MXene flexible self-supporting membrane electrode based on micro-channel regulation and control as well as preparation method and application of MXene flexible self-supporting membrane electrode

The MXene flexible self-supporting membrane electrode with microchannel structure was prepared by the hard template method, which solved the problems of poor conductivity and insufficient site exposure of Li-CO2 battery catalysts, and achieved battery performance with low overpotential, high magnification and long cycle life. And meets the mechanical requirements of flexible batteries.

CN119009362AActive Publication Date: 2024-11-22TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411046688.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing Li-CO2 batteries are slow in reaction kinetics, high overpotential, severe polarization and poor reversibility due to poor conductivity of the positive electrode catalyst and insufficient site exposure. The MXene materials are prone to stacking and collapse during charging and discharging, resulting in low capacity. , poor magnification and cycle performance.

Method used

The hard template method is used to prepare MXene flexible self-supporting membrane electrodes with rich microchannel structures. Through selective etching and nano-scale magnesium oxide templates, the specific surface area and active sites are increased, and the stable layered structure is reduced. Collapse between layers to improve the efficiency of electrochemical reactions.

Benefits of technology

The low overpotential, long cycle life and good rate performance of Li-CO2 batteries are achieved, and the flexible electrode meets the mechanical requirements of wearable devices, reducing the battery weight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009362A_ABST
    Figure CN119009362A_ABST
Patent Text Reader

Abstract

The invention discloses an MXene flexible self-supporting membrane electrode based on microchannel regulation and control and a preparation method and application thereof.The preparation method comprises the steps that firstly, lithium fluoride and concentrated hydrochloric acid serve as selective etching agents, an aluminum layer of an MAX-phase precursor Ti3AlC2 is selectively etched, a single-layer or few-layer Ti3C2 dispersion liquid is obtained through centrifugal ultrasound, at the moment, a template agent is introduced, and the template agent is prepared; the microenvironment of the two-dimensional Ti3C2 thin electrode is regulated and controlled; then the MXene flexible self-supporting membrane material with rich microchannel structures is used as an independent electrode of the lithium-carbon dioxide battery, the obtained electrode can provide a shorter transmission path for ion transmission, and the accessibility of an electrolyte is improved; compared with a Li-CO2 battery prepared from an unregulated Ti3C2 self-supporting membrane electrode, the Li-CO2 battery prepared from the electrode has the advantages that the polarization voltage is smaller, and the rate capability is more excellent; and the cycle performance is also obviously enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a MXene flexible self-supporting membrane electrode based on microchannel regulation, a preparation method thereof and application in a Li-CO2 battery, belonging to the technical field of metal-gas battery catalysts. Background Art

[0002] In modern society, with the rapid development of economy and technology, human demand for energy is growing, mineral fuels and fossil energy are used in large quantities, and greenhouse gases represented by carbon dioxide are continuously released, exacerbating global warming. Lithium-carbon dioxide (Li-CO2) batteries, as a technology that converts the chemical energy of carbon dioxide gas into electrical energy at room temperature and stores it, have become an important secondary battery in the "post-lithium ion era" due to their extremely high energy density and low-carbon green characteristics. Even among many metal-air batteries, Li-CO2 batteries still have high charge and discharge potentials (≈ 2.8 V) and high theoretical specific capacity (1876 Wh kg -1 )’s typical advantages.

[0003] At present, Li-CO2 batteries have made some progress after more than ten years of development since their birth, but the high overpotential, poor cycle performance, weak rate performance and low discharge capacity caused by the wide band gap of the discharge product Li2CO3 seriously restrict the rapid development of Li-CO2. The positive electrode catalyst is a key factor in increasing the electrode reaction rate and reducing the overpotential during the charge and discharge process, and is the core of achieving efficient and reversible Li-CO2.

[0004] MXene (two-dimensional transition metal carbon / nitride) has a unique layered structure, with significant advantages such as hydrophilicity, high conductivity and adjustable surface groups, and is one of the most promising energy storage materials. However, due to its own weight and the accumulation of products during the charge and discharge process, the original MXene is prone to stacking and collapse, and the inert functional groups on the surface have insufficient catalytic activity, resulting in low capacity, poor rate and cycle performance in Li-CO2 battery applications. Therefore, it is necessary to load or modify surface functional groups to generate additional reaction sites, build a favorable electrochemical reaction microenvironment, and improve the specific capacity of the battery. At the same time, its unique structure provides a shorter diffusion path for ions and electrons, improves ion diffusion rate and conductivity, and improves battery rate and cycle performance. Summary of the invention

[0005] The present invention aims to provide a MXene flexible self-supporting membrane electrode based on microchannel regulation, and a preparation method and application thereof. The MXene flexible self-supporting membrane material with rich microchannel structure is used as an independent electrode of a lithium-carbon dioxide battery. The shortcomings of the current catalyst, such as poor conductivity and insufficient site exposure, can be addressed, and the problems of slow reaction kinetics, high overpotential, severe polarization, and poor reversibility of lithium-carbon dioxide batteries can be solved. At the same time, the requirements of the lithium-carbon dioxide battery system for low overpotential and long cycle life can be met. In addition, the use of the self-supporting membrane material as an independent electrode can reduce the weight of the battery itself and meet the battery's requirements for flexibility.

[0006] The present invention utilizes a hard template method to use a MgO template agent to micro-regulate the MXene material, so that the MXene material has abundant microchannels, which is beneficial to the accessibility of the electrolyte. In addition, the layered structure of MXene can be stabilized, and the interlayer collapse of MXene can be prevented to a certain extent. At the same time, the specific surface area of ​​MXene material is increased, more active sites are provided, and the flexibility of the membrane material is not destroyed.

[0007] The present invention provides a method for regulating microchannels of a MXene flexible self-supporting membrane electrode. A Ti3C2 flexible thin film material with a rich microchannel structure is synthesized by regulating a template using a simple synthesis process. The method comprises using lithium fluoride and concentrated hydrochloric acid as selective etchants to selectively etch the aluminum layer of a MAX phase precursor Ti3AlC2, obtaining a single layer or a few layers of Ti3C2 dispersion by centrifugal ultrasound, introducing a template at this time, controlling the type and amount of the template, and realizing the regulation of the microenvironment of a two-dimensional Ti3C2 thin electrode.

[0008] The hard template has high stability and good narrow confinement effect. The hard template can be used to adjust the interlayer spacing and intralayer pore size distribution of two-dimensional Ti3C2, stabilize the interlayer structure, and provide a favorable reaction interface and transport channel for lithium-carbon dioxide batteries. In the present invention, nano-magnesium oxide is selected as a hard template agent. Magnesium oxide has good stability, is not easy to react with Ti3C2, and is easily removed by dilute acid, which is environmentally friendly. Nano-magnesium oxide particles (30-50nm) are used to form a unique microenvironment between Ti3C2 layers, so that the two-dimensional layered structure of Ti3C2 has a certain confinement effect, which can reduce the size of the discharge product to a certain extent, making the discharge product easier to decompose. By using different proportions of magnesium oxide, the interlayer structure and pore size of Ti3C2 can be adjusted to prepare a Ti3C2 thin film electrode with good catalytic activity and strong conductivity, giving the lithium-carbon dioxide battery a lower overpotential and better cycle stability. In addition, since the prepared thin film electrode has good mechanical flexibility, it can be used as an independent positive electrode to prepare a flexible lithium-carbon dioxide battery, and this flexible battery has good charge and discharge performance.

[0009] The present invention provides a method for preparing a MXene flexible self-supporting membrane electrode having abundant microchannels after microscopic regulation, comprising the following steps: (1) Selective etching of precursor Ti3AlC2 Place 10-50 mL of 12 M HCl in a polytetrafluoroethylene liner, dissolve 0.8-4 g of LiF in HCl, and the molar ratio of LiF to HCl is 1:4-1:40. Then heat and stir in a water bath to prepare a selective etchant for the Al layer.

[0010] Take 0.5-5 g Ti3AlC2 and slowly add it to the etchant, the molar ratio of Ti3AlC2 to LiF is 1:10-1:100, then heat and stir in a water bath to fully react; (2) Ti3C2 layering process Transfer the mixed solution in step (1) to a 50 mL centrifuge tube, wash with 1 M HCl 2-3 times, then wash with water until the supernatant reaches neutrality, the precipitate begins to swell, and the supernatant turns dark green, wash with water again, then shake well without pouring out the supernatant, and centrifuge. After the mixed solution is shaken well, place it in an ice-water bath for ultrasonication, and centrifuge again to obtain the supernatant, which is the monolayer or few-layer Ti3C2 dispersion.

[0011] (3) Micro-control of Ti3C2 using hard template method Take a Ti3C2 dispersion (concentration of 10 mg / mL), add MgO to the Ti3C2 dispersion at a ratio of Ti3C2:MgO = 1:2~1:10 (mass ratio), stir at room temperature for 24 h, then pickle with 3 M glacial acetic acid, then wash with water, add ultrapure water, shake well and sonicate to obtain a Ti3C2 dispersion after micro-control.

[0012] (4) Preparation of Ti3C2 self-supporting film The micro-controlled Ti3C2 dispersion was filtered into a membrane using a vacuum filter and then dried at 60 °C in vacuum.

[0013] Application of the MXene flexible self-supporting film material obtained by the preparation method of the present invention in lithium-carbon dioxide batteries.

[0014] In the above application, the Li-CO2 button battery is assembled in a glove box with Ar atmosphere, the electrolyte is configured with lithium bis(trifluoromethanesulfonyl)imide as lithium salt dissolved in tetraethylene glycol dimethyl ether solvent, the battery negative electrode is a metal lithium sheet, the diaphragm is glass fiber, the electrolyte is dripped on both sides of the diaphragm, and a total of 80-120 μl of electrolyte is dripped. The MXene flexible self-supporting film is cut into discs with a diameter of 12 mm and directly used as the positive electrode. A porous metal shell is used as the positive electrode shell to facilitate CO2 gas transportation; the assembled button battery is tested for its electrochemical performance in a high-purity CO2 atmosphere, and the test temperature is controlled at 30-35 ℃.

[0015] In the above application, the Li-CO2 flexible battery is assembled in a glove box with Ar atmosphere. The electrolyte is configured with lithium bis(trifluoromethanesulfonyl)imide as lithium salt dissolved in tetraethylene glycol dimethyl ether solvent. The battery negative electrode is lithium foil, and the diaphragm is glass fiber. The electrolyte is dripped on both sides of the diaphragm, and a total of 20-60 μL of electrolyte is dripped. The MXene flexible self-supporting film is cut into 1*3cm strips and directly used as the positive electrode. Copper wire is used as the conductor, and the obtained flexible strip battery is enclosed in a heat-shrinkable insulating sleeve. Several small holes are left on the positive electrode side to facilitate the transportation of CO2 gas. The assembled flexible strip battery is tested for its electrochemical performance in a high-purity CO2 atmosphere, and the test temperature is controlled at 30-35 ℃.

[0016] The principle of the present invention is as follows: a certain proportion of a selective etchant is prepared to etch the Al layer in situ to obtain a single layer or a few layers of Ti3C2, and then a hard template method is used to expand the Ti3C2 interlayer spacing by using MgO as a template agent, and at the same time, the microstructure of Ti3C2 is regulated so that Ti3C2 has a rich microchannel structure, which is convenient for ion transmission during the reaction process, and at the same time, the Ti3C2 layer is made wrinkled to increase the specific surface area, and the interlayer collapse of the Ti3C2 reaction process is suppressed to a certain extent, and at the same time, the film-forming property of Ti3C2 is utilized to obtain a flexible and thin Ti3C2 film material through vacuum-assisted filtration as an independent positive electrode of a Li-CO2 battery, so that the Li-CO2 battery has good cycle stability and lower overpotential.

[0017] Optionally, the raw materials required for the preparation of the selective etchant in step (1) are LiF and HCl.

[0018] Optionally, the method used for selectively etching the Al layer in step (1) is heating and stirring in a water bath at a temperature range of 30-60°C.

[0019] Optionally, in the step (2) of stratifying Ti3C2, the pickling reagent is 1 M HCl, and the pickling method is high-speed centrifugation.

[0020] Optionally, in the step (2), the washing method for the stratified treatment of Ti3C2 is high-speed centrifugation, and the precipitate is shaken evenly without being poured out until the precipitate expands and the supernatant is neutral.

[0021] Optionally, the step (2) is to obtain a single layer or a few layers of Ti3C2 by ultrasonic treatment in an ice-water bath.

[0022] Optionally, the step (3) is to obtain micro-regulated Ti3C2 by using a MgO hard template method and a mixing method of stirring at room temperature.

[0023] Optionally, the MgO template used in step (3) is nano-scale particles with a particle size of 30-50 nm.

[0024] Optionally, the step (3) is to remove the MgO template by washing with 3 M glacial acetic acid.

[0025] Optionally, in step (3), in order to obtain a Ti3C2 self-supporting membrane material, a single layer or a few layers of Ti3C2 dispersion is subjected to vacuum-assisted filtration treatment, and then dried at 60°C under a vacuum environment to obtain a naturally formed membrane material.

[0026] Beneficial effects of the present invention: (1) The Ti3C2 self-supporting membrane electrode with rich microchannel structure prepared by the present invention has a significantly increased specific surface area, an increased pore volume, an obvious porous structure, and an increased interlayer spacing, which can provide a shorter transmission path for ion transmission and improve the accessibility of the electrolyte.

[0027] (2) The Li-CO2 battery prepared by the Ti3C2 self-supporting membrane electrode with rich microchannel structure prepared by the present invention has a smaller polarization voltage and better rate performance than the Li-CO2 battery prepared by the unregulated Ti3C2 self-supporting membrane electrode; and the cycle performance is also significantly enhanced.

[0028] (3) The Ti3C2 self-supporting membrane electrode with rich microchannel structure provided by the present invention has good flexibility and can meet the requirements of flexible batteries. In addition, the membrane electrode is light and thin, which effectively reduces the weight of the battery and has positive significance for the development of wearable devices.

[0029] (4) The experimental operation provided by the present invention is simple, low-cost and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a scanning electron microscope image (SEM) of Ti3C2 prepared in Example 1 of the present invention; Figure 2 XRD diffraction patterns of Examples 1, 2, 3, 4 and Comparative Examples 1 and 4 of the present invention; Figure 3 It is a N2 adsorption-desorption curve diagram of Examples 1, 2, 3 and Comparative Example 1 of the present invention; Figure 4 The pore size distribution diagram of Examples 1, 2, 3 and Comparative Example 1 of the present invention; Figure 5 The charge and discharge performance diagrams of the lithium-carbon dioxide batteries of Examples 1, 2, 3, 4 and Comparative Examples 1 and 4 of the present invention; Figure 6 The figure is a charge and discharge performance diagram of the lithium-carbon dioxide battery of Example 1 of the present invention and Comparative Examples 1, 2, and 3; Figure 7 The figure is a rate performance diagram of the lithium-carbon dioxide battery of Examples 1, 2, 4 and Comparative Example 1 of the present invention; Figure 8 The graphs are the cycle performances of the lithium-carbon dioxide batteries of Example 1 and Comparative Example 1 of the present invention; Fig. 9 This is a charge and discharge performance diagram of the flexible belt-type lithium-carbon dioxide battery prepared in Example 1 of the present invention at a current of 20 μA. DETAILED DESCRIPTION

[0031] The present invention is further illustrated by the following examples, but is not limited to the following examples. Example 1

[0032] S1: Place 10 ml of 12 M HCl in a polytetrafluoroethylene liner, dissolve 0.8 g of LiF in the HCl, and then heat and stir in a water bath at 45°C for 15 min to prepare a selective etchant for the Al layer.

[0033] S2: Take 0.5 g Ti3AlC2 and slowly add the etchant, then heat and stir in a water bath at 45 °C for 24 h.

[0034] S3: Transfer the mixed solution prepared in S2 to a 50 ml centrifuge tube, wash with 1M HCl for 2-3 times, and then wash with water for 3 times until the supernatant reaches neutrality, the precipitate begins to swell, and the supernatant becomes dark green. Add 30 ml of ultrapure water again, shake well without pouring out the supernatant, and centrifuge for 3 times.

[0035] S4: After the mixture is shaken, it is placed in an ice-water bath for ultrasonic treatment (temperature 0℃-4℃, ultrasonic frequency 80kHz) for 1 h, and centrifuged again to obtain the supernatant to obtain a single-layer or few-layer Ti3C2 dispersion.

[0036] S5: Take 10 ml of Ti3C2 dispersion (concentration is 10 mg / ml), weigh 600 mg of MgO, add it to the Ti3C2 dispersion and stir at room temperature for 24 h.

[0037] S6: Then, it was washed with 3 M glacial acetic acid for 3 times, washed with water for 3 times, and 30 ml ultrapure water was added and shaken for 20 min to obtain the expanded Ti3C2 dispersion.

[0038] S7: Use a vacuum filter to filter the Ti3C2 dispersion after MgO expansion to form a film, and then vacuum dry it at 60 °C for 15 h.

[0039] In this example, LiF+HCl is used to prepare a selective etchant to selectively etch the Al layer to obtain Ti3C2, and then dilute hydrochloric acid is used to remove excess etchant, and centrifugation and ultrasound are used to perform stratification to obtain a single-layer or few-layer Ti3C2 dispersion. The MgO hard template method is used to expand the Ti3C2 interlayer spacing, and a vacuum-assisted filtration method is used to synthesize a Ti3C2 self-supporting film.

[0040] The expanded Ti3C2 self-supporting film was used as the air positive electrode, the lithium sheet was used as the negative electrode, and 80 μl of tetraethylene glycol dimethyl ether electrolyte containing lithium salt was added to form a Li-CO2 battery.

[0041] The specific surface area of ​​the Ti3C2 self-supporting film obtained by the above method is 69.81297 m 2 g -1 (See Table 1). MgO template can expand the interlayer spacing of Ti3C2 and micro-regulate the Ti3C2 self-supporting film, so that Ti3C2 forms abundant microchannels and a unique porous structure. At the same time, it prevents interlayer collapse to a certain extent, which is beneficial for the storage of discharge products. Its unique structure provides a shorter diffusion path for ions and electrons, so that the Li-CO2 battery has a lower charging voltage and a smaller overpotential.

[0042] The thin film positive electrode prepared in Example 1 has good mechanical flexibility and meets the basic conditions for being a flexible battery, and the weight of the prepared flexible battery is only 0.3 g. Example 2

[0043] The same as in Example 1, the amount of MgO added was 200 mg, and other conditions remained unchanged to obtain a Ti3C2 self-supporting film. The Ti3C2 self-supporting film was obtained by the above method. The ratio of MgO added in this example was not optimal, and the interlayer spacing was expanded (see Table 1), but the effective specific surface area was small (38.86750 m 2 g -1 ), the pore volume is small, the discharge product storage sites are few, and the rate performance of Li-CO2 batteries is Figure 7 shown. Example 3

[0044] The same as in Example 1, the amount of MgO added was 400 mg, and other conditions remained unchanged to obtain a Ti3C2 self-supporting film. The Ti3C2 self-supporting film was obtained by the above method. The proportion of MgO added in this example is not the optimal ratio. The performance of the Li-CO2 battery is as follows Figure 5 shown. Example 4

[0045] The same as in Example 1, the amount of MgO added was 800 mg, and other conditions remained unchanged to obtain a Ti3C2 self-supporting film. The Ti3C2 self-supporting film was obtained by the above method. The proportion of MgO added in this example is not the optimal ratio. The performance of the Li-CO2 battery is as follows Figure 5 and 7 shown.

[0046] Comparative Example 1: The same as Example 1, without adding MgO, and other conditions remain unchanged, to obtain a Ti3C2 self-supporting film. The Ti3C2 self-supporting film is obtained by the above method. In this comparative example, since the MgO template is not used, the interlayer spacing of Ti3C2 is relatively small, the active sites are few, and the effective specific surface area is reduced by only 34.50731 m 2 g -1 , the electron transmission path is blocked and the catalytic performance is limited, resulting in the Li-CO2 battery not having an advantage in overpotential, rate, and cycle performance.

[0047] Comparative Example 2: Same as Comparative Example 1, 2 ml of [BMIM][TFSI] ionic liquid was added as an intercalation agent, and the obtained Ti3C2 powder was dissolved in an ethanol solution and drop-coated on a carbon paper with a diameter of 12 mm as the positive electrode of a button battery. The material obtained by the above method was used as a Li-CO2 air positive electrode, and its battery performance was not superior to that of Example 1, and it had no mechanical flexibility and could not be used in flexible batteries.

[0048] Comparative Example 3: S1: Add 2 g [Emim]PF6 into 30 mL HCl aqueous solution (9 M) and stir magnetically for 10 min.

[0049] S2: Slowly add 1 g Ti3AlC2 powder and stir at 50 °C for 36 h. The product was washed with deionized water until pH = 6, and then the precipitate was vacuum dried at 80 °C for 12 h.

[0050] S3: The Ti3C2 powder obtained by etching with [Emim]PF6 was dissolved in an ethanol solution and dripped onto a carbon paper with a diameter of 12 mm as the positive electrode of a button battery. The material obtained by the above method was used as a Li-CO2 air positive electrode. Although its battery performance was slightly better than that of comparative example 1, it was not superior to that of example 1, and it had no mechanical flexibility and could not be used in flexible batteries.

[0051] Comparative Example 4: S1: Same as S1-S4 in Example 1, to obtain a single-layer or few-layer Ti3C2 dispersion; S2: 0.4 g CuSO4 and 0.15 g sodium citrate were dissolved in 100 ml deionized water and stirred for 15 min, followed by addition of 1.25 M NaOH and 0.03 M vitamin C to obtain a Cu2O dispersion; S3: Take 10 ml of single-layer or few-layer Ti3C2 dispersion and add it to the above Cu2O dispersion and let it stand at room temperature for 1 hour, then wash it with ethanol and deionized water respectively; S4: Use a vacuum filter to filter the mixed dispersion into a membrane and vacuum dry it at 60 °C for 15 h.

[0052] The Ti3C2 self-supporting film was obtained by the above method. The comparative example used Cu2O for intercalation, but did not expand Ti3C2, and the performance of the Li-CO2 battery was inferior to that of Examples 1, 2, 3, and 4.

[0053] Table 1

[0054] It can be seen from Table 1 that Example 1 has the largest specific surface area and the largest pore volume, indicating its obvious porous structure.

[0055] Figure 1 This is a scanning electron microscope (SEM) image of Ti3C2 prepared in Example 1 of the present invention; it can be seen from the figure that the cross-section of the electrode material prepared in Example 1 presents an accordion morphology and has a uniform and neat layered structure, which is convenient for ion transmission.

[0056] Figure 2 The XRD diffraction patterns of Examples 1, 2, 3, 4 of the present invention and Comparative Examples 1 and 4 are shown in FIG. 1 . As can be seen from the figure, the peak of the (002) crystal plane of Example 1 shifts to a small angle, and the corresponding crystal plane spacing increases, indicating that the two-dimensional interlayer spacing is effectively expanded.

[0057] Figure 3 The N2 adsorption-desorption curves of Examples 1, 2, 3 and Comparative Example 1 of the present invention are shown in the figure. It can be seen from the figure that the sample prepared in Example 1 shows a type IV isotherm, indicating the presence of mesopores of 2-50 nm. There is an obvious hysteresis loop in the higher relative pressure range (0.6-1.0), indicating the presence of a rich mesoporous structure.

[0058] Figure 4 The pore size distribution diagram of Examples 1, 2, 3 and Comparative Example 1 of the present invention is shown. It can be seen from the figure that the pore size of the sample prepared in Example 1 is relatively concentrated around 2-50 nm, indicating the presence of abundant mesoporous and macroporous structures.

[0059] Figure 5 The charge and discharge performance diagram of the lithium-carbon dioxide battery of Examples 1, 2, 3, 4 and Comparative Examples 1 and 4 of the present invention is shown in the figure. It can be seen from the figure that: at 10 μA cm -2 At a current density of , the lithium-carbon dioxide battery using the sample prepared in Example 1 as the thin film positive electrode has a smaller polarization voltage of only 0.65V in the first cycle of charge and discharge compared with other examples.

[0060] Figure 6 The charge and discharge performance diagram of the lithium-carbon dioxide battery of Example 1 and Comparative Examples 1, 2, and 3 of the present invention is shown in the figure. It can be seen from the figure that: at 10 μA cm -2 At a current density of , the Li-CO2 battery using the sample prepared in Example 1 as the thin film positive electrode has a smaller polarization voltage of only 0.65V in the first cycle of charge and discharge compared with other comparative examples.

[0061] Figure 7 The figure is a rate performance diagram of the lithium-carbon dioxide battery of Examples 1, 2, 4 and Comparative Example 1 of the present invention; it can be seen from the figure that: at 10-100 μA cm -2 At different current densities, the lithium-carbon dioxide battery using the sample prepared in Example 1 as the thin film positive electrode has better rate performance than other examples, even after 100 μA cm -2 After the high current density returned to 10µA cm -2 Even at low current density, its performance remains stable.

[0062] Figure 8 The cycle performance diagram of the lithium-carbon dioxide battery of Example 1 and Comparative Example 1 of the present invention is shown in the figure. It can be seen from the figure that at 10 μA cm -2 The current density is 100µAh cm -2 Under the above conditions, the Li-CO2 battery using the sample prepared in Example 1 as the thin film positive electrode has better cycle performance than that of Comparative Example 1, and can be stably cycled for about 1800 hours.

[0063] Fig. 9 This is a charge and discharge performance diagram of the flexible belt-type lithium-carbon dioxide battery prepared in Example 1 of the present invention at a current of 20μA; it can be seen from the figure that the flexible belt-type lithium-carbon dioxide battery prepared in Example 1 can be bent and folded at different angles, and has stable charge and discharge performance at a current of 20μA.

Claims

1. A method for regulating microchannels of a MXene flexible self-supporting membrane electrode, characterized in that: The Ti3C2 flexible thin film material with rich microchannel structure was synthesized through the regulation of template. The method comprises using lithium fluoride and concentrated hydrochloric acid as selective etchants to selectively etch the aluminum layer of the MAX phase precursor Ti3AlC2, obtaining a single layer or a few layers of Ti3C2 dispersion by centrifugal ultrasound, and introducing a template agent, wherein the template agent is nano-scale magnesium oxide, and controlling the dosage of the template agent to achieve regulation of the microenvironment of the two-dimensional Ti3C2 thin electrode.

2. A method for preparing a MXene flexible self-supporting membrane electrode based on microchannel regulation, characterized in that The following steps are involved: (1) Selective etching of precursor Ti3AlC2 Place 10-50 mL of 12 M HCl in a polytetrafluoroethylene-lined reactor, dissolve 0.8-4 g of LiF in HCl, and the molar ratio of LiF to HCl is 1:4-1:40, then heat and stir in a water bath to prepare a selective etchant for the Al layer; Take 0.5-5 g Ti3AlC2 and slowly add it to the etchant, the molar ratio of Ti3AlC2 to LiF is 1:10-1:100, then heat and stir in a water bath to fully react; (2) Ti3C2 layering process Transfer the mixed solution in step (1) to a 50 mL centrifuge tube, wash with acid 2-3 times, then wash with water until the supernatant reaches neutrality, the precipitate begins to swell, and the supernatant turns dark green, wash with water again, then shake well without pouring out the supernatant, and centrifuge; after the mixed solution is shaken well, place it in an ice water bath for ultrasonication, and centrifuge again to obtain the supernatant, which is the monolayer or few-layer Ti3C2 dispersion; (3) Micro-control of Ti3C2 using hard template method Take a Ti3C2 dispersion with a concentration of 10 mg / mL, add MgO to the Ti3C2 dispersion at a mass ratio of Ti3C2:MgO = 1:2~1:10 and stir at room temperature for 24 h, then use 3 M glacial acetic acid for acid washing, then wash with water, add ultrapure water, shake well and perform ultrasound to obtain a Ti3C2 dispersion after micro-control; (4) Preparation of Ti3C2 self-supporting film The micro-controlled Ti3C2 dispersion was filtered into a membrane using a vacuum filter and then dried at 60 °C in vacuum.

3. The method for preparing a MXene flexible self-supporting membrane electrode based on microchannel regulation according to claim 2, characterized in that: The temperature range of the water bath heating in step (1) is 30-60°C.

4. The method for preparing a MXene flexible self-supporting membrane electrode based on microchannel regulation according to claim 2, characterized in that: In step (2), the pickling reagent is 1 M HCl, and the pickling method is high-speed centrifugation; the water washing method is high-speed centrifugation.

5. The method for preparing a MXene flexible self-supporting membrane electrode based on microchannel regulation according to claim 2, characterized in that: The parameters of the ice-water bath ultrasonic treatment in step (2) are: temperature 0°C-4°C, ultrasonic frequency 60kHz-120kHz.

6. The method for preparing a MXene flexible self-supporting membrane electrode based on microchannel regulation according to claim 2, characterized in that: The MgO template used in step (3) is nano-sized particles with a particle size of 30-50 nm.

7. A MXene flexible self-supporting membrane electrode obtained by the preparation method according to any one of claims 1 to 6.

8. Use of the MXene flexible self-supporting membrane electrode according to claim 7 in a lithium-carbon dioxide battery.

9. The use according to claim 8, characterized in that: Used for Li-CO2 button cells; Li-CO2 button cells are assembled in a glove box with Ar atmosphere, the electrolyte is configured with lithium bis(trifluoromethanesulfonyl)imide as lithium salt dissolved in tetraethylene glycol dimethyl ether solvent, the battery negative electrode is a metal lithium sheet, the diaphragm is glass fiber, the electrolyte is dripped on both sides of the diaphragm, a total of 80-120 μl of electrolyte is dripped, the MXene flexible self-supporting film is cut into discs with a diameter of 12 mm and directly used as the positive electrode, and a porous metal shell is used as the positive electrode shell to facilitate CO2 gas transportation.

10. The use according to claim 8, characterized in that: Used for Li-CO2 flexible batteries; Li-CO2 flexible batteries are assembled in a glove box with Ar atmosphere. The electrolyte is configured with lithium bis(trifluoromethanesulfonyl)imide as the lithium salt dissolved in tetraethylene glycol dimethyl ether solvent. The battery negative electrode is lithium foil, and the diaphragm is glass fiber. The electrolyte is dripped on both sides of the diaphragm, and a total of 20-60 μL of electrolyte is dripped. The MXene flexible self-supporting film is cut into 1*3cm strips to directly serve as the positive electrode. Copper wire is used as the conductor, and the resulting flexible strip battery is enclosed in a heat-shrinkable insulating sleeve. Several small holes are left on the positive electrode side to facilitate the transport of CO2 gas.

Citation Information

Patent Citations

  • Mxene flexible self-supporting lithium-air battery positive electrode material, preparation method thereof, Mxene flexible composite membrane and preparation method of Mxene flexible composite membrane

    CN112072126A

  • Ti3C2Tx-MXene flexible self-supporting film and preparation method thereof

    CN113493207A

  • Ultralight porous aerogel based on MXene-graphene compounding, preparation method and application

    CN115939423A

  • Nanometer MoSe2-coated MXene positive electrode catalyst for lithium carbon dioxide battery and preparation method of nanometer MoSe2-coated MXene positive electrode catalyst

    CN117117218A

  • Preparation method of three-dimensional porous flexible self-supporting film electrode material

    CN118156060A