High-sodium-permeability high-entropy oxygen fluorine sodium vanadium phosphate positive electrode material and preparation method thereof

By introducing a variety of adjustable transition metal elements into Vanadium-oxyfluorophosphate and adopting solid-phase thermally coupled sintering method, the problem of low conductivity of Vanadium-oxyfluorophosphate is solved, and hyperosmotic sodium hyperentropy vanadium-oxyfluorophosphate is achieved The performance of vanadium cathode materials is improved and the simplicity and low cost of industrial production.

CN118983439AActive Publication Date: 2024-11-19XI AN JIAOTONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411079546.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The intrinsic conductivity of sodium vanadium phosphate is low, which limits its electrochemical performance and application development. The existing modification methods have problems such as harsh conditions, limited performance improvement, complex preparation process and high cost, and have failed to effectively promote it. Industrial production and application.

Method used

A variety of adjustable transition metal elements are used to replace part of vanadium, and a hypertonic sodium high-structure entropy vanadium phosphate sodium positive electrode material is prepared by a one-step solid-phase thermal coupling sintering method. A material with stable morphology, excellent performance and uniformity is designed to simplify the Process flow and reduce costs.

Benefits of technology

The configuration entropy, structural stability, charge and discharge voltage, sodium ion diffusion rate and electronic conductivity of the material are significantly improved, and the excellent performance of sodium battery positive electrode material is obtained, which is simple in process, low in cost, and is easy to produce on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004983311140000011
    Figure HDA0004983311140000011
  • Figure HDA0004983311140000012
    Figure HDA0004983311140000012
  • Figure HDA0004983311140000021
    Figure HDA0004983311140000021
Patent Text Reader

Abstract

The invention relates to a high-sodium-permeability high-entropy oxygen fluorine sodium vanadium phosphate positive electrode material and a preparation method thereof, the molecular formula of the material is Na3V2-x (TM) x (PO4) 2F3-eta O eta / 2, 0 lt; xlt; 2, 0lt; eta < lt >; 3, preparing by adopting a one-step high-temperature solid-phase thermal coupling sintering method, and ensuring that the raw materials are uniformly mixed and dissolved through a solvent; the nucleation growth and the product synthesis rate of the high-sodium-permeability and high-entropy material are regulated and controlled by using an additive; the problems of non-uniform drying, external coke and internal growth and the like are solved by adopting microwave control drying, a homogeneous precursor is helped to be formed, and the material preparation quality and efficiency are improved; thermodynamic coupling sintering is carried out by pressing a flaky precursor in combination with temperature order regulation and control, so that nucleation, growth and agglomeration kinetics of crystal seeds are improved; the high-sodium-permeability and high-entropy oxygen fluorine sodium phosphate positive electrode material which is accurate in structure, good in crystallization and uniform in particle is prepared, shows excellent electrochemical performance and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation and application of a high-performance positive electrode material for a sodium battery, and in particular to a high-permeability sodium and high-structural entropy sodium oxyvanadium fluorophosphate positive electrode material and a preparation method thereof. Background Art

[0002] With the development of industrialization and modernization, the global demand for energy is growing rapidly. Energy storage technologies used in renewable energy generation and new power systems, such as large-scale pumped storage, battery energy storage technology, and hydrogen energy storage technology, have received widespread attention. As an emerging battery energy storage technology, rechargeable sodium batteries are suitable for application scenarios such as low-speed, short-range electric vehicles and large-scale energy storage power stations due to their advantages such as long cycle life, wide temperature range and low cost, showing broad application prospects.

[0003] The positive electrode material is the key to determining the performance and cost of sodium batteries. The widely studied positive electrode materials for sodium batteries currently include polyanion compounds, layered oxides and Prussian materials. Among them, polyanion positive electrode materials have excellent thermal stability, safety and good cycle performance. In particular, polyanion sodium vanadium oxyfluorophosphate positive electrode materials have super stable three-dimensional framework structure and significant advantages such as high working voltage, high energy density, and small charge and discharge volume change. It is a potential sodium battery positive electrode material. However, the intrinsic conductivity of sodium vanadium oxyfluorophosphate is low, resulting in its electrochemical properties such as rate performance being unsatisfactory, which limits its development and application.

[0004] To this end, traditional modification techniques such as ion doping, surface coating and material composite have been used to enhance the conductivity of sodium vanadium oxyfluorophosphate, thereby improving its actual electrochemical performance. For example, Yang Ju et al. prepared iron-doped Na3V 2-x Fe x (PO4)2F3 (Chemical Engineering Journal, 2024, 485: 149834.), which promotes Na + The transfer of the material during the charge and discharge process reduces the structural deterioration of the material; Zhuang Shuhan et al. prepared aluminum-doped Na3V by the sol-gel method. 2-x Al x (PO4)2F3 (Surface & Coatings Technology, 2022, 434: 128184.), which improves the electronic conductivity and sodium ion diffusion rate of the material, thereby improving the electrochemical performance of sodium vanadium oxyfluorophosphate; He Jiarong et al. prepared rGO-coated stacked Na3(VO x PO4)2F 3-2x@NVP fine core-shell structure, based on the synergistic effect of the core-shell structure and rGO, improves the rate performance of the material (《ACS Applied Materials & Interfaces, 2021, 13(50): 60099-114.》). However, this type of modification method has problems such as harsh modification conditions, limited performance improvement, complex preparation process, and large cost increase, and fails to effectively promote the industrial production and application of sodium vanadium oxyfluorophosphate. Summary of the Invention

[0005] Aiming at the problems in the prior art, the purpose of the present invention is to provide a high-sodium and high-configurational-entropy sodium vanadium oxyfluorophosphate cathode material and its preparation method. By selecting a variety of adjustable transition metal elements to replace part of vanadium, a high-sodium and high-configurational-entropy sodium vanadium oxyfluorophosphate cathode material with stable morphology, excellent performance, and good uniformity is prepared through a one-step solid-phase thermo-mechanical coupling sintering method, which has the characteristics of simplicity and controllability.

[0006] To achieve the above purpose, the present invention provides the following technical solutions:

[0007] A high-sodium and high-configurational-entropy sodium vanadium oxyfluorophosphate cathode material, with the molecular formula Na3V 2-x (TM) x (PO4)2F 3-η O η / 2 , where 0 < x < 2, 0 < η < 3, and TM is a variety of adjustable transition metal elements, including Ti, Cr, Mn, Fe, Co, Ni, Cu, Zn, Al, Mg, Li, Ca, Zr, Nb, Mo, Cd, Ga, In, Y, Ba, Sn, Sb, or Bi;

[0008] For the high-sodium and high-configurational-entropy sodium vanadium oxyfluorophosphate cathode material, the configurational entropy △S conf is 1.4R to 1.8R;

[0009] For the high-sodium and high-configurational-entropy sodium vanadium oxyfluorophosphate cathode material, D Na + is 1×10 -8 ~1×10 -11 cm 2 s -1 .

[0010] A preparation method of a high-sodium and high-configurational-entropy sodium vanadium oxyfluorophosphate cathode material, comprising the following steps:

[0011] Step S1, mixing and dissolving a sodium source, a vanadium source, a phosphorus source, a fluorine source, and a transition metal source in a solvent, adding an additive and a reducing agent, and wet-mixing and grinding evenly to obtain a mixed solution;

[0012] Step S2, subjecting the mixed solution obtained in Step S1 to microwave-controlled drying to obtain a mixed powder;

[0013] Step S3, grinding the mixed powder obtained in step S2 and pressing it into a sheet precursor;

[0014] Step S4, under atmosphere protection conditions, the sheet precursor obtained in step S3 is subjected to thermomechanical coupling sintering, then cooled to room temperature, and ground and sieved to obtain a high-permeability sodium and high-structural entropy sodium oxyvanadium fluorophosphate positive electrode material with uniform particle size.

[0015] The sodium source in step S1 includes: a mixture of one or more of NaCl, Na2O, NaNO3, Na2S2O3, Na2SO4, Na2CO3, Na3PO4, Na2HPO4, CH3COONa, C6HNaO7, NaOH, NaF, sodium dodecyl sulfate, and sodium glycinate in any proportion.

[0016] The vanadium source in step S1 includes: a mixture of one or more of V2O5, V2O3, VOSO4, NH4VO3, Na3VO4, vanadium acetylacetonate, and vanadyl acetylacetonate in any proportion.

[0017] The phosphorus source in step S1 includes: a mixture of one or more of Na3PO4, Na2HPO4, Na4P2O7, NH4H2PO4, (NH4)2HPO4, H3PO4, (NH4)2HPO3, NH4H2PO2, and diphenyl phosphite in any proportion.

[0018] The fluorine source in step S1 includes: a mixture of one or more of NaF, H2SiF6, HF, NH4F, CF4, CaF2, AlF3, CHF3, C2F6, tetrabutylammonium fluoride, and polytetrafluoroethylene in any proportion.

[0019] The transition metal source in step S1 includes a mixture of carbonates, nitrates, sulfates, oxides or hydroxides of five or more different metal elements; the carbonates, nitrates, sulfates, oxides or hydroxides of different metal elements specifically include: NiCO3, Ni(NO3)2·6H2O, MgCO3, MgSO4, Mg(NO3)2·6H2O, Al(NO3)3·9H2O, Al2(CO3)3, Cr(NO3)3·9H2O, CuSO4, Cu(NO3)2·3H2O, Fe(NO3)3·9H2O, Li2CO3, LiNO3, Li2SO4, CoCO3, Co(NO3)2·6H2O, MnCO3, Mn(NO3)2, CaCO3, Ca(NO3)2.

[0020] In the transition metal sources of five or more different metal elements, the content of each element is in an equimolar ratio.

[0021] The solvent in the step S1 is one or more of anhydrous ethanol, acetone, and deionized water in any proportion of a mixed solvent.

[0022] The additives in the step S1 include: one or more of benzene, ethyl benzoate, ethyl acetate, PVDF, DMSO, chloroform, DMF, PTFE, PEG, THF, and EC in any proportion of a mixture.

[0023] The reducing agents in the step S1 include: one or more of graphene, acetylene black, conductive carbon black, graphite, mesoporous carbon, carbon nanotubes, sucrose, glucose, sucrose, sodium thiosulfate, and sodium nitrite in any proportion of a mixture.

[0024] In the step S1, the molar ratio of the added sodium source, vanadium source, phosphorus source, fluorine source, and transition metal source is 3:2 - x:2:3 - η:x, where 0 < x < 2 and 0 < η < 3.

[0025] In the step S1, the mass fraction of the additive is 0.2% - 25% of the total mass of the raw materials.

[0026] In the step S1, the mass fraction of the reducing agent is 1% - 35% of the total mass of the raw materials.

[0027] In the step S2, the working power w of the microwave drying is adjusted, where 0 < w ≤ 2 kW, and the drying time is 3 - 30 min.

[0028] The atmosphere in the step S4 includes: one of nitrogen, argon, hydrogen - argon mixture, or nitrogen - hydrogen mixture; the hydrogen - argon mixture is a hydrogen - argon mixture with a hydrogen volume concentration of 2%; the nitrogen - hydrogen mixture is a nitrogen - hydrogen mixture with a nitrogen volume concentration of 5%.

[0029] In the step S4, the thermo - mechanical coupling sintering is carried out using one - stage, two - stage, or three - stage temperature ramps for sintering; if using one - stage temperature ramp, the sintering temperature is 500 - 950 °C and the sintering time is 0.2 - 20 h; if using two - stage temperature ramps, the sintering temperatures are 300 - 600 °C and 500 - 950 °C respectively, and the sintering times are 0.1 - 6 h and 0.1 - 20 h respectively; if using three - stage temperature ramps, the sintering temperatures are 100 - 400 °C, 300 - 700 °C, and 600 - 950 °C respectively, and the sintering times are 0.1 - 6 h, 0.1 - 6 h, and 0.1 - 20 h respectively.

[0030] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0031] (1) The present invention adopts crystal structure engineering and high entropy material theory and technology to design a high-sodium permeability and high-structural entropy sodium oxyfluorophosphate vanadium positive electrode material. The intrinsic crystal structure and electrochemical performance of sodium oxyfluorophosphate are cleverly and effectively regulated by equal proportions of transition metal elements such as Ni, Mg, Al, Cr, Cu, Fe, Li, Co, Mn, and Ca. The molecular composition and crystal structure are special, which can significantly increase the material configuration entropy and sodium permeability, improve the structural stability, charge and discharge voltage, sodium ion diffusion rate and electronic conductivity, and obtain a sodium battery positive electrode material with excellent performance. △S conf 1.4R~1.8R, stable structure, high charge and discharge voltage; high sodium permeation rate, D Na + 1×10 -8 ~1×10 -11 cm 2 s -1 , the sodium ion diffusion rate and electronic conductivity are high, and the charge and discharge rate is fast.

[0032] (2) The high-permeability sodium and high-structural entropy sodium oxyvanadium fluorophosphate positive electrode material of the present invention is prepared by sintering using a one-step high-temperature solid-phase thermomechanical coupling method, which has abundant raw material sources, simple processes, low preparation costs, and is easy to mass produce.

[0033] (3) The present invention uses solvents to ensure uniform mixing and dissolution of raw materials, and further regulates the nucleation growth of high-osmotic sodium and high-structural entropy materials through additives to improve the product synthesis rate.

[0034] (4) The present invention uses microwave controlled drying to not only solve the process problems of uneven drying and material coke generation, but also helps to form a homogeneous precursor. In addition, the puffing effect of microwave controlled drying is conducive to subsequent further grinding, improving the quality and efficiency of material preparation.

[0035] (5) The present invention utilizes the combination of pressed flake precursors and temperature step control to perform thermomechanical coupled sintering, which effectively improves the kinetics of seed nucleation, growth and agglomeration, and obtains a synthetic product with precise structure, good crystallization and uniform particles.

[0036] In summary, the present invention utilizes crystal structure engineering and high entropy material theory and technology to design and improve the intrinsic electronic conductivity and sodium permeability of sodium vanadium oxyfluorophosphate from the source of the material crystal structure, and inhibits its undesirable phase transition during charging and discharging, and develops sodium vanadium oxyfluorophosphate with high permeability and high structural entropy, which effectively improves the structural entropy, stability, conductivity and sodium permeability of sodium vanadium oxyfluorophosphate, and significantly improves the specific capacity, rate and cycle of sodium vanadium oxyfluorophosphate. The present invention adopts a one-step solid-phase thermomechanical coupling sintering method to cleverly and controllably prepare sodium vanadium oxyfluorophosphate with high permeability and high structural entropy, which has simple process, stable structure, uniform morphology, low cost and excellent performance, and is expected to promote and accelerate the scale production and application process of such materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is the XRD spectrum of the high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate material of Example 1 of the present invention.

[0038] Figure 2 This is a SEM image of the high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate material of Example 2 of the present invention.

[0039] Figure 3 This is the constant current charge and discharge curve of the high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate material of Example 2 of the present invention.

[0040] Figure 4 This is a long cycle performance diagram of the high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate material of Example 3 of the present invention. DETAILED DESCRIPTION

[0041] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0042] Example 1

[0043] The high-osmotic sodium and high-structural entropy sodium oxyfluorophosphate material of this embodiment is expressed as:

[0044] VtV 1.5 (Ni,Mg,Al,Cr,Cu) 0.5 (PO4)2F2O

[0045] The preparation method of the high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate material of this embodiment comprises the following steps:

[0046] 1. Mix and dissolve a sodium source, a vanadium source, a phosphorus source, a fluorine source, and a transition metal source in a molar ratio of 3:1.5:2:2:0.5 in a solvent, add 5wt.% of an additive and 8wt.% of a reducing agent, and wet-mix and grind them uniformly;

[0047] 2. The mixed solution is dried by microwave control, with a working power of 1 kW and a drying time of 20 min;

[0048] 3. Grind the mixed powder evenly and press it into a flake precursor;

[0049] Fourth, under the condition of atmosphere protection, the sheet precursor is sintered by thermal coupling in two stages. The temperature of the first stage is 350℃ and the holding time is 1h; then it enters the second temperature stage for sintering, the sintering temperature is 750℃ and the sintering time is 6h; then it is cooled to room temperature. After grinding and screening, a high-permeability sodium, high-structural entropy sodium oxyfluorophosphate positive electrode material with uniform particle size is obtained.

[0050] The sodium source is a mixture of Na2CO3 and NaF.

[0051] The vanadium source is V2O5.

[0052] The phosphorus source is NH4H2PO4.

[0053] The fluorine source is NaF.

[0054] The transition metal source is a mixture of NiCO3, MgCO3, Al(NO3)3·9H2O, Cr(NO3)3·9H2O, and Cu(NO3)2·3H2O.

[0055] The solvent is a mixed solvent of anhydrous ethanol and deionized water in a mass ratio of 8:2.

[0056] The additive is a mixture of PVDF and PTFE in a mass ratio of 4:6.

[0057] The reducing agent is a mixture of conductive carbon black and sucrose in a mass ratio of 7:3.

[0058] The protective atmosphere is argon.

[0059] Figure 1 The XRD diagram of the high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate material prepared in Example 1 of the present invention has sharp diffraction peaks, good crystallinity, and no obvious by-products, indicating that the increase in entropy is beneficial to promoting the formation of a single-phase material.

[0060] Example 2

[0061] The high-osmotic sodium and high-structural entropy sodium oxyfluorophosphate material of this embodiment is expressed as:

[0062] VtV 1.9 (Ni,Mg,Al,Fe,Mn) 0.1 (PO4)2F2O

[0063] The high permeability sodium and high structural entropy sodium oxyfluorophosphate vanadium positive electrode material has high structural entropy, △S conf 1.4R~1.8R, stable structure, high charge and discharge voltage;

[0064] The high sodium permeability and high structural entropy sodium oxyfluorophosphate vanadium positive electrode material has a high sodium permeability, D Na + 1×10 -8 ~1×10 - 11 cm 2 s -1 , the sodium ion diffusion rate and electronic conductivity are high, and the charge and discharge rates are fast.

[0065] The preparation method of the high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate material of this embodiment comprises the following steps:

[0066] 1. Mix and dissolve a sodium source, a vanadium source, a phosphorus source, a fluorine source, and a transition metal source in a molar ratio of 3:1.9:2:2:0.1 in a solvent, add 10 wt.% of an additive and 10 wt.% of a reducing agent, and wet-mix and grind them uniformly;

[0067] 2. The mixed solution was dried by microwave control, with an operating power of 1 kW and a drying time of 16 min.

[0068] 3. Grind the mixed powder evenly and press it into a flake precursor;

[0069] 4. Under the condition of atmosphere protection, the sheet precursor is subjected to thermal coupling sintering, sintering is performed in a temperature step, the sintering temperature is 750℃, the sintering time is 10h, and then cooled to room temperature. After grinding and screening, a high-permeability sodium, high-structural entropy sodium oxyfluorophosphate positive electrode material with uniform particle size is obtained.

[0070] The sodium source is a mixture of NaOH, Na2CO3 and NaF.

[0071] The vanadium source is NH4VO3.

[0072] The phosphorus source is a mixture of H3PO4 and NH4H2PO4.

[0073] The fluorine source is a mixture of NaF and NH4F.

[0074] The transition metal source is a mixture of Ni(NO3)2·6H2O, Mg(NO3)2·6H2O, Al(NO3)3·9H2O, Fe(NO3)3·9H2O and Mn(OH)2.

[0075] The solvent is anhydrous ethanol solvent.

[0076] The additive is a mixture of PEG and PVDF in a mass ratio of 2:8.

[0077] The reducing agent is a mixture of graphene, glucose and acetylene black in a mass ratio of 0.5:2.5:7.

[0078] The protective atmosphere is a hydrogen-argon mixed gas containing 2% hydrogen by volume.

[0079] Figure 2 , Figure 3 They are respectively the SEM image and the constant current charge-discharge curve of the high-osmotic sodium high-structural entropy sodium oxyfluorophosphate material prepared in Example 2 of the present invention. Figure 2 From the SEM image, it can be seen that the sample morphology is irregularly shaped secondary particles with some slight agglomeration. Figure 3The charge-discharge curves show that the material has a high charge-discharge voltage platform, the first-cycle Coulomb efficiency is as high as 95.37%, and the reversible specific capacities at 0.1C, 1C, 5C, 10C, 20C, and 40C rates are 132, 108, 83, 70, 56, and 41 mAh g, respectively. -1 After 500 cycles at a current density of 1C, the capacity retention rate is as high as 81.2%, indicating that the high sodium permeability and high structural entropy sodium vanadium oxyfluorophosphate material effectively improves the material's configurational entropy, sodium permeability rate and actual electrochemical performance by regulating the crystal structure of sodium vanadium oxyfluorophosphate.

[0080] Example 3

[0081] The high-osmotic sodium and high-structural entropy sodium oxyfluorophosphate material of this embodiment is expressed as:

[0082] VtV 1.85 (Ni,Mg,Al,Cr,Cu,Li) 0.15 (PO4)2F2O

[0083] The method for preparing the sodium vanadium oxyfluorophosphate material with high permeability and high structural entropy comprises the following steps:

[0084] 1. Mix and dissolve a sodium source, a vanadium source, a phosphorus source, a fluorine source, and a transition metal source in a molar ratio of 3:1.85:2:2:0.15 in a solvent, add 10 wt.% of an additive and 5 wt.% of a reducing agent, and wet-mix and grind them uniformly;

[0085] 2. The mixed solution was dried by microwave control, with a working power of 1.5 kW and a drying time of 8 min;

[0086] 3. Grind the mixed powder evenly and press it into a flake precursor;

[0087] 4. Under the condition of atmosphere protection, the sheet precursor was subjected to thermal coupling sintering at a temperature of 700°C and a sintering time of 8 hours, and then cooled to room temperature. After grinding and screening, a high-permeability sodium and high-structural entropy sodium oxyfluorophosphate vanadium positive electrode material with uniform particle size was obtained.

[0088] Fourth, under the condition of atmosphere protection, the sheet precursor is sintered by thermal coupling in three stages. The temperature of the first stage is 400℃ and the holding time is 0.5h; then it enters the second temperature stage for sintering, the sintering temperature is 500℃ and the sintering time is 5h; finally, it enters the third temperature stage for sintering, the sintering temperature is 700℃ and the sintering time is 8h; then it is cooled to room temperature. After grinding and screening, a high-permeability sodium, high-structural entropy sodium oxyfluorophosphate positive electrode material with uniform particle size is obtained.

[0089] The sodium source is a mixture of Na2CO3 and NaF.

[0090] The vanadium source is a mixture of V2O5 and NH4VO3 in a molar ratio of 1:1.

[0091] The phosphorus source is NH4H2PO4.

[0092] The fluorine source is NaF.

[0093] The transition metal source is a mixture of Ni(NO3)2·6H2O, Mg(NO3)2·6H2O, Al(NO3)3·9H2O, Cr(NO3)3·9H2O, Cu(NO3)2·3H2O and Li2CO3.

[0094] The solvent is a mixed solvent of anhydrous ethanol and deionized water.

[0095] The additive is a mixture of PTFE and DMSO in a mass ratio of 9:1.

[0096] The reducing agent is a mixture of conductive carbon black, sucrose and carbon nanotubes in a mass ratio of 8:1.5:0.5.

[0097] The protective atmosphere is a nitrogen-argon mixed gas with a nitrogen content of 5% by volume.

[0098] Figure 4 This is a long cycle performance diagram of the high-osmotic sodium and high-structural entropy sodium vanadium oxyfluorophosphate material of Example 3 of the present invention. After 500 cycles at a rate of 1C, the capacity retention rate is as high as 80%, and the Coulomb efficiency is basically always maintained at around 100%, indicating that the high-osmotic sodium and high-structural entropy sodium vanadium oxyfluorophosphate material effectively improves the cycle stability of the material and significantly improves the electrochemical properties of the sodium vanadium oxyfluorophosphate material.

Claims

1. A high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate positive electrode material, characterized in that: Molecular formula: Na3V 2-x (TM) x (PO4)2F 3-η O η / 2 , where 0 < x < 2, 0 < η < 3, and TM is a variety of adjustable transition metal elements, including Ti, Cr, Mn, Fe, Co, Ni, Cu, Zn, Al, Mg, Li, Ca, Zr, Nb, Mo, Cd, Ga, In, Y, Ba, Sn, Sb, or Bi; The high permeability sodium high configuration entropy sodium oxyfluorophosphate vanadium positive electrode material, configuration entropy △S conf 1.4R~1.8R; The high permeability sodium high structural entropy sodium oxyfluorophosphate vanadium positive electrode material, D Na + 1×10 -8 ~1×10 -11 cm 2 s -1 .

2. A method for preparing a high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate positive electrode material, characterized in that: The following steps are involved: Step S1, mixing and dissolving a sodium source, a vanadium source, a phosphorus source, a fluorine source, and a transition metal source in a solvent, adding an additive and a reducing agent, and wet-mixing and grinding them uniformly to obtain a mixed solution; Step S2, subjecting the mixed solution obtained in step S1 to microwave controlled drying to obtain a mixed powder; Step S3, grinding the mixed powder obtained in step S2 and pressing it into a sheet precursor; Step S4, under atmosphere protection conditions, the sheet precursor obtained in step S3 is subjected to thermomechanical coupling sintering, then cooled to room temperature, and ground and sieved to obtain a high-permeability sodium and high-structural entropy sodium oxyvanadium fluorophosphate positive electrode material with uniform particle size.

3. The method for preparing a high-osmotic sodium and high-structural entropy sodium oxyvanadium fluorophosphate positive electrode material according to claim 2, characterized in that: The sodium source in step S1 includes: a mixture of one or more of NaCl, Na2O, NaNO3, Na2S2O3, Na2SO4, Na2CO3, Na3PO4, Na2HPO4, CH3COONa, C6HNaO7, NaOH, NaF, sodium dodecyl sulfate, and sodium glycinate in any proportion; The vanadium source in step S1 includes: a mixture of one or more of V2O5, V2O3, VOSO4, NH4VO3, Na3VO4, vanadium acetylacetonate, and vanadyl acetylacetonate in any proportion; The phosphorus source in step S1 includes: a mixture of one or more of Na3PO4, Na2HPO4, Na4P2O7, NH4H2PO4, (NH4)2HPO4, H3PO4, (NH4)2HPO3, NH4H2PO2, and diphenyl phosphite in any proportion; The fluorine source in step S1 includes: a mixture of one or more of NaF, H2SiF6, HF, NH4F, CF4, CaF2, AlF3, CHF3, C2F6, tetrabutylammonium fluoride, and polytetrafluoroethylene in any proportion; The transition metal source in step S1 includes a mixture of carbonates, nitrates, sulfates, oxides or hydroxides of five or more different metal elements; the carbonates, nitrates, sulfates, oxides or hydroxides of different metal elements specifically include: NiCO3, Ni(NO3)2·6H2O, MgCO3, MgSO4, Mg(NO3)2·6H2O, Al(NO3)3·9H2O, Al2(CO3)3, Cr(NO3)3·9H2O, CuSO4, Cu(NO3)2·3H2O, Fe(NO3)3·9H2O, Li2CO3, LiNO3, Li2SO4, CoCO3, Co(NO3)2·6H2O, MnCO3, Mn(NO3)2, CaCO3, Ca(NO3)2; The solvent in step S1 is one or more mixed solvents of anhydrous ethanol, acetone, and deionized water in any proportion; The additives in the step S1 include one or more of benzene, ethyl benzoate, ethyl acetate, PVDF, DMSO, chloroform, DMF, PTFE, PEG, THF, EC and any proportion mixture thereof; The reducing agents in the step S1 include one or more of graphene, acetylene black, conductive carbon black, graphite, mesoporous carbon, carbon nanotubes, sucrose, glucose, sucrose, sodium thiosulfate, sodium nitrite and any proportion mixture thereof.

4. The preparation method of a high-osmotic sodium and high-configurational entropy oxygen fluorophosphate sodium cathode material according to claim 3, characterized in that In the transition metal sources of five or more different metal elements, the content of each element is in an equimolar ratio.

5. The preparation method of a high-osmotic sodium and high-configurational entropy oxygen fluorophosphate sodium cathode material according to claim 2, characterized in that In the step S1, the molar ratio of the added sodium source, vanadium source, phosphorus source, fluorine source, and transition metal source is 3:2 - x:2:3 - η:x, where 0 < x < 2 and 0 < η < 3.

6. The preparation method of a high-osmotic sodium and high-configurational entropy oxygen fluorophosphate sodium cathode material according to claim 2, characterized in that In the step S1, the mass fraction of the additive is 0.2% - 25% of the total mass of the raw materials.

7. The preparation method of a high-osmotic sodium and high-configurational entropy oxygen fluorophosphate sodium cathode material according to claim 2, characterized in that In the step S1, the mass fraction of the reducing agent is 1% - 35% of the total mass of the raw materials.

8. The preparation method of a high-osmotic sodium and high-configurational entropy oxygen fluorophosphate sodium cathode material according to claim 2, characterized in that In the step S2, the working power w of the microwave drying is adjusted, 0 < w ≤ 2 kW, and the drying time is 3 - 30 min.

9. The preparation method of a high-osmotic sodium and high-configurational entropy oxygen fluorophosphate sodium cathode material according to claim 2, characterized in that The atmosphere in the step S4 includes one of nitrogen, argon, hydrogen-argon mixture or nitrogen-hydrogen mixture; the hydrogen-argon mixture is a hydrogen-argon mixture with a hydrogen volume concentration of 2%; the nitrogen-hydrogen mixture is a nitrogen-hydrogen mixture with a nitrogen volume concentration of 5%.

10. The preparation method of a high-osmotic sodium and high-configurational entropy oxygen fluorophosphate sodium cathode material according to claim 2, characterized in that In the step S4, the thermomechanical coupling sintering is carried out using one-stage, two-stage or three-stage temperature ramps for sintering; if using one-stage temperature ramp, the sintering temperature is 500 - 950 °C and the sintering time is 0.2 - 20 h; if using two-stage temperature ramps, the sintering temperatures are 300 - 600 °C and 500 - 950 °C respectively, and the sintering times are 0.1 - 6 h and 0.1 - 20 h respectively; if using three-stage temperature ramps, the sintering temperatures are 100 - 400 °C, 300 - 700 °C, 600 - 950 °C respectively, and the sintering times are 0.1 - 6 h, 0.1 - 6 h, 0.1 - 20 h respectively.

Citation Information

Patent Citations

  • Positive electrode material for transition metal-doped sodium ion battery and preparation and application thereof

    CN109755565A

  • High-entropy doped sodium vanadium fluorophosphate positive electrode material and preparation method thereof

    CN117012918A

  • Method of obtaining composite cathode material based on na3v2 (PO4)2f3 for sodium-ion batteries

    RU2747565C1

  • Vanadium sodium phosphate positive electrode material, sodium ion battery, preparation method therefor, and use thereof

    US20210167387A1

  • Nickel-rich high-voltage sodium-ion positive electrode material for battery, preparation method therefor, and application thereof

    WO2023093180A1