Preparation method of atomic-scale PtFe bimetallic supported catalyst and application of atomic-scale PtFe bimetallic supported catalyst in selective hydrogenation of halogenated nitrobenzene
The atomic-level PtFe bimetallic catalyst prepared by strong electrostatic adsorption method uses hydrogen overflow effect and the adsorption effect of FeOx species to solve the problems of complex catalyst preparation and low selectivity in the prior art, and achieves efficient preparation of halogenated aniline , the conversion rate and selectivity reached more than 99%, and there were no obvious dehalogenated by-products.
Patent Information
- Application Number
- CN202410932894.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-12
AI Technical Summary
In the prior art, the C-X bond is prone to hydrogenation during catalytic halogenated nitrobenzene, resulting in low selectivity of halogenated aniline, and obvious dehalogenation reaction of precious metal catalysts, and the existing ALD method is complex and cost-effective. High, limiting industrial production.
Atomic-level PtFe bimetallic supported catalyst was prepared by strong electrostatic adsorption method, and the hydrogen overflow effect between Pt and reducing oxides and the adsorption of -NO2 groups by FeOx species was achieved. Efficient preparation, easy to operate and easy to recycle.
The efficient preparation of halogenated aniline is achieved, with conversion and selectivity up to more than 99%, and there is no obvious dehalogenated by-product generation for a long time, which significantly improves the activity and selectivity of the catalyst.
Smart Images

Figure CN118988341A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal catalysts, and in particular to a method for preparing an atomic-level PtFe bimetallic supported catalyst and application of the catalyst in the selective hydrogenation of halogenated nitrobenzene. Background Art
[0002] Substituted aromatic amines are an important class of chemical intermediates and are important raw materials for the synthesis of various fine chemicals and drugs. For example, p-chloroaniline is widely used in dyes, rubbers, medicines, pesticides and other fine chemicals. At present, the industry mainly uses the process of reducing substituted nitrobenzene to prepare substituted aromatic amines, including chemical reduction (Fe powder, alkali sulfide and hydrogen sulfide reduction) and catalytic hydrogenation reduction. Among them, the multiphase catalytic hydrogenation reduction method with hydrogen as the reducing agent has the advantages of less "three wastes", low cost, high product purity and easy separation and regeneration of catalysts, and has become the main means of preparing substituted aromatic amines in industry. However, when catalyzing the hydrogenation of halogenated nitrobenzene, the CX bond is very easy to undergo hydrogenolysis reaction, resulting in low selectivity of the target product halogenated aniline, especially when using precious metals such as Pt and Pd as catalysts, the dehalogenation reaction is more obvious. Adding a dechlorination inhibitor is a common strategy to inhibit the cleavage of a CX bond, but it will introduce additional impurities. Therefore, researchers often optimize the type and structure of the catalyst to achieve its efficient and selective hydrogenation activity, thereby avoiding the formation of dehalogenation byproducts and the introduction of impurities.
[0003] Wang et al. decoupled the geometric effect and electronic effect of the Pt center on the CX bond breaking activity by regulating the geometric structure and electronic structure of the supported Pt-based catalyst (Chem., 2020, 6, 752-765; Nat. Commun., 2022, 13, 3561). Among them, the positively valenced Pt single atoms with quasi-planar positions and the Pt sites on the surface of larger Pt particles have a higher coordination number, which causes the d orbital deformation of the Pt site to be serious, and it is impossible to effectively bond with the electrons on the non-bonding orbital of Cl in the C-Cl bond, thus showing excellent selectivity for chloroaniline. CN116651442A reports a method for preparing surface-confined atomically dispersed Pt@SiO using atomic layer deposition (ALD) technology. 2 -N catalyst, a 99% yield of p-chloroaniline can be obtained at a reaction temperature of 80 °C. However, this ALD method has the disadvantages of slow deposition rate, limited and expensive precursors, complex deposition mechanism and high equipment cost, which seriously restricts its industrial production. Therefore, it is particularly important to develop a universal and efficient method to prepare atomically dispersed Pt-based catalysts on a large scale to improve the selectivity of halonitrobenzene hydrogenation to halogenated aromatic amines. Summary of the invention
[0004] In view of this, the present invention provides a method for preparing an atomic-level PtFe bimetallic supported catalyst and its application in the selective hydrogenation of halogenated nitrobenzene, and prepares an atomic-level PtFe bimetallic supported catalyst having the advantages of low Pt loading, high atomic utilization, high activity, high selectivity and easy recycling by a strong electrostatic adsorption method, and utilizes the hydrogen overflow effect between Pt and the defect-rich reducible oxide carrier and FeO x Species-NO 2 The adsorption effect of the group realizes the efficient preparation of halogenated aniline under mild conditions, effectively solving the problems of complex catalyst preparation process, low activity and selectivity in the existing technology.
[0005] To achieve the above purpose, the technical solution of the present invention is as follows: In the first step, the reducible metal oxide support prepared by the hydrothermal method is heated to 2 or H 2 Pretreatment in a reducing atmosphere such as a mixed gas of Ar / O2 gives a defect oxide MO with surface rich oxygen vacancies and coordinated unsaturated metal cations. x ; In the second step, the MO obtained in the first step x The carrier is dispersed in water, and then the pH regulator is added dropwise to adjust the MO x The isoelectric point of the surface is obtained by adding the precursor solution containing Pt and Fe after dispersion and stirring at room temperature for 0.5-6 h. After centrifugation, overnight drying, calcination at 250-500 °C and reduction at 100-300 °C, atomically dispersed PtFe / MO can be obtained. x Bimetallic catalysts.
[0006] In the third step, the prepared PtFe bimetallic supported catalyst was used in the selective hydrogenation reaction of halonitrobenzene. In a high-pressure reactor, p-chloronitrobenzene was used as the raw material at a reaction temperature of 40-60 °C and a pressure of 1 MPa H 2 The selective hydrogenation performance evaluation experiment was carried out under pressure.
[0007] Preferably, the reducible oxide carrier in step 1 is CeO 2 , WO 3 , Nb 2 O 5 、TiO 2 、ZrO 2 and MoO 3 One or more of the following.
[0008] Preferably, in step 1, the carrier pretreatment temperature is 200-400° C., and the calcination time is 1-2 h.
[0009] Preferably, the pH regulator in step 2 is Na 2 CO 3 , K 2 CO 3 , Li 2 CO 3 、NaHCO 3 , KHCO 3 NH 3 ∙H 2 O、(NH 4 ) 2 CO 3 NH 4 HCO 3 , 3-aminopropyltrimethoxysilane and ethylenediamine solution, wherein the concentration of the solution is 0.01-0.2 mol / L.
[0010] The pH regulator in step 2 is Na2CO3 with a concentration of 0.01-0.2 mol / L. 2 CO 3 , K 2 CO 3 , Li 2 CO 3 、NaHCO 3 , KHCO 3 NH 3 ∙H 2 O、(NH 4 ) 2 CO 3 NH 4 HCO 3 , 3-aminopropyltrimethoxysilane (APTMS) and ethylenediamine solution. For negatively charged metal anion precursors, the pH value is adjusted to be lower than MO x The zero charge point of the cation makes its surface rich in positive charge, and for positively charged metal cation precursors, the pH value is adjusted to be higher than MO x The zero charge point makes its surface negatively charged. x The surface is enriched with charged ions with opposite charges, which can be strongly adsorbed on MO by electrostatic adsorption. x Highly dispersed PtFe / MO is formed on the surface x Supported Catalyst.
[0011] Preferably, the Pt precursor in step 2 is (NH 4 ) 2 PtCl 6 , K 2 PtCl 6 、Na 2 PtCl 6 , H2 PtCl 6 、Pt(NH 3 ) 4 (NO 3 ) 2 、Pt(acac) 2 , K 2 Pt(NO 2 ) 4 and Pt(NH 3 ) 4 Cl 2 One or more of the following.
[0012] The Fe precursor is Fe(NO 3 ) 3 、FeCl 3 、Fe(acac) 3 、FeCl 2 、FeSO 4 and Fe 2 (SO 4 ) 3 One or more of the following. The concentrations of the Pt and Fe precursor solutions are 0.5-5 and 3-12 mmol / L, respectively, and the Fe / Pt molar ratio is 2-6.
[0013] Preferably, in the PtFe bimetallic supported catalyst in step 2, the Pt loading amount is 0.02-0.5 wt%, and the Fe loading amount is 0.05-0.5 wt%.
[0014] Preferably, in step 3, the mass ratio of p-chloronitrobenzene to Pt is 100-435%.
[0015] In summary, compared with the prior art, the present invention has the following advantages: (1) The present invention relates to an atomic-level PtFe bimetallic supported catalyst, which is prepared by a strong electrostatic adsorption method. The method is simple to operate and does not require complex or expensive instruments and equipment; (2) The atomic-level PtFe bimetallic supported catalyst can be synthesized through the hydrogen overflow effect between Pt and the reducible metal oxide, the defect sites on the surface of the reducible oxide and the FeO x Oxygen-containing groups -NO 2 The adsorption effect of the catalyst can improve the hydrogenation activity of halonitrobenzene and the selectivity of halogenated aniline under mild conditions. The conversion rate and selectivity of the reaction can be as high as 99% or more, and no obvious dehalogenation byproducts are generated over a long period of time. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 10.2Pt0.2Fe / WO in Example 1 of the present invention x Spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscopy (AC-HAADF-STEM) image of the catalyst.
[0017] Figure 2 It is 0.2Pt0.2Fe / WO in Example 4 of the present invention. x High magnification transmission electron microscopy (HRTEM) image of the -IM catalyst.
[0018] Figure 3 1 is the p-chloronitrobenzene hydrogenation kinetic curve of Application Examples 1, 12 and 13 of the present invention.
[0019] Figure 4 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0020] In order to more clearly explain the purpose, technical solution and corresponding advantages of the present invention, the present invention will provide a series of catalyst preparation examples and application examples using p-chloronitrobenzene as a probe molecule, and explain in detail the specific operation process and actual application effect of the present invention, so as to verify the effectiveness and practicality of the present invention. In this embodiment, the preparation method of atomic-grade PtFe bimetallic supported catalyst consists of the following steps: (1) Disperse ammonium metatungstate and citric acid in an aqueous solution and place in a hydrothermal kettle at 180 °C for 12 h. After cooling to room temperature, wash and dry to obtain a light blue WO 3 . Will WO 3 In H 2 The surface was enriched with oxygen vacancies and W by pretreatment at 400 °C for 1 h in an atmosphere. δ+ (0<δ<6) dark blue powder WO x ; (2) The pre-treated WO x Disperse in water, then add 30 mL of 0.1 mol / L ammonium bicarbonate solution dropwise, and after stirring evenly, add H 2 PtCl 6 and Fe(NO 3 ) 3 The solution was stirred at room temperature for 1 h, centrifuged and dried, and then calcined in a muffle furnace at 300 °C for 2 h, and then heated in H 2 Atomic-dispersed 0.2Pt0.2Fe / WO with Pt and Fe loadings of 0.2 wt% and 0.2 wt%, respectively, was obtained by reduction at 200 °C in an atmosphere for 2 h. x Bimetallic catalysts (see Figure 1 ), where Fe is in the form of FeO x Form exists.
[0021] Example 2 Example 2 was prepared by the impregnation method. No pH regulator was added in step (2). x Add H 2 PtCl 6 and Fe(NO 3 ) 3 The solution was then stirred and evaporated to dryness at 80°C, and the remaining steps were the same as in Example 1. HRTEM images show that the 0.2Pt0.2Fe / WO prepared by this method x -IM catalysts Pt and Fe are mainly present in the form of nanoparticles and the particle sizes are not uniform (e.g. Figure 2 ).
[0022] Examples 3 and 4 The preparation methods of Examples 3 and 4 are the same as those of Example 1, except that the ammonium bicarbonate solution in step (2) is replaced with 3-aminopropyltrimethoxysilane (APTMS) and ethylenediamine solution.
[0023] Embodiments 5 to 9 The preparation methods of Examples 5-9 are the same as those of Example 1, except that: The loading amount of Pt in step (2) is 0.2 wt%, and 0.2Pt / WO is obtained. x catalyst; In step (2), the loading amount of Pt is 0.2 wt%, and the loading amount of Fe is 0.1 wt%, and 0.2Pt0.1Fe / WO is obtained. x catalyst; In step (2), the loading amount of Pt is 0.2 wt%, and the loading amount of Fe is 0.3 wt%, and 0.2Pt0.3Fe / WO is obtained. x catalyst; In step (2), the loading amount of Pt is 0.1 wt%, and the loading amount of Fe is 0.2 wt%, and 0.1Pt0.2Fe / WO is obtained. x catalyst; In the step (2), the loading amount of Pt is 0.3 wt%, and the loading amount of Fe is 0.2 wt%, and 0.3Pt0.2Fe / WO is obtained. x catalyst.
[0024] Embodiments 10 to 12 The preparation methods of Examples 10 to 12 are the same as those of Example 1, except that the reducible oxides in step (1) are CeO 2 、ZrO 2 and TiO 2, and obtain 0.2Pt0.2Fe / CeO x 、0.2Pt0.2Fe / ZrO x and 0.2Pt0.2Fe / TiO x Catalyst. Among them, CeO 2 The ZrO was prepared by mixing cerium nitrate with NaOH solution and heating to 100 °C for 24 h. 2 It was prepared by mixing zirconium oxynitrate and urea in methanol solution and then hydrothermal treatment at 140 °C for 12 h. 2 TiCl 4 It was obtained by dissolving in ethylene glycol solution containing a small amount of water and then hydroheating at 150 °C for 4 h.
[0025] Comparative Examples 1 and 2 The preparation methods of Comparative Examples 1 and 2 are the same as those of Example 1, except that the reducible metal oxide in step (1) is replaced by non-reducible carriers of commercial activated carbon and SiO 2 , and obtain 0.2Pt0.2Fe / C and 0.2Pt0.2Fe / SiO 2 catalyst.
[0026] Application Examples 1~14 The defect-rich reducible metal oxide-supported PtFe-based catalysts prepared in Examples 1 to 12 and the non-reducing carrier-supported PtFe catalysts prepared in Comparative Examples 1 to 2 were respectively evaluated for the selective hydrogenation performance of p-chloronitrobenzene to obtain Application Examples 1 to 14, and the specific reaction conditions were: The catalytic hydrogenation reaction of p-chloronitrobenzene was carried out in a 50 mL stainless steel high-pressure batch reactor. With anhydrous ethanol as solvent, the mass ratio of p-chloronitrobenzene (p-CNB) to Pt in the PtFe bimetallic supported catalyst was 435, and the selective hydrogenation performance evaluation experiment of p-chloronitrobenzene was carried out at a hydrogen pressure of 1 MPa and a reaction temperature of 40 °C. After the reaction, the reaction mixture was centrifuged, and the supernatant was taken for gas chromatography quantitative analysis, and the product composition was confirmed by gas chromatography-mass spectrometry.
[0027] Application Examples 15 and 16 The atomic-grade 0.2Pt0.2Fe / WO prepared in Example 1 x The catalyst was subjected to selective hydrogenation experiments of p-CNB at p-CNB / Pt mass ratios of 238 and 100, respectively, to obtain corresponding application examples 15 and 16, and the remaining conditions were the same as those of application examples 1 to 14. The kinetic data obtained from application examples 1, 15 and 16 were plotted as Figure 3It can be seen that with the increase of p-CNB conversion, the yield of p-chloroaniline gradually increases. When p-CNB is fully converted, the selectivity of p-chloroaniline (p-CAN) can reach more than 99%. More importantly, at a low p-CNB / Pt mass ratio, that is, at an excess of 0.2Pt0.2Fe / WO x Under the catalyst, the selectivity of p-CAN can still be maintained at more than 99%, and after the reaction time is further extended to 23 h when p-chloronitrobenzene is completely converted, the selectivity of p-CAN can still reach more than 95.6%, indicating that the catalyst significantly inhibits the breakage of the C-Cl bond.
[0028] Table 1. Catalytic performance of a series of PtFe bimetallic supported catalysts in hydrogenation of p-chloronitrobenzene.
[0029]
[0030] The above experiments show that the 0.2Pt0.2Fe / WO prepared by the impregnation method has a non-uniform metal particle size. x Compared with the 0.2Pt0.2Fe / WO-IM catalyst prepared by strong electrostatic adsorption method, x Pt and Fe in the catalyst are highly dispersed and no obvious particles appear. x The introduction of species can increase the -NO in p-chloronitrobenzene 2 The adsorption of functional groups further improved the hydrogenation activity of p-chloronitrobenzene and the selectivity of p-chloroaniline, and successfully inhibited the occurrence of dechlorination side reactions. 2 In contrast, hydrogen is activated on Pt and overflows to the reducible oxide WO x 、CeO x 、ZrO x 、TiO 2 The surface can significantly improve the hydrogenation activity of chloronitrobenzene. In addition, the surface of the reducible oxide after hydrogen reduction is rich in oxygen vacancies and coordinated unsaturated metal cations, which can promote the hydrogenation of oxygen-containing groups -NO 2 The adsorption on the catalyst surface is beneficial to the 2 Therefore, the PtFe bimetallic catalyst prepared by strong electrostatic adsorption has both atomically dispersed precious metal Pt, which improves the atomic utilization of Pt, and also inhibits the breakage of C-Cl bonds. x The species, active component Pt and reducible oxide defect sites synergistically catalyze the selective hydrogenation of p-chloronitrobenzene, greatly improving the yield of p-chloroaniline.
[0031] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An atomic-level PtFe bimetallic supported catalyst, It is characterized in that Pt and Fe metals are anchored in an atomically dispersed form on the surface defect-rich reducible oxide MO via strong electrostatic adsorption. x On the PtFe / MO x Bimetallic catalysts.
2. The method for preparing the atomic-grade PtFe bimetallic supported catalyst according to claim 1, It is characterized in that The following steps are involved: (1) Carrier pre-reduction treatment: The reducible oxide carrier is heated in H 2 or H 2 The defect oxide MO with rich surface oxygen vacancies and coordinated unsaturated metal cations was obtained by calcination in a reducing atmosphere of a mixed gas of Ar. x ; (2) Preparation of PtFe / MO by strong electrostatic adsorption method x Catalyst: MO obtained in step (1) x Disperse in water, then add pH adjuster drop by drop to adjust MO x The isoelectric point of the surface is obtained by adding a precursor solution containing Pt and Fe after dispersion and stirring at room temperature. After centrifugation, drying, calcination and reduction, atomically dispersed PtFe / MO x Bimetallic catalysts.
3. The method for preparing the atomic-grade PtFe bimetallic supported catalyst according to claim 1, It is characterized in that The reducible oxide support is selected from CeO 2 , WO 3 , Nb 2 O 5 、TiO 2 、ZrO 2 and MoO 3 One or more of the reduced defect oxide MO x CeO x , WO x 、NbO x 、TiO x 、ZrO x and MoO x One or more of .
4. The method for preparing the atomic-grade PtFe bimetallic supported catalyst according to claim 2, It is characterized in that In the step (1), the carrier pre-reduction calcination temperature is 150-500°C, and the calcination time is 0.5-6 h, preferably 200-400°C, 1-2 h.
5. The method for preparing the atomic-grade PtFe bimetallic supported catalyst according to claim 2, It is characterized in that The pH adjusting agent in step (2) involves Na 2 CO 3 , K 2 CO 3 , Li 2 CO 3 、NaHCO 3 , KHCO 3 NH 3 ∙H 2 O、(NH 4 ) 2 CO 3 NH 4 HCO 3 , 3-aminopropyltrimethoxysilane and ethylenediamine solution, wherein the concentration of the solution is 0.01~0.2mol / L.
6. The method for preparing the atomic-grade PtFe bimetallic supported catalyst according to claim 2, It is characterized in that The Pt precursor in step (2) is (NH 4 ) 2 PtCl 6 , K 2 PtCl 6 、Na 2 PtCl 6 , H 2 PtCl 6 、Pt(NH 3 ) 4 (NO 3 ) 2 、Pt(acac) 2 , K 2 Pt(NO 2 ) 4 and Pt(NH 3 ) 4 Cl 2 One or more of the following: the Fe precursor is Fe(NO 3 ) 3 、FeCl 3 、Fe(acac) 3 、FeCl 2 、FeSO 4 and Fe 2 (SO 4 ) 3 One or more of .
7. The method for preparing the atomic-grade PtFe bimetallic supported catalyst according to claim 2, It is characterized in that In the step (2), the concentration of the Pt precursor solution is 0.5-5 mmol / L, the concentration of the Fe precursor solution is 3-12 mmol / L, and the molar ratio of Fe to Pt is 2-6.
8. The method for preparing the atomic-grade PtFe bimetallic supported catalyst according to claim 2, It is characterized in that In the step (2), the calcination temperature is 250-500°C, and the calcination time is 1-4 h; the reduction temperature is 100-300°C, and the reduction time is 0.5-3.5 h; the Pt loading is 0.02-0.5 wt%, and the Fe loading is 0.05-0.5 wt%.
9. Use of the atomic-grade PtFe bimetallic supported catalyst prepared according to the method according to any one of claims 2 to 8 in the selective hydrogenation of halonitrobenzene to halogenated aniline.
10. The use according to claim 9, It is characterized in that The prepared catalyst was placed in a high-pressure reactor with a mass ratio of halogenated nitrobenzene to Pt of 100-435%. The reaction temperature was 40-60 °C and the pressure was 1-2 MPa H 2 Selective hydrogenation of halogenated nitrobenzenes to halogenated anilines under pressure.
Citation Information
Patent Citations
Pt-Fe / C catalyst as well as preparation method and application thereof
CN109225258A
Fine regulation supported alloy catalyst and preparation method and application thereof
CN112495393A
Sub-nano Pt selective hydrogenation catalyst, preparation method and application thereof
CN114471540A
Atomic-scale catalyst for efficiently catalyzing hydrogen and oxygen to directly synthesize hydrogen peroxide and preparation method of atomic-scale catalyst
CN115212873A
Method for rapid catalytic reduction of 4-nitrophenol by Pt-Fe bimetallic nanomaterial
CN116041192A