Method for pre-discarding tailings and floating silver ore
By performing pre-tailing treatment during the silver ore ore dressing process, using heavy medium selection and multiple sorting techniques, the problem of uneven insertion of valuable metals in silver ore is solved, reducing the selection cost and improving the silver ore recovery rate and grade.
Patent Information
- Application Number
- CN202411367624.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-22
AI Technical Summary
The uneven insertion of valuable metals in silver ore leads to an increase in ore dressing costs, especially during the flotation process, which increases the selection cost of grinding and flotation.
Pre-tailing treatment is carried out before grinding-flotation, and ore of different particle sizes is obtained by sieving after crushing, and heavy medium selection is carried out to throw out low-grade waste ore, improve ore grade, and reduce grinding and flotation treatment. The amount is selected multiple times with collectors, activators and inhibitors to improve the recovery rate of silver ore.
The selection cost of grinding and flotation is reduced, the recovery rate and economic benefits of silver ore are improved, the subsequent processing volume is reduced, and the grade and quality of silver ore are improved.
Smart Images

Figure CN118988552A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of mineral processing, and in particular to a method for pre-tailings discarding-floating silver ore. Background Art
[0002] Silver is relatively rare in the earth's crust, but its unique physical and chemical properties make it widely used in many fields. The main silver minerals include argentite (Ag2S), silver copper sulfide (AgCuS), silver antimony sulfide (3Ag2S·Sb2S3), silver sulfide (3Ag2S·As2S3), silver hornite (AgCl), silver chlorobromide (AgCl·AgBr) and tellurium gold silver. These minerals often coexist with sulfide minerals of non-ferrous heavy metals such as copper, lead, and zinc, and have comprehensive recovery value.
[0003] The mining and processing of silver ore involves multiple links, including ore mining, crushing, grinding, beneficiation and smelting. Among them, flotation is a very important separation link in the beneficiation process of silver ore. The particle size of the selected minerals in the flotation operation is relatively fine, which requires all minerals to be ground to reach the required particle size range.
[0004] However, due to the uneven distribution of minerals, especially for silver mines, some of the ore content is very low, and the grade of this part of the ore is even lower than the grade of the tailings product of the flotation operation. It increases the separation cost by passing through the grinding-flotation operation. Therefore, it is urgent to propose a method for flotation of silver ore by pre-discharging tailings. Summary of the invention
[0005] In order to solve the above problems, the present application provides a method for pre-discarding tailings and flotation of silver ore. The method performs heavy medium separation treatment before grinding and flotation to discard a portion of low-grade waste ore, thereby increasing the grade of valuable metal elements in the ore entering the grinding and flotation stage, greatly reducing the amount of grinding and flotation, which is beneficial to reducing the separation cost of grinding and flotation and improving the recovery rate of silver ore.
[0006] The present application provides a method for pre-tailing-floating silver ore, the method comprising: S1. After the silver ore is crushed, it is screened to obtain a first coarse ore with a particle size of not less than 0.5 mm and a second coarse ore with a particle size of less than 0.5 mm; S2, performing heavy medium separation on the first coarse ore to obtain heavy medium concentrate and heavy medium tailings; S3, crushing the heavy medium concentrate and mixing it with the second coarse ore, grinding the obtained mixed system, adding a collector and / or an activator, and performing rough separation to obtain a silver coarse concentrate and coarse tailings; S4, adding an inhibitor to the silver rough concentrate to perform concentration to obtain a first silver concentrate; S5. Adding a collector, an activator and / or a frother to the coarse tailings for scavenging to obtain a second silver concentrate.
[0007] Further, the collector includes ethyl xanthate, ethyl thiocyanate and / or butylamine black medicine; The activator is copper sulfate; The inhibitor is water glass, sodium sulfite or sodium carbonate; The foaming agent is pine oil.
[0008] Further, in step S3, the rough selection includes: Add a collector to the ground heavy medium concentrate, react for 1 min to 5 min, and then perform a first roughing for 2 min to 10 min; An activator is added to the ore obtained from the first roughing, and after an activation reaction for 3 min to 10 min, an appropriate amount of a collector is added, and after a reaction for 1 min to 5 min, a second roughing for 2 min to 10 min is performed to obtain a silver rough concentrate and a rough tailing.
[0009] Furthermore, in step S4, the selection includes: Add an inhibitor to the silver rough concentrate, react for 1 min to 10 min, and then perform a first concentration for 2 min to 10 min; Adding an inhibitor to the ore obtained from the first concentration, reacting for 1 min to 10 min, and then performing a second concentration for 2 min to 10 min; The ore obtained from the second concentration is subjected to a third concentration for 2 min to 10 min, and then subjected to a fourth concentration for 2 min to 10 min to obtain a first silver concentrate.
[0010] Further, in step S5, the scanning includes: Add an activator to the coarse tailings, and after the activation reaction for 3 min to 10 min, add an appropriate amount of collector and frother, react for 1 min to 5 min, and then perform a first sweep for 1 min to 10 min; Adding an appropriate amount of collector to the ore obtained from the first scavenging, reacting for 1 min to 5 min, and then performing a second scavenging for 1 min to 10 min; An appropriate amount of collector is added to the ore obtained from the second scavenging, and after reacting for 1 min to 5 min, a third scavenging is performed for 1 min to 10 min to obtain a second silver concentrate.
[0011] Furthermore, in step S2, the mass percentage of the heavy medium concentrate and the heavy medium tailings is (60-85)%:(15-40)%.
[0012] Furthermore, in step S2, when the first coarse ore is subjected to heavy medium separation, the heavy medium is magnetic iron or ferrosilicon ore.
[0013] Furthermore, in step S3, after the heavy medium concentrate is crushed, the particle size of the obtained particles is less than 2 mm.
[0014] Furthermore, in step S3, after the obtained mixed system is ground, particles with a mesh size of 200-350 mesh account for 70%-90% of the total mass of the particles.
[0015] Further, in step S1, the particle size of the first coarse ore is less than 10 mm.
[0016] In summary, the present application includes at least one of the following beneficial technical effects: The present application provides a method for pre-discarding tailings and flotation of silver ore. Before flotation, the silver ore is crushed and then screened to obtain a first coarse ore with a particle size of not less than 0.5 mm and a second coarse ore with a particle size of less than 0.5 mm. Then, the coarse ore with a particle size of not less than 0.5 mm is subjected to heavy medium separation, and a portion of low-grade ore is discarded to obtain a heavy medium concentrate. The heavy medium concentrate is then mixed with the second coarse ore with a particle size of less than 0.5 mm as a sample for subsequent grinding and other treatments. After the silver ore is separated, the grade of valuable metals in the ore is increased, which greatly reduces the processing volume of grinding and subsequent flotation processes, and is conducive to reducing separation costs and improving economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0018] Figure 1 A flow chart of a method for pre-tailings discarding and flotation of silver ore proposed in an embodiment of the present application is shown; Figure 2 A flow chart of another method for pre-tailing-floating silver ore proposed in Example 1 of the present application is shown; Figure 3 A flow chart of a method for pre-tailing discarding and flotation of silver ore proposed in Comparative Example 1 of the present application is shown. DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0020] In the drawings, the size of the constituent elements, the thickness of the layer or the area may be exaggerated for the sake of clarity. Therefore, any implementation of the present disclosure is not necessarily limited to the size shown in the drawings, and the shapes and sizes of the components in the drawings do not reflect the true proportions. In addition, the drawings schematically show ideal examples, and any implementation of the present disclosure is not limited to the shapes or values shown in the drawings.
[0021] In the relevant technology, the silver ore dressing process is a complex and delicate process, the main purpose of which is to extract high-purity silver from the ore. The flotation process is the most critical step in the silver ore dressing process. It uses the difference in hydrophilicity or lipophilicity of the mineral surface to separate the target mineral from impurities under specific conditions. By adding flotation agents (such as collectors, frothers, etc.), the physical and chemical properties of the slurry are adjusted, so that the silver mineral particles are combined with bubbles to form floatable minerals, which are finally separated by the flotation machine.
[0022] However, due to the uneven distribution of valuable metals in silver ore, the degree of dissociation of the ore is reduced, making it difficult to separate silver minerals from the ore. Some parts of the ore even have very low content, and the grade of this part of the ore is lower than the grade of the tailings product of the flotation operation, so it increases the separation cost by passing through the grinding-flotation operation.
[0023] Based on the above problems, the present application proposes a method for pre-discarding tailings and flotation of silver ore. The method crushes the silver ore and then screens it, sorts the 0.5 mm-10 mm ore through a cyclone, and discards low-grade waste rock, so that the grade of valuable metal elements in the ore entering the grinding-flotation stage is increased, the recovery quality of the silver ore is improved, and about 26% of the waste rock is discarded in advance, which reduces the cost of subsequent grinding and flotation and improves the economic benefits of the enterprise.
[0024] See also Figure 1 , Figure 1 A flow chart of a method for pre-tailings discarding and flotation of silver ore proposed in an embodiment of the present application is shown, which specifically includes: S1. After the silver ore is crushed, it is screened to obtain a first coarse ore with a particle size of not less than 0.5 mm and a second coarse ore with a particle size of less than 0.5 mm; S2, performing heavy medium separation on the first coarse ore to obtain heavy medium concentrate and heavy medium tailings; S3, crushing the heavy medium concentrate and mixing it with the second coarse ore, grinding the obtained mixed system, adding a collector and / or an activator, and performing rough separation to obtain a silver coarse concentrate and coarse tailings; S4, adding an inhibitor to the silver rough concentrate to perform concentration to obtain a first silver concentrate; S5. Adding a collector, an activator and / or a frother to the coarse tailings for scavenging to obtain a second silver concentrate.
[0025] In specific implementation, after the silver ore is crushed, the second coarse ore with a particle size of less than 0.5 mm is screened out, the first coarse ore with a particle size of not less than 0.5 mm is added to the cyclone for selection, and the low-grade waste rock is discarded. The obtained heavy medium concentrate and the first coarse ore with a particle size of less than 0.5 mm are mixed to obtain the ore with improved grade that can be used in the grinding-flotation stage. This step can discard at least 20% of the waste rock, greatly reducing the processing volume of the subsequent grinding-flotation stage, thereby reducing energy consumption and costs.
[0026] After the second coarse ore is mixed with the heavy medium concentrate, it is ground to make the particles finer and more uniform, and then a collector and / or activator is added for rough selection. Rough selection can quickly enrich the silver minerals to form a rough concentrate containing higher grade silver, which provides more favorable conditions for subsequent selection.
[0027] Adding inhibitors to the silver rough concentrate can inhibit the floatability of non-target minerals. In this way, during the concentration process, silver minerals can more easily combine with bubbles and float, while non-target minerals remain in the slurry, improving the selectivity of the concentration. After the concentration treatment, the silver minerals in the silver rough concentrate can be enriched, the impurity content can be reduced, the grade of the first silver concentrate can be improved, and higher quality silver ore raw materials can be provided for subsequent smelting and other processes.
[0028] A collector, an activator and / or a frother are added to the coarse tailings for scavenging to obtain a second silver concentrate. Since the coarse tailings also contain some silver ore, after scavenging, some of the silver ore remaining in the coarse tailings can be recovered to improve the comprehensive recovery rate of the silver ore.
[0029] In practice, heavy medium separation is a process of separating materials using a heavy medium with a specific gravity between the specific gravity of two ores. In this process, the material particles are affected by gravity and buoyancy in the medium, thereby achieving separation by density.
[0030] In some embodiments, in step S1 , the particle size of the first coarse ore is less than 10 mm.
[0031] If the particle size is too large, its sedimentation rate will increase significantly. The particle size of the ore is controlled between 5 mm and 10 mm, and the particles stay in the suspension for a long time, and can fully interact with the medium in the suspension, thereby achieving a better sorting effect. Ore particles of this size are not easy to form large agglomerates in the suspension, which can prevent the agglomerates from hindering the effective stratification between particles of different densities, thereby improving the sorting accuracy; if the particle size is smaller, the dynamic resistance it encounters when moving in the suspension is greater, and the ore particles specified in this application have a faster movement speed and a higher sorting efficiency.
[0032] In some embodiments, in step S2, when the first coarse ore is subjected to heavy medium separation, the heavy medium is magnetic iron or ferrosilicon ore.
[0033] Magnetic iron (such as magnetite) can be recovered by magnetic separators during the sorting process due to its magnetic properties, thereby reducing the loss of heavy media and production costs and improving the economic benefits of recovery; Ferrosilicon ore (such as ferrosilicon) has stable chemical properties and is not easy to react with other minerals during the screening process, thus ensuring the stability and reliability of the separation. These heavy medium particles have high density and good magnetic or physical stability, and can effectively separate silver ore from other minerals.
[0034] In some embodiments, preferably, the heavy medium is magnetic iron, and the density of magnetic iron powder is 4 g / cm 2 ~5 g / cm 2 Preferably, the density of the magnetic iron powder is 4.5 g / cm 2 .
[0035] In some embodiments, in the heavy medium separation step, the suspension used includes water, heavy medium particles, a regulator, etc. The specific components of the suspension are not specifically limited in the embodiments of the present application. The density of the suspension is 1.3 g / cm 2 ~3.0g / cm 2 .
[0036] In some embodiments, in step S2, the mass percentage of the heavy medium concentrate and the heavy medium tailings is (60-85)%:(15-40)%.
[0037] In specific implementation, 15% to 40% of low-grade waste ore can be discarded through heavy medium separation, and the discarding rate is relatively high, so that the obtained heavy medium concentrate is more in line with the grade requirements of grinding-flotation treatment, thereby improving the efficiency of grinding-flotation treatment and improving the quality of the recovered first silver concentrate and the second concentrate.
[0038] In some embodiments, in step S3, after the heavy medium concentrate is crushed, the particle size of the obtained particles is less than 2 mm.
[0039] In specific implementation, grinding the heavy medium concentrate to less than 2 mm can fully dissociate the silver ore to improve the recovery rate of the subsequent flotation process, and the silver minerals in the fine-grained ore are more easily captured by the flotation agent and attached to the bubbles, which also helps to improve the recovery rate.
[0040] In some embodiments, in step S3, after the obtained mixed system is ground, particles with a mesh size of 200-350 mesh account for 70%-90% of the total mass of the particles.
[0041] In specific implementation, the silver minerals in the silver mine have a relatively fine particle size, generally between 0.074 mm and 0.005 mm. Grinding the mixed system to 200-350 mesh is conducive to flotation to obtain silver concentrate with higher precision.
[0042] In some embodiments, the collector includes ethyl xanthate, ethyl thiocyanate and / or butylamine black drug; The activator is copper sulfate; The inhibitor is water glass, sodium sulfite or sodium carbonate; The foaming agent is pine oil, also known as 2# oil.
[0043] In specific implementation, preferably, the collector includes ethyl xanthate, ethyl thiocyanate and butylamine black drug.
[0044] The collector in the embodiment of the present application adopts a compound of ethyl xanthate, ethyl thiocyanate and butylamine black medicine. The three can produce a synergistic effect to enhance the capture effect of silver minerals, have high selectivity, and are particularly suitable for efficient recovery of high-grade silver ores, with significant economic benefits.
[0045] In some embodiments, in step S3, the rough selection includes: Add a collector to the ground heavy medium concentrate, react for 1 min to 5 min, and then perform a first roughing for 2 min to 10 min; An activator is added to the ore obtained from the first roughing, and after an activation reaction for 3 min to 10 min, an appropriate amount of a collector is added, and after a reaction for 1 min to 5 min, a second roughing for 2 min to 10 min is performed to obtain a silver rough concentrate and a rough tailing.
[0046] In specific implementation, the ground heavy medium concentrate undergoes two roughing processes, which can reduce the impurity content in the ore and improve the grade and quality of the ore obtained by roughing.
[0047] In specific implementation, preferably, a collector is added to the ground heavy medium concentrate, and after reacting for 2 min-4 min, a first roughing for 3 min-5 min is performed; Preferably, an activator is added to the ore obtained from the first roughing, and an appropriate amount of a collector is added after the activation reaction for 4 min-6 min. After the reaction for 2 min-4 min, a second roughing for 3 min-5 min is performed to obtain a silver rough concentrate and rough tailings.
[0048] In the embodiment of the present application, only the collector is added in the first roughing because the heavy medium concentrate after grinding contains a lot of galena and argillite with good floatability. If the activator is added, it will produce extra consumption, resulting in excessive activator usage. Therefore, in the first roughing, most of the galena and argillite are first collected, and then the activator is added in the second roughing to float the sphalerite in the ore for collection, which has higher selectivity, better roughing effect, and less reagent material, so as to reduce the flotation cost.
[0049] In the present application, the activator copper sulfate is first added in the second roughing, and the copper sulfate is ionized after dissolving, and the copper ions are adsorbed to the surface of the ore. Then, when the collector is added, the collector and the copper ions are first adsorbed, and then floated with the bubbles. Therefore, it is necessary to add the activator and the collector separately, and then flotation is carried out after the activator has fully acted, which is conducive to enhancing the flotation effect.
[0050] In step S4, the selection includes: Add an inhibitor to the silver rough concentrate, react for 1 min to 10 min, and then perform a first concentration for 2 min to 10 min; Adding an inhibitor to the ore obtained from the first concentration, reacting for 1 min to 10 min, and then performing a second concentration for 2 min to 10 min; The ore obtained from the second concentration is subjected to a third concentration for 2 min to 10 min, and then subjected to a fourth concentration for 2 min to 10 min to obtain a silver concentrate.
[0051] Preferably, an inhibitor is added to the silver rough concentrate, and after reacting for 3 min to 6 min, a first concentration is carried out for 3 min to 5 min.
[0052] Preferably, an inhibitor is added to the ore obtained from the first concentration, and after reacting for 3 min to 6 min, a second concentration is carried out for 3 min to 5 min.
[0053] Preferably, the ore obtained from the second concentration is subjected to a third concentration for 3 min to 5 min.
[0054] Preferably, a fourth concentration is performed for 3 min to 5 min to obtain the first silver concentrate.
[0055] In the specific implementation, a small amount of inhibitor water glass is added in the first two concentrations to disperse and inhibit non-target ores. After two concentrations, the content of miscellaneous ores is very small, so no inhibitor needs to be added in the third and fourth concentrations to avoid excessive inhibitors affecting subsequent precipitation, filtration and other treatments, and also to reduce the amount of flotation reagents used and reduce flotation costs.
[0056] In step S5, the scanning includes: Add an activator to the coarse tailings, and after the activation reaction for 3 min to 10 min, add an appropriate amount of collector and frother, react for 1 min to 5 min, and then perform a first sweep for 1 min to 10 min; Adding an appropriate amount of collector to the ore obtained from the first scavenging, reacting for 1 min to 5 min, and then performing a second scavenging for 1 min to 10 min; An appropriate amount of collector is added to the ore obtained from the second scavenging, and after reacting for 1 min to 5 min, a third scavenging is performed for 1 min to 10 min to obtain a second silver concentrate.
[0057] Preferably, an activator is added to the coarse tailings, and after the activation reaction for 4 min-6 min, an appropriate amount of collector and frother are added, and after the reaction for 2 min-4 min, a first sweep is performed for 2 min-5 min.
[0058] Preferably, a proper amount of collector is added to the ore obtained from the first scavenging, and after reacting for 2 min-4 min, a second scavenging is performed for 2 min-5 min.
[0059] Preferably, a proper amount of collector is added to the ore obtained from the second scavenging, and after reacting for 2 min-4 min, a third scavenging is performed for 2 min-5 min to obtain a second silver concentrate.
[0060] In specific implementation, some miscellaneous ores still remain in the coarse tailings. During the first scavenging, adding an appropriate amount of activator copper sulfate helps to promote the floating of copper ore and further enhance the flotation effect. After the first scavenging, the remaining miscellaneous ores have been screened out. Therefore, during the second and third scavenging, only the collector needs to be added to achieve efficient collection, reduce the amount of activator, and reduce the flotation cost.
[0061] In some embodiments, in steps S3, S4, and S5, during roughing, cleaning, and scavenging, the pH of the pulp under natural conditions is 7-9. No additional pH adjustment is required, and a good flotation effect can be achieved, reducing the types of additives used and further reducing the flotation cost.
[0062] Since the second silver concentrate still contains some impurity ores, the second silver concentrate is not directly used as silver concentrate. The obtained second silver concentrate is returned to step S3, the second silver concentrate is mixed with the ground mixed system, and participates in the next roughing and other treatments, and the silver ore therein is recovered again, thereby improving the comprehensive recovery rate of the silver ore.
[0063] In order to enable those skilled in the art to more clearly understand the present application, the method for pre-tailing discarding and flotation of silver ore described in the present application is now described in detail through the following examples.
[0064] Example 1 Reference Figure 2 The method for pre-tailing-floating silver ore shown is carried out as follows: Crushing and screening: Crushing the silver ore with an Ag content of 433.8 g / t to less than 10 mm, and then screening to separate the first coarse ore with a particle size of not less than 5 mm and the second coarse ore with a particle size of less than 5 mm; Heavy medium separation: Add heavy medium material-magnetic iron powder into the cyclone, and adjust the medium density to 4.5 g / cm by controlling the amount of heavy medium material added 2 , then add water to obtain a suspension density of 2.0 g / cm 2 , and then add the second coarse ore into the cyclone for heavy medium separation to obtain heavy medium concentrate and heavy medium tailings; Grinding: crush the heavy medium concentrate to less than 2 mm, mix it with the first coarse ore, and the resulting mixed system is the flotation sample. Grind the mixed system so that the particles of 325 mesh account for 85% of the total ore; Roughing: add 0-50 g / t of ethyl xanthate, 0-30 g / t of ethyl thiocyanate and 0-40 g / t of butylamine black medicine to the mixed system after grinding, react for 3 minutes, and then carry out the first roughing for 4 minutes; then add 0-300 g / t of copper sulfate, an activator, to the ore obtained from the first roughing, and after 5 minutes of activation reaction, add 0-50 g / t of ethyl xanthate, 0-30 g / t of ethyl thiocyanate and 0-40 g / t of butylamine black medicine, react for 3 minutes, and then carry out the second roughing for 4 minutes to obtain a silver rough concentrate and a rough tailing; Concentration: adding 0-200 g / t of water glass as an inhibitor to the silver rough concentrate, after acting for 5 minutes, carrying out the first concentration for 4 minutes, adding 0-100 g / t of water glass as an inhibitor to the ore obtained by the first concentration, after acting for 5 minutes, carrying out the second concentration for 4 minutes, carrying out the third concentration for 4 minutes on the ore obtained by the second concentration, and then carrying out the fourth concentration for 4 minutes to obtain the first silver concentrate; Sweeping: add activator copper sulfate 0-100 g / t to the coarse tailings, after 5 minutes of activation reaction, add collector ethyl xanthate 0-30 g / t, ethyl thiocyanate 0-10 g / t and butylamine black medicine 0-20 g / t, and foaming agent 2# oil 0-10 g / t, after 3 minutes of action, carry out the first sweeping for 3 minutes, add collector ethyl xanthate 0-20 g / t, ethyl thiocyanate 0-10 g / t and butylamine black medicine 0-10 g / t to the ore obtained by the first sweeping, after 3 minutes of action, carry out the second sweeping for 3 minutes; add collector ethyl xanthate 0-20 g / t, ethyl thiocyanate 0-10 g / t and butylamine black medicine 0-10 g / t to the ore obtained by the second sweeping, after 3 minutes of action, carry out the second sweeping for 3 minutes. The second silver concentrate (also called tailings) is obtained by the third scavenging of min. The second silver concentrate is added to the next roughing stage and mixed with the mixing system for subsequent treatment such as re-roughing.
[0065] In Example 1, the silver ore used has an Ag content of 433.8 g / t, and the main silver-containing mineral is argentite. The minerals are pre-classified (i.e., heavy medium separation treatment) to obtain a first coarse ore of 0.5 mm-10 mm and a second coarse ore less than 0.5 mm. The first coarse ore of 0.5 mm-10 mm is subjected to heavy medium separation, and low-grade waste rock is preferentially discarded. The results of the discard rate are shown in Table 1.
[0066] Table 1
[0067] Fine-grained products refer to ore particles with a particle size of 0.5 mm; As shown in Table 1, the cyclone pre-tailing process pre-discarded 26.35% of the waste rock with a silver grade of 51.65 g / t, which increased the ore processing capacity entering the grinding-flotation stage by 26.35% and improved the efficiency of the grinding-flotation treatment; greatly improved the valuable metal grade of the ore and reduced the separation cost of subsequent grinding and other treatments.
[0068] Although Example 1 of the present application discarded 26.35% of the waste rock with a silver grade of 51.65 g / t, it only lost 3.07% of the silver recovery rate, which is a small loss and has little impact on the comprehensive recovery rate of the silver ore.
[0069] Comparative Example 1 Reference Figure 3 The method for pre-tailing-floating silver ore shown is carried out as follows: Crushing and screening: Crushing silver ore with Ag content of 433.8 g / t to less than 10 mm; Grinding: The screened ore is then ground so that particles with a size of 325 mesh account for 85% of the total ore; Roughing: add 0-50 g / t of ethyl xanthate, 0-30 g / t of ethyl thiocyanate and 0-40 g / t of butylamine black medicine to the mixed system after grinding, react for 3 minutes, and then carry out the first roughing for 4 minutes, then add 0-300 g / t of copper sulfate, an activator, to the ore obtained from the first roughing, and after 5 minutes of activation reaction, add 0-50 g / t of ethyl xanthate, 0-30 g / t of ethyl thiocyanate and 0-40 g / t of butylamine black medicine, react for 3 minutes, and then carry out the second roughing for 4 minutes to obtain a silver rough concentrate and rough tailings; Concentration: adding 0-200 g / t of water glass as an inhibitor to the silver rough concentrate, after acting for 5 minutes, carrying out the first concentration for 4 minutes, adding 0-100 g / t of water glass as an inhibitor to the ore obtained by the first concentration, after acting for 5 minutes, carrying out the second concentration for 4 minutes, carrying out the third concentration for 4 minutes on the ore obtained by the second concentration, and then carrying out the fourth concentration for 4 minutes to obtain the first silver concentrate; Sweeping: add activator copper sulfate 0-100 g / t to the coarse tailings, after 5 minutes of activation reaction, add collector ethyl xanthate 0-30 g / t, ethyl thiocyanate 0-10 g / t and butylamine black medicine 0-20 g / t, and foaming agent 2# oil 0-10 g / t, after 3 minutes of action, carry out the first sweeping for 3 minutes, add collector ethyl xanthate 0-20 g / t, ethyl thiocyanate 0-10 g / t and butylamine black medicine 0-10 g / t to the ore obtained by the first sweeping, after 3 minutes of action, carry out the second sweeping for 3 minutes, add collector ethyl xanthate 0-20 g / t, ethyl thiocyanate 0-10 g / t and butylamine black medicine 0-10 g / t to the ore obtained by the second sweeping, after 3 minutes of action, carry out the second sweeping. The second silver concentrate (also called tailings) is obtained by the third scavenging of min. The second silver concentrate is added to the next roughing stage and mixed with the mixing system for subsequent treatment such as re-roughing.
[0070] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not have a heavy medium separation treatment step, and grinding and flotation are directly performed after crushing and screening. The separation results of Example 1 and Comparative Example 1 are shown in Table 2.
[0071] Table 2
[0072] According to Table 2, in Comparative Example 1, the ore grade entering the grinding-flotation stage is lower, and some low-grade waste rocks are processed together, but the content of low-grade waste rocks is too high, resulting in higher separation costs. According to the method of Example 1, by pre-discarding about 26% of the waste rocks, the subsequent flotation processing capacity is increased by 26%, so that the obtained concentrate grade is higher, and the recovery rate is equivalent to that of Comparative Example 1. It is proved that even if the waste rocks are discarded in advance, the impact on the recovery rate is negligible, and efficient recovery can still be achieved, and the separation cost of the flotation stage can also be reduced.
[0073] According to Table 1, compared with Comparative Example 1, Example 1 of the present application processes one ton of ore after tailings disposal under the same grinding and flotation system processing capacity. Since the ore grade after tailings disposal in Example 1 increases from 443.31 g / t to 588.58 g / t, the grinding-flotation selection grade is improved, and the discarded waste rock can be used as building materials. At the same time, the tailings processing cost can be reduced, and the potential economic benefits are very large.
[0074] In summary, the present application provides a method for pre-discarding tailings and flotation of silver ore, which adds ore (first coarse ore) with a particle size of not less than 0.5 mm into a cyclone for sorting, discards low-grade waste rock, and mixes the obtained heavy medium concentrate with ore (first coarse ore) with a particle size of less than 0.5 mm, so as to obtain an ore with increased grade that can be used in the grinding-flotation stage. This method can discard at least 20% of the waste rock, greatly reducing the processing volume of the subsequent grinding-flotation stage, thereby reducing the energy consumption and cost of sorting. The discarded waste rock can be used as building materials, and the processing cost of tailings can also be reduced, with great potential economic benefits.
[0075] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0076] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.
[0077] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.
[0078] The above is a detailed introduction to a process of pre-tailing-floating silver ore provided by the present application. Specific examples are used in this article to illustrate the principle and implementation method of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present application.
Claims
1. A method for pre-tailing-floating silver ore, characterized in that: The method comprises: S1. After the silver ore is crushed, it is screened to obtain a first coarse ore with a particle size of not less than 0.5 mm and a second coarse ore with a particle size of less than 0.5 mm; S2, performing heavy medium separation on the first coarse ore to obtain heavy medium concentrate and heavy medium tailings; S3, crushing the heavy medium concentrate and mixing it with the second coarse ore, grinding the obtained mixed system, adding a collector and / or an activator, and performing rough separation to obtain a silver coarse concentrate and coarse tailings; S4, adding an inhibitor to the silver rough concentrate to perform concentration to obtain a first silver concentrate; S5. Adding a collector, an activator and / or a frother to the coarse tailings for scavenging to obtain a second silver concentrate.
2. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: The collector includes ethyl xanthate, ethyl thiocyanate and / or butylamine black medicine; The activator is copper sulfate; The inhibitor is water glass, sodium sulfite or sodium carbonate; The foaming agent is pine oil.
3. The method for pre-tailing-floating silver ore according to claim 1 or 2, characterized in that: In step S3, the rough selection includes: Add a collector to the ground heavy medium concentrate, react for 1 min to 5 min, and then perform a first roughing for 2 min to 10 min; An activator is added to the ore obtained from the first roughing, and after an activation reaction for 3 min to 10 min, an appropriate amount of a collector is added, and after a reaction for 1 min to 5 min, a second roughing for 2 min to 10 min is performed to obtain a silver rough concentrate and a rough tailing.
4. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: In step S4, the selection includes: Add an inhibitor to the silver rough concentrate, react for 1 min to 10 min, and then perform a first concentration for 2 min to 10 min; Adding an inhibitor to the ore obtained from the first concentration, reacting for 1 min to 10 min, and then performing a second concentration for 2 min to 10 min; The ore obtained from the second concentration is subjected to a third concentration for 2 min to 10 min, and then subjected to a fourth concentration for 2 min to 10 min to obtain a first silver concentrate.
5. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: In step S5, the scanning includes: Add an activator to the coarse tailings, and after the activation reaction for 3 min to 10 min, add an appropriate amount of collector and frother, react for 1 min to 5 min, and then perform a first sweep for 1 min to 10 min; Adding an appropriate amount of collector to the ore obtained from the first scavenging, reacting for 1 min to 5 min, and then performing a second scavenging for 1 min to 10 min; An appropriate amount of collector is added to the ore obtained from the second scavenging, and after reacting for 1 min to 5 min, a third scavenging is performed for 1 min to 10 min to obtain the second silver concentrate.
6. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: In step S2, the mass percentages of the heavy medium concentrate and the heavy medium tailings are (60-85)%:(15-40)%.
7. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: In step S2, when the first coarse ore is subjected to heavy medium separation, the heavy medium is magnetic iron or ferrosilicon ore.
8. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: In step S3, after the heavy medium concentrate is crushed, the particle size of the obtained particles is less than 2 mm.
9. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: In step S3, after the obtained mixed system is ground, particles with a mesh size of 200-350 mesh account for 70%-90% of the total mass of the particles.
10. The method for pre-tailing-floating silver ore according to claim 1, characterized in that: In step S1, the particle size of the first coarse ore is less than 10 mm.