 18.4mV, which is further reduced compared with the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0082] Embodiment 10:

[0083] Take 90g of deionized water, add 0.15g of methylglycine diacetic acid, 0.1g of tetrasodium iminodisuccinate chelating agent, 0.1g of sodium secondary alkyl sulfonate, 0.1g of tetradecyl alcohol polyoxyethylene ether surfactant, 0.003g of octadecyl fatty acid and 0.004g of oleic acid into the deionized water in a beaker, stir to dissolve them, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.25wt%, the concentration of the surfactant is 0.2wt%, and the concentration of the potential protective agent is 0.007wt%.

[0084] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 16.3mV, which is further reduced compared to the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0085] Embodiment 11:

[0086] Take 90g of deionized water, add 0.25g of methylglycine diacetic acid, 0.1g of glutamic acid diacetic acid tetrasodium, 0.1g of secondary alkyl sulfonate sodium, 0.1g of tetradecyl alcohol polyoxyethylene ether surfactant, 0.003g of octadecyl fatty acid and 0.004g of oleic acid in a beaker, stir to dissolve them, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.35wt%, the concentration of the surfactant is 0.2wt%, and the concentration of the potential protective agent is 0.007wt%.

[0087] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 7.2mV, which is further reduced compared to the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0088] Embodiment 12:

[0089] Take 90g of deionized water, add 0.25g of ethylenediamine disuccinic acid, 0.1g of tetrasodium glutamate diacetate, 0.1g of sodium secondary alkyl sulfonate, 0.1g of tetradecyl alcohol polyoxyethylene ether surfactant, 0.003g of octadecyl fatty acid and 0.004g of oleic acid into the deionized water in a beaker, stir to dissolve them, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.35wt%, the concentration of the surfactant is 0.2wt%, and the concentration of the potential protective agent is 0.007wt%.

[0090] The copper and cobalt sheets contaminated by BTA were immersed in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 5.6mV, which is further reduced compared with the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0091] Embodiment 13:

[0092] Take 90g of deionized water, add 0.4g of methylglycine diacetic acid, 0.1g of glutamic acid diacetic acid tetrasodium, 0.1g of secondary alkyl sulfonate sodium, 0.1g of tetradecyl alcohol polyoxyethylene ether surfactant, 0.003g of octadecyl fatty acid and 0.004g of oleic acid into the deionized water in a beaker, stir to dissolve them, add deionized water to prepare the solution to 100g, and then use sodium hydroxide to adjust the pH of the solution to 11 to obtain a cleaning solution. The concentration of the chelate in the solution is 0.5%, the concentration of the surfactant is 0.2%, and the concentration of the potential protector is 0.007%.

[0093] The copper and cobalt sheets contaminated by BTA were soaked in a cleaning solution for cleaning, dried with nitrogen after treatment, and the treated samples were used as electrodes for Tafel curve test. The data are listed in Table 1. Compared with the corrosion current density of the copper and cobalt surfaces after contamination, it can be seen that the corrosion current density of the copper and cobalt surfaces increased after cleaning with the cleaning agent, indicating that the organic contamination on the metal surface has been cleaned. In this cleaning solution, the difference in the self-corrosion potential of copper and cobalt is 8.3mV, which is further reduced compared to the potential difference between copper and cobalt in Comparative Example 2, and the galvanic corrosion problem between copper and cobalt has been alleviated.

[0094] Table 1 Cleaning efficiency and potential difference of copper and cobalt after treatment in comparative examples and embodiments

[0095]

[0096]

[0097] From Table 1, it can be seen that a single chelating agent, surfactant and potential protective agent can also achieve the cleaning effect and potential protection effect. However, when the above-mentioned active ingredients are compounded, compared with a single chelating agent, surfactant and potential protective agent, under the compounding conditions, due to the different structures, the steric hindrance between the same structures is reduced, thereby having better contact with the copper-cobalt surface, and the cleaning purpose can be achieved at a lower concentration.

[0098] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A cleaning solution for copper interconnects after polishing with cobalt as a barrier layer, characterized in that: The invention comprises the following raw material components in mass fractions: 0.04%-0.5% of a biodegradable chelating agent, 0.02%-0.5% of a wetting agent, 0.001%-0.2% of a potential protective agent, and the rest being deionized water.

2. A post-polishing cleaning solution for copper interconnects using cobalt as a barrier layer according to claim 1, characterized in that: The cleaning solution satisfies at least one of the following conditions: ① The mass fraction of the biodegradable chelating agent is preferably 0.10% to 0.3%; ② The mass fraction of the wetting agent is preferably 0.10% to 0.3%; ③ The mass fraction of the potential protection agent is preferably 0.001% to 0.1%.

3. The cleaning solution for copper interconnect after polishing with cobalt as a barrier layer according to claim 1, characterized in that: The chelating agent is selected from one or more of the biodegradable chelating agents tetrasodium iminodisuccinate, tetrasodium glutamate diacetate, methylglycine diacetic acid or ethylenediamine disuccinic acid.

4. The cleaning solution for copper interconnect after polishing with cobalt as a barrier layer according to claim 1, characterized in that: The wetting agent is selected from one or more of the biodegradable anionic surfactant sodium secondary alkyl sulfonate series or the nonionic surfactant fatty alcohol polyoxyethylene ether series.

5. The cleaning solution for copper interconnect after polishing with cobalt as a barrier layer according to claim 1, characterized in that: The potential protective agent is a fatty acid potential protective agent.

6. The cleaning solution for copper interconnect after polishing with cobalt as a barrier layer according to claim 1, characterized in that: The potential protective agent is selected from one or more of oleic acid, lauric acid, palmitic acid or octadecyl fatty acid.

7. A method for preparing a cleaning solution for copper interconnect after polishing with cobalt as a barrier layer as claimed in any one of claims 1 to 6, characterized in that: The method comprises the following steps: adding a biodegradable chelating agent, a wetting agent and a potential protecting agent into deionized water, uniformly stirring with ultrasonic wave to form a solution, and then adjusting the pH value of the solution to alkaline with a pH adjusting agent to obtain a copper interconnect post-polishing cleaning solution with cobalt as a barrier layer.

8. The cleaning solution for copper interconnect after polishing with cobalt as a barrier layer according to claim 7, characterized in that: The pH regulator is sodium hydroxide.

9. The method for preparing a cleaning solution for copper interconnect after polishing with cobalt as a barrier layer according to claim 7, characterized in that: The pH of the solution is 10-11.

10. A use of a cleaning solution for copper interconnect after polishing using cobalt as a barrier layer as claimed in any one of claims 1 to 6, characterized in that: The cleaning solution is used for cleaning copper interconnects after chemical mechanical polishing using cobalt as a barrier layer.