Aluminum negative electrode based on MOF interface modification and preparation method thereof
By forming an MOF particle layer on the surface of the aluminum anode, the problems of aluminum corrosion and aluminum dendrite formation in aluminum secondary batteries are solved, improving the cycle performance and safety of the battery, making it suitable for industrial production.
Patent Information
- Application Number
- CN202411173844.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing aluminum secondary batteries suffer from problems such as easy corrosion of the aluminum negative electrode and formation of aluminum dendrites, resulting in insufficient cycle life and safety.
An aluminum anode based on MOF interface modification is used. A MOF particle layer is formed on the surface of an aluminum metal substrate. The specific steps include mixing water, nitric acid and coordination materials, surface pretreatment, hydrothermal synthesis and drying treatment to form a uniform and dense MOF modification layer.
It significantly improves the cycle performance and safety of aluminum secondary batteries, inhibits the formation of aluminum dendrites, extends the cycle life of the battery, and reduces maintenance costs, thus achieving environmental protection and energy-saving effects.
Smart Images

Figure CN118983397A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aluminum negative electrode based on MOF interface modification and a preparation method thereof, belonging to the technical field of batteries, and specifically to an MOF-based interface modification technology for realizing a stable and long-cycle aluminum negative electrode. Background Art
[0002] With the development of the field of electrochemical energy storage, the research and development of battery materials has become increasingly important. As a new type of electrochemical energy storage device, aluminum secondary batteries have the advantages of low cost, environmental friendliness and high safety. The aluminum negative electrode is an important component of aluminum secondary batteries, and its performance directly affects the cycle life and safety of the battery. The aluminum negative electrode is prone to problems such as aluminum corrosion and aluminum dendrites during the cycle, resulting in a decrease in battery performance. However, there are some problems in the practical application of aluminum secondary batteries, mainly including the corrosion of the aluminum negative electrode and the formation of aluminum dendrites, which limit its cycle life and safety.
[0003] Although the importance of aluminum negative electrode in aluminum secondary batteries has been widely recognized, the current protection technology still has many shortcomings. Existing aluminum negative electrode protection methods mainly include surface coating and alloying. However, each of these methods has certain limitations. Surface coating technology often faces the problem of insufficient adhesion between the coating and the aluminum substrate, which is easy to fall off during the cycle, resulting in a gradual weakening of the protection effect. Although alloying can improve the corrosion resistance of aluminum negative electrode, the complex alloy preparation process and high material cost limit its large-scale application. Summary of the invention
[0004] The technical problem solved by the present invention is: to overcome the deficiencies of the prior art and to propose an aluminum negative electrode based on MOF interface modification and a preparation method thereof.
[0005] The technical solution of the present invention is:
[0006] An aluminum negative electrode based on MOF interface modification, the aluminum negative electrode based on MOF interface modification includes an aluminum metal matrix and a MOF particle layer located on the surface of the aluminum metal matrix, and can also be an aluminum metal matrix and a MOF-C particle layer located on the surface of the aluminum metal matrix. The stability and durability of the aluminum negative electrode based on MOF interface modification are improved, and a stable long cycle of the aluminum negative electrode based on MOF interface modification is achieved.
[0007] The technical solution of the present invention is:
[0008] The preparation method of an aluminum negative electrode based on MOF interface modification, wherein the aluminum negative electrode based on MOF interface modification prepared by the method comprises an aluminum metal matrix and a MOF particle layer located on the surface of the aluminum metal matrix, and the specific steps are as follows:
[0009] The first step is to mix water, nitric acid and a coordination material to obtain a mixture, wherein the mass ratio of water, nitric acid and the coordination material is 200:5-20:2-5;
[0010] The second step is to perform surface pretreatment on the aluminum metal substrate. Surface pretreatment refers to removing the oxide film on the surface of the aluminum metal substrate by using an alkaline or acidic reagent; the alkaline reagent is preferably a NaOH solution, and the acidic reagent is preferably hydrochloric acid;
[0011] The third step is to perform hydrothermal synthesis on the aluminum metal substrate after the surface pretreatment in the second step and the mixture obtained in the first step in a hydrothermal reactor, the hydrothermal synthesis temperature is 160-200° C., and the hydrothermal synthesis time is 10-16 hours;
[0012] In the fourth step, the hydrothermal synthesis product of the third step is washed and dried to obtain an aluminum negative electrode based on MOF interface modification.
[0013] The preparation method of an aluminum negative electrode based on MOF interface modification, wherein the aluminum negative electrode based on MOF interface modification prepared by the method comprises an aluminum metal matrix and a MOF-C particle layer located on the surface of the aluminum metal matrix, and the specific steps are as follows:
[0014] The first step is to mix water, nitric acid and a coordination material to obtain a mixture, wherein the mass ratio of water, nitric acid and the coordination material is 200:5-20:2-5;
[0015] The second step is to perform surface pretreatment on the aluminum metal substrate. Surface pretreatment refers to removing the oxide film on the surface of the aluminum metal substrate by using an alkaline or acidic reagent; the alkaline reagent is preferably a NaOH solution, and the acidic reagent is preferably hydrochloric acid;
[0016] The third step is to perform hydrothermal synthesis on the aluminum metal substrate after the surface pretreatment in the second step and the mixture obtained in the first step in a hydrothermal reactor, the hydrothermal synthesis temperature is 160-200° C., and the hydrothermal synthesis time is 10-16 hours;
[0017] In the fourth step, the hydrothermal synthesis product of the third step is washed, dried and heated to obtain an aluminum negative electrode based on MOF-C interface modification, wherein the heating temperature is 550-600°C and the heating time is 12-16h.
[0018] The application of aluminum negative electrode based on MOF interface modification and the application of aluminum negative electrode based on MOF interface modification to aluminum secondary batteries can improve the cycle performance and safety of aluminum secondary batteries.
[0019] The coordination material is one of benzoic acids, aromatic amines, aromatic diketones, aromatic triketones, pyridines, amino acids, ethers, nitro compounds, and heterocyclic compounds;
[0020] The benzoic acids include benzoic acid, phthalic acid, and trimesic acid;
[0021] The aromatic amines include p-phenylenediamine and p-hydroxyaniline;
[0022] The aromatic diketones include isophthalic acid and terephthalic acid;
[0023] The aromatic triketones include benzotrione and pyrobenzotrione;
[0024] The pyridines include pyridine, para-dipyridine, and pyridone;
[0025] The amino acids include aminoacetic acid and aminopropionic acid;
[0026] The ethers include ethylene glycol and glycine ethyl ester;
[0027] The nitro compounds include nitrobenzene and nitroethylene;
[0028] The MOF is an aluminum-based MOF, such as at least one of MIL-96, MIL-100, MIL-110, MIL-53, CAU-10, MOF-74, NOTT-300, MIL-68, PCN-333, MOF-177, CAU-17, MIL-125, NU-1000, DUT-5, MMPF-12, MIL-160, CPO-27, and NU-901;
[0029] The thickness of the MOF particle layer located on the surface of the aluminum metal substrate is 10-20 μm;
[0030] The thickness of the MOF-C particle layer located on the surface of the aluminum metal substrate is 10-20 μm;
[0031] When drying, the drying temperature is 80-200°C and the drying time is 10-24h.
[0032] Beneficial Effects
[0033] (1) The method of the present invention effectively increases the active sites on the negative electrode surface by forming a modified layer on the surface of the aluminum metal substrate, which is beneficial to reducing the polarization voltage of the battery electrode;
[0034] (2) The method of the present invention can improve the cycle performance of aluminum secondary batteries and inhibit the formation of aluminum dendrites and corrosion by forming a modified layer on the surface of the aluminum metal substrate, thereby significantly improving the cycle performance of the battery;
[0035] (3) The present invention relates to an interface modification technology based on metal organic framework materials (MOF), which aims to solve the problems existing in the aluminum negative electrode in aluminum secondary batteries, such as aluminum corrosion, aluminum dendrite formation, etc., so as to improve the cycle life and safety of the battery. This technology improves the interaction between the negative electrode surface and the electrolyte and enhances the stability and durability of the aluminum negative electrode by forming a uniform and dense MOF modification layer on the surface of the aluminum negative electrode. The present invention provides detailed implementation steps, including preparing a precursor solution, treating an aluminum substrate, hydrothermal synthesis, drying and heat treatment. Experimental results show that this technology can effectively improve the cycle performance of aluminum secondary batteries and has good industrial application prospects. The present invention uses a method of in-situ synthesizing a MOF modification layer on the aluminum surface, so that aluminum metal can be stably circulated in an electrolyte of an ionic liquid system, inhibiting the corrosion of aluminum metal and the growth of dendrites, preventing battery failure, and effectively improving the cycle stability of aluminum secondary batteries. The technical solution of the present invention is simple and feasible, can effectively improve the cycle life and safety of aluminum secondary batteries, and has good application prospects;
[0036] (4) The method of the present invention successfully improves the negative electrode performance of aluminum secondary batteries by in-situ synthesizing a MIL-96-C modification layer on the surface of aluminum foil using a hydrothermal method. This modification layer not only increases the active site density on the surface of the aluminum negative electrode, optimizes the electrode reaction interface structure, and significantly improves the battery's cycle performance and safety, but also successfully inhibits the formation of aluminum dendrites and reduces the risk of short circuits during battery cycling. In addition, the MIL-96-C modification layer, as a protective layer, effectively prevents aluminum corrosion in the electrolyte, extends the service life of the aluminum foil, and reduces the maintenance cost of the battery.
[0037] (5) The preparation process of the present invention is simple and efficient, does not require complicated preparation steps and expensive raw materials, is conducive to reducing preparation costs, and is suitable for industrial production. At the same time, the method of synthesizing the MIL-96-C modification layer by the hydrothermal method does not require a large amount of organic solvents and toxic reagents, has good environmental protection, and can effectively utilize raw materials and save energy. In general, the present invention can not only improve the cycle life and safety of aluminum secondary batteries, but also has good environmental protection and energy-saving effects, providing a higher possibility for the optimization of aluminum secondary batteries.
[0038] (6) The aluminum negative electrode preparation method based on MOF interface modification proposed in the present invention has significant advantages. By in-situ synthesizing MOF materials on the surface of aluminum foil, a uniform and firm protective layer can be formed on the surface of the aluminum negative electrode. Due to its unique porous structure and adjustable chemical properties, MOF materials can not only effectively inhibit the formation of aluminum dendrites, but also significantly reduce the corrosion of aluminum metal. In addition, the in-situ synthesis technology ensures the close bonding between the MOF layer and the aluminum substrate, improves the stability of the interface, and thus extends the cycle life of the battery. Compared with traditional coating and alloying methods, the MOF modification technology in this patent is more cost-effective and provides reliable technical support for the practical application of aluminum secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the SEM image of the MIL-96-C modified layer;
[0040] Figure 2 Electrochemical performance diagram of symmetric cells assembled with aluminum with MIL-96-C modification layer. DETAILED DESCRIPTION
[0041] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0042] A method for treating an aluminum negative electrode in an aluminum secondary battery of the present invention comprises the following steps:
[0043] 1. Preparation of precursor solution:
[0044] a. In a clean container, weigh an appropriate amount of M.
[0045] b. Add an appropriate amount of N into the container.
[0046] c. Stir the mixture thoroughly with a glass rod or magnetic stirrer to obtain a uniform mixture.
[0047] 2. Processing of aluminum substrate:
[0048] a. Place the aluminum foil in solution L and ensure that the oxide film on the surface of the aluminum foil is completely removed.
[0049] b. Take out the treated aluminum foil and clean it with alcohol.
[0050] 3. Hydrothermal synthesis:
[0051] a. Place the treated aluminum foil and precursor solution in a hydrothermal reactor.
[0052] b. Heat the reactor.
[0053] c. After the reaction is completed, remove the reactor from the heating source and wait for it to cool to room temperature.
[0054] d. Open the reactor, take out the aluminum foil, and wash it thoroughly with deionized water or other solvents to remove unreacted substances and residual solvents.
[0055] 4. Drying:
[0056] a. Place the treated aluminum foil in a vacuum drying oven to allow it to dry completely.
[0057] 5. Heat treatment:
[0058] a. Place the dried aluminum foil in a heating device protected by inert gas.
[0059] b. Heat the heating device and keep the temperature stable.
[0060] c. Heat the aluminum foil for a certain period of time to convert the MIL-96 on the surface of the aluminum foil into MIL-96-C.
[0061] d. After the heat treatment is completed, cool the heating device to room temperature.
[0062] 6. Collect samples and test:
[0063] a. Store the heated aluminum foil in a sealed container to prevent the aluminum foil from coming into contact with air and reacting to form an oxide film.
[0064] b. Conduct characterization analysis on the prepared aluminum foil, such as scanning electron microscopy (SEM), assembling it into a symmetrical battery test in an ionic liquid system, etc.
[0065] In step 1, the raw materials of the precursor solution are: M is HNO3, N is Me3BTC (1,3,5-benzenetricarboxylic acid trimethyl ester). The aluminum foil is an aluminum sheet that can be used in the negative electrode of an aluminum secondary battery.
[0066] In step 2, the L solution for treating the aluminum substrate is an acidic reagent or an alkaline reagent, preferably a NaOH solution.
[0067] In step 3, the hydrothermal treatment time is 12 hours and the heating temperature is 180°C.
[0068] In step 5, the heating time is 12 hours and the heating temperature is 600°C.
[0069] In step six, the raw materials of the ionic liquid are 1-ethyl-3-methylimidazolium chloride and aluminum chloride powder, and the molar ratio of the two is EMIC:AlCl3=1:1.3.
[0070] The controllable diameter of MIL-96 on the surface of the high-purity aluminum sheet is 10-20 μm, occupying 100% of the surface of the high-purity aluminum sheet.
[0071] Example 1
[0072] The preparation method of aluminum negative electrode based on MOF interface modification, the specific steps are:
[0073] 1. Preparation of precursor solution:
[0074] In a clean container, take 0.8 g of nitric acid (HNO3).
[0075] 1.5 g of Me3BTC (trimethyl 1,3,5-benzenetricarboxylate) was added to the container.
[0076] Add 100 ml of water to the container and stir the mixture thoroughly using a glass rod or a magnetic stirrer to obtain a homogeneous mixture.
[0077] 2. Processing of aluminum substrate:
[0078] A piece of aluminum foil with a size of 5 cm x 5 cm was placed in a container containing 100 mL of 10% NaOH solution (L), ensuring that the oxide film on the surface of the aluminum foil was completely removed.
[0079] The treated aluminum foil was taken out and cleaned with 75% ethanol to remove impurities on the surface.
[0080] 3. Hydrothermal synthesis:
[0081] The treated aluminum foil and the precursor solution were placed in a hydrothermal reactor with a capacity of 500 mL.
[0082] The reactor was heated to 180°C and kept at this temperature for 12 hours.
[0083] After the reaction is completed, the reactor is removed from the heating source and cooled to room temperature.
[0084] The reactor is opened, the aluminum foil is taken out, and it is thoroughly washed with deionized water or other solvents to remove unreacted substances and residual solvents.
[0085] 4. Drying:
[0086] The treated aluminum foil was placed in a vacuum drying oven and dried at 80° C. for 24 hours.
[0087] 5. Collect samples and test:
[0088] The aluminum foil modified with the MIL-96 modification layer prepared in the above steps is stored in a sealed container to prevent the aluminum foil from coming into contact with air and reacting to form an oxide film.
[0089] Example 2
[0090] The preparation method of aluminum negative electrode based on MOF interface modification, the specific steps are:
[0091] 1. Preparation of precursor solution:
[0092] In a clean container, take 0.8 g of nitric acid (HNO3).
[0093] 1.5 g of Me3BTC (trimethyl 1,3,5-benzenetricarboxylate) was added to the container.
[0094] Add 100 ml of water to the container and stir the mixture thoroughly using a glass rod or a magnetic stirrer to obtain a homogeneous mixture.
[0095] 2. Processing of aluminum substrate:
[0096] A piece of aluminum foil with a size of 5 cm x 5 cm was placed in a container containing 100 mL of 10% NaOH solution (L), ensuring that the oxide film on the surface of the aluminum foil was completely removed.
[0097] The treated aluminum foil was taken out and cleaned with 75% ethanol to remove impurities on the surface.
[0098] 3. Hydrothermal synthesis:
[0099] The treated aluminum foil and the precursor solution were placed in a hydrothermal reactor with a capacity of 500 mL.
[0100] The reactor was heated to 180°C and kept at this temperature for 12 hours.
[0101] After the reaction is completed, the reactor is removed from the heating source and cooled to room temperature.
[0102] The reactor is opened, the aluminum foil is taken out, and it is thoroughly washed with deionized water or other solvents to remove unreacted substances and residual solvents.
[0103] 4. Drying:
[0104] The treated aluminum foil was placed in a vacuum drying oven and dried at 80° C. for 24 hours.
[0105] 5. Heat treatment:
[0106] Place the dried aluminum foil into a heating device.
[0107] Heat the heating device to 600°C and keep the temperature stable for 12 h.
[0108] The aluminum foil was heated at 600°C for 12 hours. After the heat treatment was completed, the heating device was cooled to room temperature.
[0109] 6. Collect samples and test:
[0110] Store the heated aluminum foil in a sealed container to prevent the foil from coming into contact with air and reacting to form an oxide film.
[0111] The above steps prepare an aluminum foil sheet modified with a MIL-96-C modification layer, which is used to assemble an aluminum secondary battery.
[0112] The SEM image of the aluminum foil modified with the MIL-96-C modification layer is as follows: Figure 1 As shown by Figure 1 It can be seen that the synthesized MIL-96-C material has good particle morphology and high crystallinity, presenting a dense and uniform hexagonal double-truncated particle structure, with uniform particle distribution and a particle size of about 15 μm;
[0113] The assembled aluminum symmetrical battery was electrochemically tested, and the test results are as follows: Figure 2 As shown by Figure 2 It can be seen that the aluminum symmetric battery assembled with aluminum foil modified with MIL-96-C modification layer has a deposition / dissolution overpotential of 15 mV and a cycle time of 7800 hours, showing excellent stability and long cycle performance;
[0114] Example 3
[0115] According to the method described in Example 1, the difference is that the mixed solution is 3g of terephthalic acid, 2g of sodium oxalate and 100mL of deionized water, which are added to a clean container in sequence. Use a glass rod or a magnetic stirrer to fully stir the mixture, transfer the mixture to a hydrothermal reactor, put an aluminum substrate, heat the hydrothermal reactor to 180°C, and keep the reaction temperature constant for 12 hours. After the reaction is completed, remove the reactor from the heating source and cool to room temperature. Obtain an aluminum foil with a CAU-10 modified layer.
[0116] Example 4
[0117] According to the method described in Example 1, the difference is that the mixed solution is 2g of benzene trimecyl carboxylic acid, 1g of lithium fluoride and 100mL of deionized water, which are added to a clean container in sequence. Use a glass rod or a magnetic stirrer to fully stir the mixture, transfer the mixture to a hydrothermal reactor, put an aluminum substrate, heat the hydrothermal reactor to 180°C, and keep the reaction temperature constant for 12 hours. After the reaction is completed, remove the reactor from the heating source and cool to room temperature. Obtain an aluminum foil with a NOTT-300 modified layer.
[0118] Example 5
[0119] According to the method described in Example 1, the difference is that the mixed solution is 1.5g phthalic acid, 1 gram of lithium fluoride and 100mL deionized water, which are added to a clean container in sequence. Use a glass rod or a magnetic stirrer to fully stir the mixture, transfer the mixture to a hydrothermal reactor, put an aluminum substrate, heat the hydrothermal reactor to 180°C, and keep the reaction temperature constant for 12 hours. After the reaction is completed, the reactor is removed from the heating source and cooled to room temperature. Obtain an aluminum foil with a PCN-333 modified layer.
[0120] Example 6
[0121] According to the method described in Example 1, the difference is that the mixed solution is 2.5g benzoic acid, 1.8g potassium chloride and 100mL deionized water, which are added to a clean container in sequence. Use a glass rod or a magnetic stirrer to fully stir the mixture, transfer the mixture to a hydrothermal reactor, put an aluminum substrate, heat the hydrothermal reactor to 180°C, and keep the reaction temperature constant for 12 hours. After the reaction is completed, remove the reactor from the heating source and cool to room temperature. Obtain an aluminum foil with a CPM-800 modified layer.
[0122] Comparative Example: Aluminum foil is directly used to assemble into aluminum secondary batteries.
[0123] Table 1: Comparison of overpotentials of metal symmetric batteries after stabilization in the examples and comparative examples
[0124]
[0125]
[0126] It can be seen from the results of Examples 1-6 and Comparative Example 1 that the cycle life of the aluminum-battery assembled with the optimized aluminum sheets in Examples 1-6 of the present invention is significantly better than that of the aluminum-battery assembled with the untreated aluminum sheets, which can significantly improve the stability of the battery.
[0127] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0128] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0129] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
[0130] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. Preparation method of aluminum negative electrode based on MOF interface modification, Features The specific steps are: In the first step, water, nitric acid and a coordination material are mixed to obtain a mixture; The second step is to perform surface pretreatment on the aluminum metal substrate; The third step is to hydrothermally synthesize the aluminum metal substrate after the surface pretreatment in the second step and the mixture obtained in the first step in a hydrothermal reactor; In the fourth step, the hydrothermal synthesis product of the third step is washed and dried to obtain an aluminum negative electrode based on MOF interface modification.
2. The method for preparing an aluminum negative electrode based on MOF interface modification according to claim 1, Features: The obtained aluminum negative electrode based on MOF interface modification is heated in an inert gas protection atmosphere to obtain an aluminum negative electrode based on MOF-C interface modification.
3. The method for preparing an aluminum negative electrode based on MOF interface modification according to claim 2, Features: The heating temperature in the heating device is 550-600° C., the heating time is 12-16 hours, and the inert gas is one of helium, neon, argon, krypton, xenon and nitrogen.
4. The method for preparing an aluminum negative electrode based on MOF interface modification according to any one of claims 1 to 3, Features: In the first step, the mass ratio of water, nitric acid and coordination material is 200:5-20:2-5.
5. The method for preparing an aluminum negative electrode based on MOF interface modification according to any one of claims 1 to 3, Features: In the second step, surface pretreatment refers to removing the oxide film on the surface of the aluminum metal substrate by using an alkaline or acidic reagent; the alkaline reagent is NaOH solution, and the acidic reagent is hydrochloric acid.
6. The method for preparing an aluminum negative electrode based on MOF interface modification according to any one of claims 1 to 3, Features: In the third step, the hydrothermal synthesis temperature is 160-200° C., and the hydrothermal synthesis time is 10-16 h; In the fourth step, the drying temperature is 80-200° C. and the drying time is 10-24 hours.
7. The method for preparing an aluminum negative electrode based on MOF interface modification according to any one of claims 1 to 3, Features: In the third step, the coordination material is one of benzoic acids, aromatic amines, aromatic diketones, aromatic triketones, pyridines, amino acids, ethers, nitro compounds, and heterocyclic compounds; The benzoic acid is benzoic acid, phthalic acid or trimesic acid; The aromatic amine is p-phenylenediamine or p-hydroxyaniline; The aromatic diketone is isophthalic acid or phthalic acid; The aromatic triketone is benzotrione or pyrobenzotrione; The pyridine is pyridine, para-dipyridine or pyridone; The amino acid is aminoacetic acid or aminopropionic acid; The ether is ethylene glycol or glycine ethyl ester; The nitro compound is nitrobenzene or nitroethylene; The MOF is an aluminum-based MOF.
8. The method for preparing an aluminum negative electrode based on MOF interface modification according to claim 7, Features: The MOF is at least one of MIL-96, MIL-100, MIL-110, MIL-53, CAU-10, MOF-74, NOTT-300, MIL-68, PCN-333, MOF-177, CAU-17, MIL-125, NU-1000, DUT-5, MMPF-12, MIL-160, CPO-27, and NU-901; The thickness of the MOF particle layer located on the surface of the aluminum metal substrate is 10-20 μm.
9. The method for preparing an aluminum negative electrode based on MOF interface modification according to claim 2, Features: The thickness of the MOF-C particle layer located on the surface of the aluminum metal substrate is 10-20 μm.
10. Application of aluminum anode based on MOF interface modification, Features: Applying aluminum negative electrodes based on MOF interface modification to aluminum secondary batteries can improve the cycle performance and safety of aluminum secondary batteries.
Citation Information
Patent Citations
Electrode material surface coating method and application thereof
CN106099047A
Preparation method and application of Al-MOF negative electrode material synthesized by solvothermal method
CN112054186A
Lithium ion battery negative electrode material MIL-53 (Al-Fe) with MOF structure and preparation method thereof
CN112614975A
Preparation method of metal organic framework derived carbon with high specific surface area
CN113072056A
Preparation method of metal organic framework MIL-53 series membrane
CN115569537A