Battery and electric device
By using molecular sieve to adsorb the lithium replenishing agent deliquency product in the positive electrode coating of the battery, and adding unsaturated bond imidazole carboxylic acid ester to the electrolyte, the oxidation and gas release of the electrolyte after the lithium replenishing agent deliquency of the battery is solved. Problem, improving battery performance.
Patent Information
- Application Number
- CN202411076533.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The products of existing battery lithium supplements after deliquification have strong oxidation to the electrolyte, resulting in a decrease in battery performance and the released gases aggravate the oxidation of the electrolyte or the expansion of lithium-ion batteries.
Add molecular sieve to the positive electrode coating to adsorb the product after deliquification of lithium supplement agent, and add imidazole carboxylic acid ester containing unsaturated bonds to the electrolyte to form a stable SEI film, inhibit the oxidation and side reaction of the electrolyte, and reduce the loss of active lithium .
Through the synergistic effect of molecular sieve and unsaturated bond imidazole carboxylic acid ester, the damage of lithium supplement products to the electrolyte is reduced, the loss of active lithium is reduced, the battery performance is improved, the electrolyte is inhibited from oxidation and gas release, and the battery is improved Overall performance.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery materials, and in particular to a battery and an electrical device. Background Art
[0002] Lithium replenisher refers to a general term for materials that replenish irreversible lithium loss by pre-lithiation of electrode materials. It is one of the important means to solve the problem of irreversible lithium loss in battery materials. At present, the positive lithium replenishers used by major battery factories, material factories, etc. are mainly lithium-rich compounds and binary lithium compounds. However, the products of most lithium replenishers after delithiation have strong oxidizing properties to the electrolyte, and have high requirements for the working window of the electrolyte. In addition, the gas released after lithium replenishment will further aggravate the oxidation of the electrolyte or the expansion of the lithium-ion battery, resulting in reduced battery performance. Summary of the invention
[0003] In view of this, in order to solve the problem of strong oxidizing properties of the electrolyte and gas release caused by the deoxidation of the positive electrode lithium supplement, the present application provides a battery and an electrical device that can effectively suppress the problem of battery performance degradation caused by oxidation of the electrolyte or gas release.
[0004] In a first aspect, the present application provides a battery, the battery comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, the positive electrode sheet comprising a positive electrode current collector and a positive electrode coating disposed on the positive electrode current collector;
[0005] The positive electrode coating comprises a positive electrode active material, a lithium supplement and a molecular sieve;
[0006] The electrolyte includes a negative electrode film-forming additive, and the negative electrode film-forming additive includes an imidazole carboxylate additive containing an unsaturated bond.
[0007] In an optional embodiment, in the positive electrode coating, the content of the lithium supplement agent is 0.5%-3%; the content of the molecular sieve is 0.5%-5%, calculated by mass percentage.
[0008] In an optional embodiment, the content of the unsaturated bond-containing imidazole carboxylate additive in the electrolyte is 0.3%-3% by mass percentage.
[0009] In an optional embodiment, in the electrolyte, the content of the unsaturated bond-containing imidazole carboxylate additive is 0.3%-1.0%;
[0010] And / or, in terms of mass percentage, in the positive electrode coating, the content of the lithium supplement agent is 1%-2%, and the content of the molecular sieve is 1%-3%.
[0011] In an optional embodiment, the unsaturated bond-containing imidazole carboxylate additive includes any one of 2-propyn-1-yl-imidazole-1-carboxylate, 1H-imidazole-1-carboxylate allyl ester and 1H-imidazole-1-carboxylate-3-butene ester or a combination of at least two thereof.
[0012] In an optional embodiment, the electrolyte further comprises a fluorinated solvent and a fluorinated lithium salt;
[0013] The fluorinated solvent includes any one of fluorinated cyclic carbonate, fluorinated linear carbonate, fluorinated linear carboxylate or fluorinated ether or a combination of at least two thereof; in terms of mass percentage, the content of the fluorinated solvent in the electrolyte is 10%-15%;
[0014] The fluorinated lithium salt includes any one of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(trifluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorobis(oxalatophosphate), lithium difluorooxalatoborate, lithium hexafluoroarsenate and lithium bis(trifluoromethanesulfonyl)imide, or a combination of at least two thereof; in terms of mass percentage, the content of the fluorinated lithium salt in the electrolyte is 13.5%-18.0%.
[0015] In an optional embodiment, the electrolyte further comprises cyclic carbonate and / or linear carbonate;
[0016] And / or, the electrolyte further comprises a positive electrode film-forming additive, and the positive electrode film-forming additive comprises tris(trimethylsilyl)phosphate and / or tris(trimethylsilyl)borate.
[0017] In an optional embodiment, the negative electrode active material in the negative electrode sheet includes graphite and / or silicon-containing material;
[0018] And / or, the negative electrode film-forming additive further includes any one or a combination of at least two of vinyl sulfate, methylene methanedisulfonate, 1,3-propane sultone and vinylene carbonate.
[0019] In an optional embodiment, the lithium supplement comprises lithium ferrite and / or lithium nickelate;
[0020] And / or, the positive electrode active material includes any one of lithium iron phosphate, lithium manganese iron phosphate and lithium nickel cobalt manganese oxide, or a combination of at least two thereof.
[0021] In a second aspect, the present application provides an electrical device, comprising the battery.
[0022] Compared with the prior art, the beneficial effects of this application are:
[0023] The battery provided by the present application includes a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet includes a positive electrode current collector and a positive electrode coating located at least on one side of the positive electrode current collector; the positive electrode coating includes a positive electrode active material, a lithium supplement and a molecular sieve; the electrolyte includes an imidazole carboxylate containing an unsaturated bond. The molecular sieve is added to the positive electrode coating in the present application to adsorb the product after the lithium supplement is removed from the lithium supplement, thereby inhibiting the O2 / O 2- Damage to the electrolyte; adding imidazole carboxylates containing unsaturated bonds to the electrolyte not only makes it easy to form a stable SEI film at the negative electrode and reduce the loss of active lithium, but also can combine with lithium replenishment products to inhibit the problem of electrolyte oxidation. The molecular sieve and imidazole carboxylates containing unsaturated bonds work synergistically to reduce the damage of lithium replenishment products to the electrolyte, inhibit the side reactions at the interface between the negative electrode and the electrolyte, reduce the loss of active lithium, and improve battery performance. DETAILED DESCRIPTION
[0024] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.
[0025] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0026] In the present application, the selection scope involving "and / or" includes any one of two or more related listed items, and also includes any and all combinations of the related listed items. For example, "A and / or B" includes three parallel options of A, B and A+B.
[0027] In the present application, "combination" includes all suitable combinations of any two or more of the listed items.
[0028] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0029] In the present application, the percentage content, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and refers to volume percentage for liquid-liquid mixing.
[0030] In this application, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0032] Lithium-ion battery electrolytes are generally composed of carbonate-based organic solvents and lithium salts. These organic solvents will be reduced and decomposed on the surface of the negative electrode during the first charge to form a solid electrolyte interface film containing lithium, namely the SEI film. This process will consume a portion of the active lithium from the positive electrode, reducing the first cycle Coulomb efficiency (ICE) and the energy density of the battery. Graphite is currently the most widely used commercial lithium-ion battery negative electrode material. Due to the above reasons, its first irreversible capacity loss can reach about 10%; and the volume expansion of graphite when used as a negative electrode will destroy the SEI film. The newly exposed graphite continues to generate a new SEI film during the charge and discharge process; the volume change ratio of silicon material when used as a negative electrode is as high as 320%, and its huge volume change causes more serious irreversible lithium loss than other electrodes.
[0033] At present, lithium replenishers are mainly used to solve the above-mentioned irreversible lithium loss problem. However, they are unstable in themselves and have a high lithium replenishment voltage (>4.0V). The products of lithium replenishers after de-lithiation have strong oxidizing properties to the electrolyte, and have high requirements on the working window of the electrolyte. In addition, the gas released after lithium replenishment will further aggravate the oxidation of the electrolyte or the expansion of the lithium-ion battery, resulting in reduced battery performance.
[0034] In order to solve the problems existing in the above-mentioned related technologies, according to the first aspect of the present application, the present application provides a battery, the battery comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, the positive electrode sheet comprising a positive electrode current collector and a positive electrode coating disposed on the positive electrode current collector;
[0035] The positive electrode coating comprises a positive electrode active material, a lithium supplement and a molecular sieve;
[0036] The electrolyte includes a negative electrode film-forming additive, and the negative electrode film-forming additive includes an imidazole carboxylate additive containing an unsaturated bond.
[0037] The present invention adds molecular sieves to the positive electrode coating to remove lithium from the lithium supplement (including O 2- , O2) is adsorbed into the molecular sieve to reduce O2 / O 2- release, inhibiting O2 / O 2-It is understandable that the molecular sieve itself has an adsorption effect. Due to the high quadrupole moment of the molecular sieve and the strong electric field of the molecular sieve, the molecular sieve can achieve the adsorption of O2 / O 2- adsorption.
[0038] At the same time, the present invention adds an imidazole carboxylate containing an unsaturated bond to the electrolyte. On the one hand, the presence of the unsaturated bond (electron-withdrawing group) makes the additive have better reducibility, making it easier to form a stable SEI film on the negative electrode surface, inhibiting the occurrence of side reactions, thereby reducing the loss of active lithium; on the other hand, the imidazole cation in the reduction product of the imidazole carboxylate containing an unsaturated bond is more effective for the lithium supplement product O 2- It has a strong binding ability with O2 and can effectively resist O 2- and O2 attack, inhibiting the side reactions at the negative electrode interface.
[0039] Therefore, the molecular sieve and the imidazole carboxylate containing an unsaturated bond work synergistically to reduce the damage of the lithium supplement product to the electrolyte; moreover, it effectively isolates the negative electrode, inhibits the side reaction at the interface between the negative electrode and the electrolyte, reduces the loss of active lithium, and improves the battery performance.
[0040] In some embodiments, the molecular sieve includes any one or a combination of at least two of Cu-Y molecular sieve, Ce-Y molecular sieve, La-Beta molecular sieve, Zn-ZSM molecular sieve, Rh-ZSM molecular sieve, Ru-Y molecular sieve, Pt-Y molecular sieve and Ce-X molecular sieve.
[0041] The molecular sieve includes metal cations, imidazole carboxylate containing unsaturated bonds and the imidazole groups in its reduction products, which can complex the molecular sieve containing metal cations. The imidazole group contains two nitrogen atoms that can form coordination bonds with the metal ions in the molecular sieve, thereby tightly wrapping the metal ions in the imidazole molecules, complexing the molecular sieve, and promoting the selective adsorption and aggregation of O2 / O in the molecular sieve. 2- And because O2 is adsorbed into the molecular sieve or bound to the reduction product of the unsaturated bond of imidazole carboxylate, after this part of O2 is disproportionated with lithium ions to form Li2O2, Li2O2 will be deposited on the molecular sieve and the positive electrode surface, isolating the positive electrode coating, avoiding the reaction between the positive electrode and the electrolyte, and reducing the release of oxygen; reducing the polarization side reaction in the battery cell during high-rate charge and discharge, and more effectively inhibiting the problem of electrolyte oxidation and the degradation of battery performance due to gas release.
[0042] Therefore, imidazole carboxylates containing unsaturated bonds, on the one hand, can easily form a stable SEI film at the negative electrode due to the reducibility of the unsaturated bonds, thus reducing the loss of active lithium; on the other hand, the imidazole cations in their reduction products can effectively resist O 2-and O2, inhibiting the side reactions at the negative electrode interface; thirdly, the imidazole molecules can also effectively complex the metal ions adsorbed into the molecular sieve, further promoting the molecular sieve to selectively adsorb the aggregated O2 / O 2- , and O2 / O 2- After being disproportionated with lithium ions to become Li2O2, it will also be deposited on the surface of the molecular sieve and the positive electrode, isolating the positive electrode from reacting with the electrolyte and reducing the release of oxygen. It can effectively inhibit the problem of electrolyte oxidation and the performance degradation caused by oxygen release.
[0043] In some embodiments, the molecular sieve includes at least one of Cu-Y molecular sieve, Ce-Y molecular sieve, Ru-Y molecular sieve and Pt-Y molecular sieve. Y molecular sieve is a microporous molecular sieve with a FAU structure, having a large cavity and a three-dimensional twelve-membered ring channel system. And the Y-type molecular sieve has a large specific surface area and pore size; the larger the specific surface area and pore size of the same molecular sieve, the more gas can be adsorbed per unit mass.
[0044] Due to the high quadrupole moment of the molecular sieve and the strong electric field of the molecular sieve, the molecular sieve can adsorb gases. The introduction of imidazole molecules will change the electric field of the molecular sieve framework. Taking Ce-Y molecular sieve as an example, the Ce 3d binding energy of Ce-Y molecular sieve modified by imidazole will increase after the Ce 3d binding energy adsorbs O2. This shows that the Ce site of Ce-Y-imidazole has a unique electron transfer interaction with O2, and more electrons are transferred to O2, thereby achieving selective adsorption of oxygen. In other words, the Ce sites in Ce-Y are activated after imidazole modification, which enables them to preferentially transfer electrons to O2, thereby enhancing the adsorption of O2.
[0045] In some embodiments, in the positive electrode coating, the content of the lithium supplement agent is 0.5%-3%; the content of the molecular sieve is 0.5%-5%, calculated by mass percentage.
[0046] And / or, in the electrolyte, the content of the imidazole carboxylate additive containing an unsaturated bond is 0.3%-3% by mass percentage.
[0047] When the content of molecular sieve is greater than 5%, many uncoordinated metal ion sites will be generated in the molecular sieve. These sites will catalyze the reaction between the positive electrode and the electrolyte, causing the side reaction to increase slightly, and reducing the proportion of positive electrode active materials, which will slightly reduce the battery energy density. When the content of molecular sieve is less than 0.5%, the screening effect will be relatively weak because the molecular sieve content is too low. When the content of imidazole carboxylate additives containing unsaturated bonds is greater than 3%, the negative electrode impedance will increase slightly due to excessive negative electrode film formation, which will slightly affect lithium ion transmission. When the content of imidazole carboxylate additives containing unsaturated bonds is less than 0.3%, it mainly participates in film formation and has a relatively weak complexation effect on the molecular sieve.
[0048] In some embodiments, in the positive electrode coating, the content of the lithium supplement agent is 1%-2%, and the content of the molecular sieve is 1%-3% by mass percentage;
[0049] And / or, in terms of mass percentage, in the electrolyte, the content of the imidazole carboxylate additive containing an unsaturated bond is 0.3%-1.0%.
[0050] In some embodiments, the unsaturated bond-containing imidazole carboxylate additive includes any one or a combination of at least two of 2-propyn-1-yl-imidazole-1-carboxylate, 1H-imidazole-1-carboxylic acid allyl ester and 1H-imidazole-1-carboxylic acid-3-butene ester.
[0051] 2-Propyne-1-yl-imidazole-1-carboxylate, 1H-imidazole-1-carboxylic acid allyl ester and 1H-imidazole-1-carboxylic acid-3-butyl ester have better reducibility and can form a relatively stable SEI film on the negative electrode surface. The substituent of 2-propyne-1-yl-imidazole-1-carboxylate has better reducibility, so the film formation on the negative electrode is more stable.
[0052] In some embodiments, the electrolyte further comprises a fluorinated solvent and a fluorinated lithium salt;
[0053] Calculated by mass percentage, in the electrolyte, the mass content of the fluorinated solvent is 10%-15%; the mass content of the fluorinated lithium salt is 13%-18%.
[0054] The fluorinated solvent includes any one or a combination of at least two of fluorinated cyclic carbonates, fluorinated linear carbonates, fluorinated linear carboxylates or fluorinated ethers;
[0055] The fluorinated lithium salt includes any one of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate, lithium difluorobis(oxalato)phosphate, lithium difluorooxalatoborate, lithium hexafluoroarsenate and lithium bis(trifluoromethanesulfonyl)imide, or a combination of at least two thereof.
[0056] A relatively stable fluorinated solvent is also introduced into the electrolyte of the present application, which can enhance the oxidation resistance and high voltage resistance of the electrolyte and broaden the electrochemical window of the electrolyte. The electronegativity and polarity of the fluorinated solvent give the electrolyte good oxidation resistance. First, the fluorine atom has a strong electronegativity and can effectively attract electrons, thereby reducing the HOMO (highest occupied molecular orbital) and LUMO (lowest unoccupied molecular orbital) energy levels of the fluorinated solvent. This effect of reducing the energy level makes the fluorinated solvent show higher oxidation resistance on the positive electrode side. The low polarity of the fluorine atom helps to reduce the side reactions between the electrolyte and the electrode, enhances the stability of the electrolyte and the electrode, and thus improves the overall antioxidant performance of the battery.
[0057] In addition, the electrolyte composed of fluorinated solvents and fluorinated lithium salts can not only increase the content of fluorine atoms in the electrolyte, further enhancing the oxidation resistance of the electrolyte, but also form an interface film rich in LiF on the surface of the positive electrode, further improving the interface stability of the positive electrode. In the high voltage range where the lithium supplement works, it can effectively inhibit the damage of the electrolyte to the high oxidation of the positive electrode under high voltage, inhibit the side reactions at the electrode / electrolyte interface, and avoid gas production during the subsequent use of the battery.
[0058] In some embodiments, the electrolyte further comprises cyclic carbonate and / or linear carbonate;
[0059] Alternatively, the electrolyte further comprises any one or a combination of at least two of vinyl sulfate (DTD), methylene disulfonate (MMDS), 1,3-propane sultone (PS) and vinyl carbonate (VC);
[0060] Alternatively, the electrolyte further comprises tris(trimethylsilyl)phosphate (TMSP) and / or tris(trimethylsilyl)borate (TMSB).
[0061] In some embodiments, the negative electrode active material in the negative electrode sheet includes graphite and / or silicon.
[0062] In some embodiments, the positive electrode active material includes any one of lithium iron phosphate, lithium iron manganese phosphate, or lithium nickel cobalt manganese oxide, or a combination of at least two thereof.
[0063] And / or, the lithium supplement includes lithium ferrite (Li5FeO4) and / or lithium nickelate (LiNO2).
[0064] In a second aspect, the present invention provides an electric device, comprising the battery. Thus, the electric device has all the features and advantages of the battery, which will not be described in detail here. Exemplarily, the electric device is a pure electric vehicle, a hybrid electric vehicle, etc.
[0065] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0066] The molecular sieves used in the following experiments were purchased from Zhuoyue Environmental Protection New Materials (Shanghai) Co., Ltd.;
[0067] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0068] Example 1
[0069] This embodiment provides a battery, including a positive electrode sheet, a negative electrode sheet and an electrolyte;
[0070] In the positive electrode coating, calculated by mass percentage, it includes 94.1% positive electrode active material (lithium iron phosphate), 1.0% lithium supplement (Li5FeO4), 2.0% Ce-Y molecular sieve, 0.6% Super P conductive agent, 0.5% single-walled carbon nanotube conductive agent and 1.8% polyvinylidene fluoride binder.
[0071] A method for preparing a positive electrode coating and a positive electrode sheet thereof comprises the following steps:
[0072] The above components are mixed according to the formula amount, and then N-methylpyrrolidone solvent is added and mixed evenly to obtain positive electrode slurry, and then the positive electrode slurry is coated on the surface of the positive electrode collector (carbon-coated aluminum foil), and then sliced after drying to form a positive electrode sheet.
[0073] Preparation of negative electrode
[0074] The negative electrode material includes a negative electrode active material (graphite and silicon-carbon composite material, wherein the silicon-carbon composite material is purchased from Lanxi Zhide New Energy Materials Co., Ltd., model S0310), Super P conductive agent, CMC-Na (sodium carboxymethyl cellulose) and styrene-butadiene latex; the graphite, silicon-carbon composite material, Super P conductive agent, CMC-Na and styrene-butadiene latex are mixed in a mass ratio of 90.9:4.8:0.95:1.3:2.0, and then deionized water is added and stirred to obtain a negative electrode slurry, and the negative electrode slurry is coated on the surface of the copper foil, and after drying, the negative electrode sheet is obtained by slicing;
[0075] Preparation of electrolyte
[0076] The electrolyte comprises, by mass percentage, 26% EC (ethylene carbonate), 41.8% EMC (ethyl methyl carbonate), 10% DFEA (ethyl difluoroacetate), 10.9% LiPF6 (lithium hexafluorophosphate), 3% LiFSI (lithium bisfluorosulfonyl imide), 0.5% LiPO2F2 (lithium difluorophosphate), 1% DTD (vinyl sulfate), 0.5% 2-propynyl-1-yl-imidazole-1-carboxylate, 3% VC (vinylene carbonate), 0.3% TMSP (tris(trimethylsilyl) phosphate) and 3.0% FEC (fluoroethylene carbonate); the above components are mixed to form an electrolyte;
[0077] The positive electrode sheet, negative electrode sheet, electrolyte and separator are assembled to form a battery, and then the battery is formed at 45°C (the formation process is: first charge to 3.1V at 0.05C, charge to 3.5V at 0.1C, then charge to 4.1V at 0.05C, and finally discharge to 3.4V at 0.2C). After the formation is completed, the battery is aged and divided to obtain a lithium-ion battery.
[0078] Example 2
[0079] This embodiment provides a battery, which is different from the embodiment 1 only in that:
[0080] The positive electrode coating includes, by mass percentage, 94.1% of positive electrode active material (lithium iron phosphate), 2.0% of lithium supplement (Li2NiO2), 1% of Ru-Y molecular sieve, 0.6% of Super P conductive agent, 0.5% of single-walled carbon nanotube conductive agent and 1.8% of polyvinylidene fluoride binder;
[0081] Electrolyte: The electrolyte includes, by mass percentage, 26% EC (ethylene carbonate), 42% EMC (ethyl methyl carbonate), 10% DFEA (ethyl difluoroacetate), 10.9% LiPF6 (lithium hexafluorophosphate), 3% LiFSI (lithium bis(fluorosulfonyl)imide), 0.5% LiPO2F2 (lithium difluorophosphate), 1% DTD (vinyl sulfate), 0.3% 2-propyn-1-yl-imidazole-1-carboxylate, 3% VC (vinyl carbonate), 0.3% TMSP (tris(trimethylsilyl) phosphate) and 3.0% FEC (fluoroethylene carbonate).
[0082] Example 3
[0083] This embodiment provides a battery, which is different from the embodiment 1 only in that:
[0084] The positive electrode coating includes, by mass percentage, 89.1% of positive electrode active material (lithium iron phosphate), 3.0% of lithium supplement (Li5FeO4), 5% of Cu-Y molecular sieve, 0.6% of Super P conductive agent, 0.5% of single-walled carbon nanotube conductive agent and 1.8% of polyvinylidene fluoride binder;
[0085] Electrolyte: The electrolyte includes, by mass percentage, 26% EC (ethylene carbonate), 41.3% EMC (ethyl methyl carbonate), 10% DFEA (ethyl difluoroacetate), 10.9% LiPF6 (lithium hexafluorophosphate), 3% LiFSI (lithium bisfluorosulfonyl imide), 0.5% LiPO2F2 (lithium difluorophosphate), 1% DTD (vinyl sulfate), 1% 2-propyn-1-yl-imidazole-1-carboxylate, 3% VC (vinyl carbonate), 0.3% TMSP (tris(trimethylsilyl) phosphate) and 3.0% FEC (fluoroethylene carbonate).
[0086] Embodiment 4:
[0087] This embodiment provides a battery, which is different from the embodiment 1 only in that:
[0088] The molecular sieve in Example 1 was replaced with Ce-X molecular sieve.
[0089] Embodiment 5:
[0090] This embodiment provides a battery, which is different from the embodiment 1 only in that:
[0091] The molecular sieve in Example 1 was replaced with La-Beta molecular sieve.
[0092] Embodiment 6:
[0093] This embodiment provides a battery, which is different from the embodiment 1 only in that:
[0094] The unsaturated imidazole carboxylate additive of Example 1 was replaced with 1H-imidazole-1-carboxylic acid allyl ester.
[0095] Embodiment 7:
[0096] This embodiment provides a battery, which is different from the embodiment 1 only in that:
[0097] In the positive electrode coating, calculated by mass percentage, it includes 90.1% positive electrode active material (lithium iron phosphate), 1.0% lithium supplement (Li5FeO4), 6.0% Ce-Y molecular sieve, 0.6% Super P conductive agent, 0.5% single-walled carbon nanotube conductive agent and 1.8% polyvinylidene fluoride binder.
[0098] Embodiment 8:
[0099] This embodiment provides a battery, which is different from the embodiment 1 only in that:
[0100] Electrolyte: The electrolyte includes, by mass percentage, 23% EC (ethylene carbonate), 41.3% EMC (ethyl methyl carbonate), 10% DFEA (ethyl difluoroacetate), 10.9% LiPF6 (lithium hexafluorophosphate), 3% LiFSI (lithium bisfluorosulfonyl imide), 0.5% LiPO2F2 (lithium difluorophosphate), 1% DTD (vinyl sulfate), 4% 2-propyn-1-yl-imidazole-1-carboxylate, 3% VC (vinyl carbonate), 0.3% TMSP (tris(trimethylsilyl) phosphate) and 3.0% FEC (fluoroethylene carbonate).
[0101] Example 9
[0102] This embodiment provides a battery, including a positive electrode sheet, a negative electrode sheet and an electrolyte;
[0103] In the positive electrode coating, calculated by mass percentage, it includes 92.6% positive electrode active material (lithium iron phosphate), 1.5% lithium supplement (Li5FeO4), 3.0% Ce-Y molecular sieve, 0.6% Super P conductive agent, 0.5% single-walled carbon nanotube conductive agent and 1.8% polyvinylidene fluoride binder.
[0104] A method for preparing a positive electrode coating and a positive electrode sheet thereof comprises the following steps:
[0105] The above components are mixed according to the formula amount, and then N-methylpyrrolidone solvent is added and mixed evenly to obtain positive electrode slurry, and then the positive electrode slurry is coated on the surface of the positive electrode collector (carbon-coated aluminum foil), and then sliced after drying to form a positive electrode sheet.
[0106] Preparation of negative electrode
[0107] The negative electrode material includes a negative electrode active material (graphite and silicon-carbon composite material, wherein the silicon-carbon composite material is purchased from Lanxi Zhide New Energy Materials Co., Ltd., model S0310), Super P conductive agent, CMC-Na (sodium carboxymethyl cellulose) and styrene-butadiene latex; the graphite, silicon-carbon composite material, Super P conductive agent, CMC-Na and styrene-butadiene latex are mixed in a mass ratio of 90.9:4.8:0.95:1.3:2.0, and then deionized water is added and stirred to obtain a negative electrode slurry, and the negative electrode slurry is coated on the surface of the copper foil, and after drying, the negative electrode sheet is obtained by slicing;
[0108] Preparation of electrolyte
[0109] The electrolyte comprises, by mass percentage, 26% EC (ethylene carbonate), 41.3% EMC (ethyl methyl carbonate), 10% DFEA (ethyl difluoroacetate), 10.9% LiPF6 (lithium hexafluorophosphate), 3% LiFSI (lithium bisfluorosulfonyl imide), 0.5% LiPO2F2 (lithium difluorophosphate), 1% DTD (vinyl sulfate), 1% 2-propynyl-1-yl-imidazole-1-carboxylate, 3% VC (vinyl carbonate), 0.3% TMSP (tris(trimethylsilyl) phosphate) and 3.0% FEC (fluoroethylene carbonate); the above components are mixed to form an electrolyte;
[0110] The positive electrode sheet, negative electrode sheet, electrolyte and separator are assembled to form a battery, and then the battery is formed at 45°C (the formation process is: first charge to 3.1V at 0.05C, charge to 3.5V at 0.1C, then charge to 4.1V at 0.05C, and finally discharge to 3.4V at 0.2C). After the formation is completed, the battery is aged and divided to obtain a lithium-ion battery.
[0111] Comparative Example 1
[0112] This comparative example provides a battery, including a positive electrode sheet, a negative electrode sheet and an electrolyte, which is different from Example 1 only in that:
[0113] The electrolyte includes, by mass percentage, 26.5% EC (ethylene carbonate), 41.8% EMC (ethyl methyl carbonate), 10% DFEA (ethyl difluoroacetate), 10.9% LiPF6 (lithium hexafluorophosphate), 3% LiFSI (lithium bis(fluorosulfonyl)imide), 0.5% LiPO2F2 (lithium difluorophosphate), 1% DTD (vinyl sulfate), 3% VC (vinylene carbonate), 0.3% TMSP (tri(trimethylsilyl) phosphate) and 3.0% FEC (fluoroethylene carbonate).
[0114] Comparative Example 2
[0115] This comparative example provides a battery, including a positive electrode sheet, a negative electrode sheet and an electrolyte, which is different from Example 1 only in that:
[0116] In the positive electrode coating, by mass percentage, it includes 96.1% positive electrode active material (lithium iron phosphate), 1.0% lithium supplement (Li5FeO4), 0.6% Super P conductive agent, 0.5% single-walled carbon nanotube conductive agent and 1.8% polyvinylidene fluoride binder.
[0117] The lithium ion batteries prepared in the above examples and comparative examples were tested as follows:
[0118] High temperature cycle test:
[0119] The lithium ion batteries in the embodiments and comparative examples were placed in a 45°C constant temperature box, charged to 3.65V at a constant current of 1C, charged to 0.05C at a constant voltage at 3.65V, and then discharged to 2.5V at a constant current of 1C. This was recorded as a charge and discharge cycle, and the initial discharge capacity was recorded; capacity retention rate = (remaining discharge capacity / initial discharge capacity) × 100%, and the number of cycles when the capacity retention rate of the secondary battery was 80% was recorded.
[0120] High temperature storage capacity retention rate:
[0121] The lithium ion batteries in the embodiments and comparative examples were charged to 3.65V at a constant current of 1C at 25°C, charged to 0.05C at a constant voltage at 3.65V, and then discharged to 2.5V at a constant current of 1C. This was recorded as a charge and discharge cycle, and the initial discharge capacity C0 was recorded. After being fully charged again, the lithium ion battery was placed in a 55°C oven. After 180 days of storage, the lithium ion battery was left to stand at room temperature for 2h and discharged to 2.5V at 1C. The remaining discharge capacity of the battery at this time was recorded and the final battery capacity retention rate was calculated, battery capacity retention rate = (remaining discharge capacity / initial discharge capacity) × 100%.
[0122] Storage gas production:
[0123] Volume test method for lithium-ion batteries: Place a beaker filled with deionized water on an electronic balance, record the reading m1 of the electronic balance at this time, fix the lithium-ion battery in mid-air with the clamp of the iron stand, and slowly immerse it in the beaker filled with deionized water until the lithium-ion battery is completely immersed in the deionized water, record the reading m2 of the electronic balance at this time, according to the formula mg = ρ H2O VP, the battery volume V=(m2-m1)×g / (ρ H2O ×P). H2O is the density of deionized water, g is the gravity coefficient, P is one standard atmospheric pressure, and V is the volume of the lithium-ion battery;
[0124] High temperature storage method: The lithium ion batteries in the examples and comparative examples were charged to 3.65 V at a constant current of 1 C at 25°C, and charged to 0.05 C at a constant voltage at 3.65 V, and then placed in a 55°C oven for 180 days.
[0125] The above-mentioned volume test method is used to calculate the battery volume V1 of the lithium-ion battery before high-temperature storage, and then the volume V2 of the lithium-ion battery after high-temperature storage (high-temperature storage test such as the storage method in the above-mentioned high-temperature storage capacity retention rate) is calculated. The gas production of the battery after high-temperature storage = V2-V1.
[0126] Table 1 Performance comparison of lithium ion batteries of the embodiment and the comparative example
[0127] test High temperature cycles High temperature storage capacity retention rate / % Storage gas production / ml Example 1 5723 92.61% 1.7 Example 2 5535 92.82% 1.5 Example 3 7642 91.50% 2.8 Example 4 5216 91.80% 2.5 Example 5 5417 92.12% 2.2 Example 6 5547 92.33% 2.0 Example 7 5248 93.20% 1.1 Example 8 5125 92.90% 1.4 Example 9 6196 92.33% 2.0 Comparative Example 1 4257 89.35% 5.0 Comparative Example 2 4682 87.21% 7.1
[0128] It can be seen from the above table that the lithium ion batteries prepared in Examples 1-9 of the present application produce less gas during use, and the lithium ion batteries prepared in Comparative Example 1 or 2 produce more gas during use than the lithium ion batteries prepared in Examples 1-9; no imidazole carboxylate is added to the electrolyte in Comparative Example 1, the gas production of the battery is large, and the oxidizing property of the electrolyte is strong, resulting in reduced battery performance; no molecular sieve is added to the positive electrode material in Comparative Example 2, the gas production of the battery is greater, and the high-temperature storage capacity retention rate is lower.
[0129] The high temperature cycle times of the lithium ion batteries prepared in Examples 1-9 are relatively high, and the high temperature storage capacity retention rate can reach 92.90%. The high temperature cycle times and high temperature storage capacity retention rate of the lithium ion batteries prepared in Comparative Examples 1 or 2 are both relatively low.
[0130] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode coating disposed on the positive electrode current collector; characterized in that: The positive electrode coating comprises a positive electrode active material, a lithium supplement and a molecular sieve; The electrolyte includes a negative electrode film-forming additive, and the negative electrode film-forming additive includes an imidazole carboxylate additive containing an unsaturated bond.
2. The battery according to claim 1, characterized in that The molecular sieve includes any one of Cu-Y molecular sieve, Ce-Y molecular sieve, La-Beta molecular sieve, Zn-ZSM molecular sieve, Rh-ZSM molecular sieve, Ru-Y molecular sieve, Pt-Y molecular sieve and Ce-X molecular sieve, or a combination of at least two thereof.
3. The battery according to claim 1, characterized in that In terms of mass percentage, in the positive electrode coating, the content of the lithium supplement agent is 0.5%-3%; the content of the molecular sieve is 0.5%-5%; And / or, in the electrolyte, the content of the imidazole carboxylate additive containing an unsaturated bond is 0.3%-3% by mass percentage.
4. The battery according to claim 3, characterized in that In terms of mass percentage, in the positive electrode coating, the content of the lithium supplement agent is 1%-2%, and the content of the molecular sieve is 1%-3%; And / or, in terms of mass percentage, in the electrolyte, the content of the imidazole carboxylate additive containing an unsaturated bond is 0.3%-1.0%.
5. The battery according to claim 1, 3 or 4, characterized in that: The unsaturated bond-containing imidazole carboxylate additive includes any one of 2-propyn-1-yl-imidazole-1-carboxylate, 1H-imidazole-1-carboxylic acid allyl ester and 1H-imidazole-1-carboxylic acid-3-butene ester or a combination of at least two thereof.
6. The battery according to any one of claims 1 to 5, characterized in that: The electrolyte also includes a fluorinated solvent and a fluorinated lithium salt; The fluorinated solvent includes any one or a combination of at least two of fluorinated cyclic carbonates, fluorinated linear carbonates, fluorinated linear carboxylates or fluorinated ethers; The fluorinated lithium salt includes any one of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate, lithium difluorobis(oxalato)phosphate, lithium difluorooxalatoborate, lithium hexafluoroarsenate and lithium bis(trifluoromethanesulfonyl)imide, or a combination of at least two thereof.
7. The battery according to any one of claims 1 to 5, characterized in that: The electrolyte further comprises cyclic carbonate and / or linear carbonate; And / or, the electrolyte further comprises a positive electrode film-forming additive, and the positive electrode film-forming additive comprises tris(trimethylsilyl)phosphate and / or tris(trimethylsilyl)borate.
8. The battery according to any one of claims 1 to 5, characterized in that: The lithium supplement comprises at least one of lithium ferrite and lithium nickelate; And / or, the negative electrode film-forming additive further includes any one or a combination of at least two of vinyl sulfate, methylene methanedisulfonate, 1,3-propane sultone and vinylene carbonate.
9. The battery according to any one of claims 1 to 5, characterized in that: The positive electrode active material includes any one of lithium iron phosphate, lithium manganese iron phosphate and lithium nickel cobalt manganese oxide, or a combination of at least two thereof.
10. An electrical device, characterized in that: A battery comprising any one of claims 1 to 9.
Citation Information
Cited By
Composite lithium supplement agent, positive lithium supplement pole piece, lithium ion battery and preparation method of lithium ion battery
CN121149245A
Battery monomer and preparation method thereof, energy storage device and electric equipment
CN121460886A
Composite solid electrolyte layer and preparation method and application thereof
CN122800717A
Lithium-ion battery, battery assembly and electrical device
WO2026194784A1