Curved composite elastic fiber, preparation method and spinning assembly

The two-component composite spinning technology forms axially rotating fibers, which solves the problem of insufficient hygroscopic properties of chemical fibers, realizes the bionic structure of the fibers, improves the curling and hygroscopic properties, and is suitable for a variety of weaving processes.

CN118979309AActive Publication Date: 2024-11-19JIANGSU ZJA NEW MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411036869.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Chemical fibers are inferior to cotton fibers in terms of moisture absorption, and it is difficult to simulate the continuous radial thickness and twisting structure of cotton fibers, affecting the overall performance of their fabrics.

Method used

Using two-component composite spinning technology, by melting polyester fiber-forming polymers with different heat shrink properties, composite spinning is used to form axial rotating fibers, forming a continuous rotating groove structure. Improves the curling and hygroscopic properties of the fiber.

Benefits of technology

It realizes the bionic structure of chemical fibers, improves the curling performance, conformal performance and wicking and sweating function of the fibers. It has a full feel, smooth and delicate, and is suitable for a variety of weaving processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979309A_ABST
    Figure CN118979309A_ABST
Patent Text Reader

Abstract

The invention discloses a curved composite elastic fiber, a preparation method and a spinning assembly, and relates to the technical field of composite fibers.The preparation method comprises the steps that after a first polyester fiber-forming high polymer and a second polyester fiber-forming high polymer are fused respectively, composite spinning is conducted through a bi-component composite spinning assembly, the two components with different thermal shrinkage properties respectively pass through respective independent spinning guide holes, and are finally bonded and compounded in a reverse tangent manner to form the rotating curved composite fiber. The composite spinning assembly and the spinneret plate which are reversely tangent left and right on the composite circumference are adopted, melt is in a tangential rotation state after being composited, the effect of a bend angle can be reduced, and filaments are prevented from being attached to the spinneret plate. The preparation process is simple, the flow is convenient, and the prepared curved composite elastic fiber has excellent curling performance, shape preserving performance and wicking and perspiration functions, feels full, smooth and fine after being woven, and can meet the requirements of weaving and knitting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite fibers, and in particular to a twisted composite elastic fiber, a preparation method, a spinning assembly and application of the bionic fiber on fabrics. Background Art

[0002] The conventional process for curling chemical staple fibers is to subject the fiber bundles to mechanical extrusion in a curling box under high temperature and humidification (oil spraying) to curl. This results in a planar zigzag curl with poor curl elasticity and difficult to maintain curl shape. Later, when studying the microstructure of wool, it was found that the cross-section of wool fibers is a two-component structure. The fibrils, crystalline regions, and amorphous regions in the two components are different in properties and arrangement, resulting in shrinkage differences, forcing the wool to curl in a spiral shape. Inspired by this, researchers designed a novel composite spinning process to develop parallel two-component composite fibers, which produce spiral three-dimensional curls after heat shrinkage. This technology has been widely used in PET-PTT composite curled fibers.

[0003] In addition, under single-screw spinning conditions, by changing the spinning process and adopting an asymmetric cooling method for the primary yarn to make the thermal shrinkage of the cortex and core layer different, three-dimensional curly fibers can also be produced. This kind of curly fiber has a memory effect and the curly shape is long-lasting. For example, when the fiber is damp, the number of curls decreases, but it can be restored after drying. The three-dimensional curly fiber has stronger fluffiness and warmth retention, a more comfortable feel, and improves the cohesion during fiber processing and the dimensional stability of the fabric.

[0004] Compared with conventional fibers, parallel composite elastic fibers have excellent three-dimensional curling elasticity, excellent bulkiness and soft feel, and have been greatly developed.

[0005] Although the above technical improvements have improved the wearing comfort of chemical fibers, they are still much inferior to cotton fibers, especially the moisture absorption performance has not been improved. In contrast, cotton fibers are a kind of plant that has a structure with natural turning and hollow grooves due to the different growth rates in different growth periods.

[0006] The longitudinal morphology of cotton fibers is characterized by being flat, and all of them are in the form of bundles of small fibers that are inclined to the fiber axis in a spiral shape and rotate along the length of the fiber. The cross section of cotton fibers is composed of many concentric layers, mainly primary layer, secondary layer, and middle cavity. Different layers have different thicknesses, forming a natural continuous radial thickness and change in direction. The comprehensive performance of cotton fiber fabrics, in addition to its cellulose component, is more importantly its continuous radial thickness and change in direction structure, and the chemical fiber structure bionic cotton fiber is the goal that technicians in this field have been striving to achieve. Summary of the invention

[0007] The purpose of the present invention is to solve the above technical problems and provide a twisted composite elastic fiber, a preparation method and a spinning assembly to achieve the bionics of the chemical fiber structure.

[0008] In order to achieve the above technical objectives and meet the above technical requirements, the technical solution adopted by the present invention is: a method for preparing a twisted composite elastic fiber, characterized in that it comprises the following steps: Step 1: The first polyester fiber-forming polymer and the second polyester fiber-forming polymer, two compatible fiber-forming polymers with different heat shrinkage, are melted separately to obtain a first melt A and a second melt B; the melting temperature of the polyester fiber-forming polymer is determined according to the melting point and viscosity of each polyester fiber-forming polymer. Generally, the melting temperature is higher than the melting point of the polyester fiber-forming polymer by more than 30°C. In order to improve the fluidity of the polyester fiber-forming polymer with high viscosity, the melting temperature can be further increased by 3-8°C.

[0009] Step 2: The first melt A and the second melt B obtained in step 1 are subjected to composite spinning using a two-component composite spinning assembly; the first melt A and the second melt B are respectively introduced into the feed plate of the composite spinning assembly at a mass ratio of 4:6 to 6:4, enter the first melt A inlet and the second melt B inlet on the spinneret through their respective melt channels, and pass through their respective oblique spinneret guide holes, tapered holes and spinneret microholes, and finally composite at the melt composite circumference; during the composite process, the two melts are tangent to each other in opposite directions on the melt composite circumference, and the intersecting part accounts for 1 / 4-3 / 4 of the total amount of the melts, and the obtained fiber is in a state of axial rotation; The two-component composite spinning assembly comprises an assembly shell, in which a feed plate, a sealing gasket, a sand pool, a filter screen, an upper distribution plate, a lower distribution plate and a spinneret are sequentially arranged along the melt flow direction. Two melt channels are arranged on the feed plate, and each melt distribution channel on the upper distribution plate is evenly provided with 4-8 countersunk holes to send the melt to the annular distribution channel on the lower distribution plate, and each melt annular distribution channel on the lower distribution plate is provided with paired countersunk holes with the same number as the composite spinneret holes, and the paired countersunk holes correspond to The first melt A feed port is connected to the oblique spinneret guide hole assembly A, and the second melt B feed port is connected to the oblique spinneret guide hole assembly B. The plane projections of the spinneret guide hole assembly A, the spinneret guide hole assembly B and the spinneret are in opposite directions on the melt composite circumference. The angle α between the spinneret guide hole assembly A, the spinneret guide hole assembly B and the spinneret main projection is 60°-120°, and the melt composite circumference diameter is 1-2 times the diameter of the spinneret microhole. Step 3: The spun fiber obtained in step 2 is subjected to ring-blowing cooling and oiling in sequence, and is wound after adjusting the tension through a pair of guide wire discs to obtain pre-stretched twisted elastic fiber (POY), which is then stretched by a texturing machine to obtain a permanent twisted elastic fiber.

[0010] Preferably: the spinneret guide hole assembly A comprises a spinneret guide hole A, a conical hole A, and a spinneret microhole A which are connected in sequence and are axially symmetrical, and the center lines of the spinneret guide hole A, the conical hole A, and the spinneret microhole A are in a straight line; the spinneret guide hole assembly B comprises a spinneret guide hole B, a conical hole B, and a spinneret microhole B which are connected in sequence and are axially symmetrical, and the center lines of the spinneret guide hole B, the conical hole B, and the spinneret microhole B are in a straight line.

[0011] Preferably, the melt compounding circle is arranged inside the spinneret, and is 0.2-0.5 mm away from the lower plane of the spinneret.

[0012] Preferably, the melt compounding circle is arranged on the lower plane of the spinneret.

[0013] Preferably, the melt compounding circle is arranged outside the spinneret, and is 0.2-0.5 mm away from the lower plane of the spinneret.

[0014] A twisted composite elastic fiber is obtained by the above-mentioned preparation method, and is composed of a first polyester fiber-forming polymer and a second polyester fiber-forming polymer with different heat shrinkage properties, and the fiber axis is in a twisted and rotated state; it has a groove structure, and the width of the groove is 1 / 2-1 / 4 of the fiber diameter; the mass ratio of the first polyester fiber-forming polymer to the second polyester fiber-forming polymer is 1:1, and the viscosity difference between the first polyester fiber-forming polymer and the second polyester fiber-forming polymer is more than 0.3dl / g.

[0015] The invention discloses an application of twisted composite elastic fiber in fabrics, including making fiber aggregates alone such as woven fabrics for underwear, shirts, sportswear, home clothes, etc., and also mixing with other fibers to make blended fabrics.

[0016] The present invention adopts a double-channel composite spinneret, a distribution plate is provided with melt channels of component A and component B, and the spinneret is provided with melt feed ports and spinneret guide hole assemblies of component A and component B respectively, the two-component melt spinneret guide holes, tapered holes and spinneret micropores are in a straight line, and the spinneret guide hole assembly A and the spinneret guide hole assembly B are non-axisymmetrically inclined and do not interpenetrate each other. Below the spinneret guide hole and the tapered hole are two spinneret micropores with the same or different diameters, and their projections are tangent to each other in the left and right directions on the composite circumference. After the two-component melt flows through the respective spinneret guide holes, tapered holes and spinneret micropores and is ejected, it converges and bonds along the composite circumference to form a rotating curved composite fiber.

[0017] After studying the morphology of the twisted composite fiber, the inventor surprisingly found that the rotating twisted composite fiber would form a continuous rotating groove structure during the asymmetric cooling process, and the groove structure had an obvious capillary wicking effect.

[0018] The surface of the spun silk obtained by the present invention has a continuous and twisted groove structure, which can further improve the curling performance of the composite elastic fiber.

[0019] Compared with the traditional structure, the invention has the following beneficial effects: 1. The present invention has a novel structure and a reasonable design. It adopts two sets of oblique melt channels that are not connected to each other. Two components with different heat shrinkage properties pass through their own independent spinneret guide holes respectively, and are finally bonded and compounded in a reverse tangential manner to form a rotating twisted composite fiber. The bonding and compounding positions can be set at three positions, namely, inside the spinneret, on the lower plane of the spinneret, and below the lower plane of the spinneret, according to the different melt viscosities, to achieve the best rotating compounding effect.

[0020] 2. The present invention adopts a composite circular design, and the melt is in a tangential rotation state after compounding, which can reduce the effect of the bend angle and prevent the filaments from adhering to the spinneret. It solves the problem that when using melts with different viscosities to spin elastic composite fibers, the difference in the viscosity of the two melts is large. When the two melts are directly compounded, the elbow angle phenomenon is easy to occur when the melt exits the spinneret, and the filaments adhere to the spinneret, causing the filament bundles to stick together, affecting the quality of the filaments, and in severe cases, continuous spinning cannot be achieved.

[0021] 3. The preparation method provided by the present invention has a simple process and a convenient flow. The prepared twisted composite elastic fiber has excellent curling performance, shape retention performance and wicking function. After weaving, it feels full, smooth and delicate, and can meet the requirements of weaving and knitting. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the structure of the spinning assembly of the present invention; Figure 2 It is a schematic diagram of the top view of the spinneret structure of the present invention; Figure 3 It is a schematic diagram of the plane projection of the oblique spinneret guide hole assembly of the present invention; Figure 4 This is one of the relative position projection diagrams of the composite spinneret of the present invention; Figure 5 This is the second projection diagram of the relative position of the composite spinneret of the present invention; Figure 6 This is the third projection diagram of the relative position of the composite spinneret of the present invention; In the figure: 1. component housing, 2. feed plate, 3. sealing gasket, 4. sand pool, 5. filter screen, 6. upper distribution plate, 7. lower distribution plate, 8. spinneret, 9. first melt A feed port, 10. second melt B feed port, 11. melt compound circle, 12. spinneret guide hole A, 13. conical hole A, 14. spinneret microhole A. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with the accompanying drawings.

[0024] A method for preparing a twisted composite elastic fiber, comprising polyethylene terephthalate (PTT) as a first polyester fiber-forming polymer and polyethylene terephthalate (PET) as a second polyester fiber-forming polymer, wherein the viscosity of PTT is 1.05 dL / g and the viscosity of PET is 0.64 dL / g; further comprising thickened polyethylene terephthalate (PET) as the first polyester fiber-forming polymer and un-tackified polyethylene terephthalate (PET) as the second polyester fiber-forming polymer, wherein the viscosity of the thickened PET is 0.95 dL / g and the viscosity of the PET is 0.64 dL / g; It also includes modified polyethylene terephthalate as the first polyester fiber-forming polymer and unmodified polyethylene terephthalate as the second polyester fiber-forming polymer, wherein the modified polyethylene terephthalate is modified with a thermoplastic elastomer, wherein the mass percentage of the thermoplastic elastomer is 1-10%, preferably 2-8%, and more preferably 2.5-6%, and the viscosity after modification is 0.95-1.15 dL / g.

[0025] The preparation method of the thermoplastic elastomer modified polyethylene terephthalate preferably comprises melt blending a thermoplastic elastomer (TPEE) and polyethylene terephthalate (PET) and then extruding to obtain the thermoplastic elastomer modified polyethylene terephthalate. The melt blending is performed in a twin-screw extruder, and the temperature of the melt blending extrusion is preferably 245-285°C, more preferably 255-275°C.

[0026] The first polyester fiber-forming polymer slice and the second polyester fiber-forming polymer slice are melted to obtain a first melt A and a second melt B. In the present invention, the moisture content of the slice is less than 50 ppm, preferably less than 30 ppm; there is no special requirement for the source of the PET or PTT in the present invention, and commercially available products can be used.

[0027] The present invention requires that the fiber-forming polymer slices be pre-treated, and the pre-treatment includes drying, the drying temperature is preferably 160-170° C., the drying time is preferably 10-15 hours, and more preferably 11-13 hours. The present invention has no special requirements for the specific implementation process of the drying.

[0028] The present invention performs pre-treatment on the fiber-forming polymer slices, and also includes pre-crystallization, which can improve the crystallinity of PET and facilitate the subsequent smooth spinning.

[0029] In the present invention, when the first polyester fiber-forming polymer is PTT, melting includes: passing the first polyester fiber-forming polymer through four temperature zones in sequence, the temperature of the first temperature zone is 235-245°C, the temperature of the second temperature zone is 255-265°C, the temperature of the third temperature zone is 255-265°C, and the temperature of the fourth temperature zone is 255-265°C.

[0030] In the present invention, the first polyester fiber-forming polymer is thermoplastic elastomer modified polyethylene terephthalate, and the melting includes: passing the first polyester fiber-forming polymer through four temperature zones in sequence, the temperature of the first temperature zone is 255-265°C, the temperature of the second temperature zone is 280-290°C, the temperature of the third temperature zone is 280-290°C, and the temperature of the fourth temperature zone is 282-292°C.

[0031] The melting of the second polyester fiber-forming polymer includes: passing the second polyester fiber-forming polymer through four temperature zones in sequence, the temperature of the first temperature zone is 255-265°C, the temperature of the second temperature zone is 285-295°C, the temperature of the third temperature zone is 288-298°C, and the temperature of the fourth temperature zone is 288-298°C.

[0032] The spinning box temperature is 290-295℃.

[0033] In a specific embodiment of the present invention, the first polyester fiber-forming polymer and the second polyester fiber-forming polymer are preferably melted and extruded in a screw extruder to obtain two molten polyester fiber-forming polymers, and then the molten polyester fiber-forming polymers are composite-spun through a two-component composite spinning assembly to obtain a twisted composite elastic fiber.

[0034] The composite spinning preferably includes the following steps: sequentially spinning, cooling, oiling and winding the molten polyester fiber-forming polymer, and further texturizing to obtain fibers that can be used for weaving.

[0035] The present invention provides a two-component composite spinning assembly used in the composite spinning of the above preparation method, such as Figure 1 The two-component composite spinning assembly includes an assembly shell 1, in which a feed plate 2, a sealing gasket 3, a sand pool 4, a filter screen 5, an upper distribution plate 6, a lower distribution plate 7 and a spinneret 8 are arranged in sequence along the melt flow direction. Two types of melt channels are arranged on the feed plate 2, and each melt distribution channel on the upper distribution plate 6 is evenly provided with 4-8 countersunk holes to send the melt to the annular distribution channel on the lower distribution plate 7. Each melt annular distribution channel on the lower distribution plate 7 is provided with paired countersunk holes with the same number as the composite spinneret holes, and the paired countersunk holes are connected to the first melt A feed port 9 and the second melt B feed port 10 on the spinneret 8 respectively. The first melt A feed port 9 is connected to the oblique spinneret guide hole assembly A, and the second melt B feed port 10 is connected to the oblique spinneret guide hole assembly B.

[0036] The spinneret guide hole assembly A includes a spinneret guide hole A12, a conical hole A13, and a spinneret microhole A14 which are connected in sequence and are axially symmetrical, and the center lines of the spinneret guide hole A12, the conical hole A13, and the spinneret microhole A14 are on a straight line. The spinneret guide hole assembly B includes a spinneret guide hole B, a conical hole B, and a spinneret microhole B which are connected in sequence and are axially symmetrical, and the center lines of the spinneret guide hole B, the conical hole B, and the spinneret microhole B are on a straight line.

[0037] like Figure 2 , Figure 3 As shown, the first melt A and the second melt B pass through their respective oblique spinneret guide holes, conical holes and spinneret microholes, and finally compound at the melt compounding circle 11; when compounding, the two melts are tangent to each other in opposite directions on the melt compounding circle 11, and the intersecting part accounts for 1 / 4-3 / 4 of the total amount of the melt.

[0038] like Figure 4 , Figure 5 , Figure 6 As shown, the spinneret guide hole assembly A and the spinneret guide hole assembly B are two groups of oblique melt channels, which are not connected to each other. The plane projections of the spinneret guide hole assembly A and the spinneret guide hole assembly B and the spinneret plate 8 are arranged in left and right opposite directions on the melt composite circumference. The spinneret guide hole assembly A and the spinneret guide hole assembly B are at an angle of 60°-120° in the main view projection of the spinneret plate 8, so that the composite melt generates a circumferential component force, and rotates with the help of the viscosity of the melt and further cooling. The diameter of the melt composite circumference 11 is 1-2 times the diameter of the spinneret microhole.

[0039] In one embodiment of the present invention, the melt compounding circle 11 is arranged inside the spinneret 8 , and is 0.2-0.5 mm away from the lower plane of the spinneret 8 .

[0040] In one embodiment of the present invention, the melt compounding circle 11 is arranged on the lower plane of the spinneret 8 .

[0041] In one embodiment of the present invention, the melt compounding circle 11 is arranged outside the spinneret 8, and is 0.2-0.5 mm away from the lower plane of the spinneret.

[0042] The twisted composite elastic fiber obtained by the preparation method described in the above technical solution is composed of a first polyester fiber-forming polymer and a second polyester fiber-forming polymer with different heat shrinkage properties, and is in a twisted and rotated state in the axial direction; it has a groove structure, and the width of the groove is 1 / 2-1 / 4 of the fiber diameter. The mass ratio of the first polyester fiber-forming polymer to the second polyester fiber-forming polymer is 1:1, and the viscosity difference between the first polyester fiber-forming polymer and the second polyester fiber-forming polymer is more than 0.3dl / g.

[0043] The two melts are passed into the spinneret 8 of the composite spinneret assembly at a mass ratio of 1:1 to obtain nascent fibers. The nascent fibers are successively subjected to ring blowing cooling, oiling, and winding after adjusting the tension through a pair of godet discs to obtain pre-drawn twisted elastic fibers (POY), which are then drawn through a texturing machine to obtain permanently twisted elastic fibers. The fiber indicators are breaking strength 2.5-3.8 cN / dtex, breaking elongation 15-35%, curling rate 20-35%, curling recovery rate 30%, and curling elasticity 80-95%.

[0044] Example 1: Using Figure 4 The melt compounding method is as follows: the diameter of the melt compounding circle is 0.35mm, the height is 0.25mm, the diameter of the spinneret microhole is 0.2mm, and the length is 0.4mm; the projection angle of the melt channel is 90°. The melt A component uses modified PET chips with a viscosity of 0.95dl / g, and the melt B component uses conventional PET chips with a viscosity of 0.64dl / g.

[0045] The modified PET slices were pre-crystallized at 120°C for 1h and dried at 165°C for 12h, with a moisture content of <30ppm; the conventional PET was dried at 175°C for 12h, with a moisture content of <25ppm. The modified PET slices were melted by a screw machine, with a melting temperature of: zone 1: 258±1°C, zone 2: 288±1°C, zone 3: 285±1°C, zone 4: 285±1°C, to obtain molten modified PET; the conventional PET was melted by a screw machine, with a melting temperature of: zone 1: 262±1°C, zone 2: 293±1°C, zone 3: 293±1°C, zone 4: 292±1°C, to obtain molten PET, with a box temperature of 293±1°C. The two melts were passed into the spinneret of the composite spinneret assembly at a mass ratio of 1:1 to obtain the nascent fiber. The spun fibers are successively subjected to ring-blowing cooling, oiling, and winding after adjusting the tension through a pair of godet discs to obtain pre-stretched twisted elastic fibers (POY). After being stretched by a texturing machine, permanently twisted elastic fibers are obtained.

[0046] The breaking strength is 3.1 cN / dtex, the breaking elongation is 18%, the curl rate is 24.5%, the curl recovery rate is 22.3%, and the curl elasticity is 89.5%.

[0047] Example 2: Using Figure 6 The melt compounding method is as follows: the diameter of the melt compounding circle is 0.35mm, the height is -0.25mm, the diameter of the spinneret microhole is 0.2mm, and the length is 0.4mm; the projection angle of the melt channel is 115°. The melt A component uses PTT chips with a melting point of 227℃ and a characteristic viscosity of 0.9~1.3 dL / g; the melt B component uses conventional PET chips with a melting point of 262℃ and a viscosity of 0.5~0.7dl / g. The spinning process conditions are as follows:

[0048] The obtained POY yarn is drawn by a texturing machine to obtain a permanently bent elastic fiber.

[0049] The breaking strength is 3.5cN / dtex, the breaking elongation is 21%, the curl rate is 23.5%, the curl recovery rate is 24.3%, and the curl elasticity is 88.7%.

[0050] The above embodiments of the present invention are merely examples to clearly illustrate the present invention, but are not intended to limit the protection scope of the present invention. All equivalent technical solutions also belong to the scope of the present invention. The patent protection scope of the present invention should be defined by the claims.

Claims

1. A method for preparing a twisted composite elastic fiber, characterized in that: The following steps are involved: Step 1: Melting a first polyester fiber-forming polymer and a second polyester fiber-forming polymer, two fiber-forming polymers that are compatible but have different heat shrinkage properties, respectively to obtain a first melt A and a second melt B; Step 2: The first melt A and the second melt B obtained in step 1 are subjected to composite spinning using a two-component composite spinning assembly; the first melt A and the second melt B are respectively introduced into the feed plate of the composite spinning assembly at a mass ratio of 4:6 to 6:4, enter the first melt A inlet and the second melt B inlet on the spinneret through their respective melt channels, and pass through their respective oblique spinneret guide holes, tapered holes and spinneret microholes, and finally composite at the melt composite circumference; during the composite process, the two melts are tangent to each other in opposite directions on the melt composite circumference, and the intersecting part accounts for 1 / 4-3 / 4 of the total amount of the melts, and the obtained fiber is in a state of axial rotation; Step 3: The spun fiber obtained in step 2 is subjected to ring-blowing cooling and oiling in sequence, and is wound after adjusting the tension through a pair of guide wire discs to obtain pre-stretched twisted elastic fiber (POY), which is then stretched by a texturing machine to obtain a permanent twisted elastic fiber.

2. The method for preparing the twisted composite elastic fiber according to claim 1, characterized in that: In step 2, the two-component composite spinning assembly comprises an assembly housing (1), wherein a feed plate (2), a sealing gasket (3), a sand pool (4), a filter screen (5), an upper distribution plate (6), a lower distribution plate (7) and a spinneret (8) are sequentially arranged in the assembly housing (1) along the melt flow direction, wherein two types of melt channels are arranged on the feed plate (2), and each melt distribution channel on the upper distribution plate (6) is evenly provided with 4-8 countersunk holes, so as to deliver the melt to the annular distribution channel on the lower distribution plate (7), and each melt annular distribution channel on the lower distribution plate (7) is provided with a pair of countersunk holes having the same number as the composite spinneret holes, so that the melt is sent to the annular distribution channel on the lower distribution plate (7), and the number of countersunk holes is the same as the number of the composite spinneret holes. The paired countersunk holes are connected to a first melt A feed port (9) and a second melt B feed port (10) on a spinneret (8), respectively; the first melt A feed port (9) is connected to an oblique spinneret guide hole assembly A, and the second melt B feed port (10) is connected to an oblique spinneret guide hole assembly B; the plane projections of the spinneret guide hole assembly A, the spinneret guide hole assembly B and the spinneret (8) are in opposite directions on the melt composite circumference (11); the main projection angle α of the spinneret guide hole assembly A, the spinneret guide hole assembly B and the spinneret (8) is 60°-120°; and the diameter of the melt composite circumference (11) is 1-2 times the diameter of the spinneret microhole.

3. The method for preparing the twisted composite elastic fiber according to claim 2, characterized in that: The spinneret guide hole assembly A comprises a spinneret guide hole A (12), a conical hole A (13), and a spinneret microhole A (14) which are connected in sequence and are axially symmetrical, and the center lines of the spinneret guide hole A (12), the conical hole A (13), and the spinneret microhole A (14) are on a straight line. The spinneret guide hole assembly B comprises a spinneret guide hole B, a conical hole B, and a spinneret microhole B which are connected in sequence and are axially symmetrical, and the center lines of the spinneret guide hole B, the conical hole B, and the spinneret microhole B are on a straight line.

4. The method for preparing the twisted composite elastic fiber according to claim 1, characterized in that: The melt compounding circle (11) is arranged inside the spinneret (8) and is 0.2-0.5 mm away from the lower plane of the spinneret.

5. The method for preparing the twisted composite elastic fiber according to claim 1, characterized in that: The melt compounding circle (11) is arranged on the lower plane of the spinneret (8).

6. The method for preparing the twisted composite elastic fiber according to claim 1, characterized in that: The melt compounding circle (11) is arranged outside the spinneret (8) and is 0.2-0.5 mm away from the lower plane of the spinneret.

7. A twisted composite elastic fiber, characterized in that: The fiber-forming polymer is prepared by the preparation method according to any one of claims 1 to 6, and is composed of a first polyester fiber-forming polymer and a second polyester fiber-forming polymer having two compatible properties with different heat shrinkage properties, and the fiber axis is in a twisted and rotated state; it has a groove structure, and the width of the groove is 1 / 2-1 / 4 of the fiber diameter; the mass ratio of the first polyester fiber-forming polymer to the second polyester fiber-forming polymer is 1:1, and the viscosity difference between the first polyester fiber-forming polymer and the second polyester fiber-forming polymer is more than 0.3dl / g.

8. An application of a twisted composite elastic fiber, characterized in that: The twisted composite elastic fiber described in claim 7 is applied to fabrics.

Citation Information

Patent Citations

  • Double-component staggered spinneret

    CN103668498A

  • Preparation method of polylactic acid side-by-side composite fiber

    CN108130606A

  • Carpet yarns and preparation method thereof

    CN111041579A

  • Preparation method of moisture absorption and quick drying fabric

    CN111041677A

  • Side-by-side composite elastic fiber, preparation method and application thereof, and composite spinning assembly

    CN113862827A