Green ceramic chip and laser drilling method thereof
By adjusting the laser beam parameters according to the thickness and hole shape of the raw ceramic sheet in HTCC technology for overall drilling, the line reliability problem caused by appearance deviation in the single-layer raw ceramic sheet stacking process is solved, and the production efficiency and holes are improved. Alignment.
Patent Information
- Application Number
- CN202411403871.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-09
AI Technical Summary
In HTCC technology, there is a problem of appearance deviation in the lamination process of multiple single-layer ceramic flakes, resulting in a reduced line reliability between stacks. How to improve the line reliability between single-layer ceramic flakes has become an urgent solution. question.
After forming the raw ceramic sheet to be punched, determine whether the depth of focus compensation parameters need to be set according to its thickness and the shape of the target hole, select appropriate laser beam processing parameters for overall drilling, ensure the alignment and shape of the holes, and improve laser drilling Reliability of holes.
This method improves the circuit reliability between single-layer raw ceramic tiles, reduces the impact of appearance quality differences on production efficiency, overcomes the problem of hole failure caused by the difficulty of special-shaped hole processing, and improves the overall drilling yield and reliability.
Smart Images

Figure CN118989669A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of HTCC, and in particular to a green ceramic sheet and a laser drilling method thereof. Background Art
[0002] HTCC (High Temperature Co-fired Ceramic) is a method of mixing ceramic powder with additives such as solvents, binders, dispersants, plasticizers, etc. into a slurry, obtaining a green ceramic tape through tape casting technology, cutting the green ceramic tape into multiple single-layer green ceramic sheets of fixed size, and then performing laser drilling one by one. The conductive metal is used to fill holes and design circuits on each single-layer green ceramic sheet using screen printing technology, and then the multiple punched single-layer green ceramic sheets are stacked, pressed, and cut. They are sintered at high temperature (such as 1500-1850℃) and inert gas protective atmosphere to form multi-layer green ceramic sheets, and finally realize vertical interconnection between different layers to complete the connection between metal and ceramic.
[0003] However, as the requirements for product appearance quality and line reliability become increasingly stringent, the problem of deviation in the appearance of multiple single-layer raw ceramic sheets cannot be avoided in the lamination process, which in turn leads to reduced line reliability between the laminated layers. Therefore, how to improve the line reliability between multiple single-layer raw ceramic sheets has become a problem that needs to be solved urgently. Summary of the invention
[0004] To solve one or more of the above problems, the disclosed embodiment proposes a raw ceramic sheet and a laser drilling method thereof. In one aspect, the laser drilling method for a raw ceramic sheet includes: forming a plurality of single-layer raw ceramic sheets; sequentially stacking the plurality of single-layer raw ceramic sheets in a first direction to form a raw ceramic sheet to be punched; the first direction is perpendicular to the surface of the single-layer raw ceramic sheet; obtaining the thickness of the raw ceramic sheet to be punched in the first direction; obtaining the shape of the target hole to be formed in the raw ceramic sheet to be punched; determining that when the thickness is greater than 1 mm and / or the shape of the target hole includes a straight line segment, the processing parameters of the laser beam include a depth of focus compensation parameter; based on the processing parameters, applying the laser beam to the raw ceramic sheet to be punched to form the target hole that penetrates the raw ceramic sheet to be punched.
[0005] In some embodiments, the depth of focus compensation parameters include 0.01 mm / 10 times and 0.05 mm / 10 times.
[0006] In some embodiments, based on the processing parameters, the laser beam is applied to the raw ceramic sheet to be punched to form the target hole penetrating the raw ceramic sheet, including: based on the processing parameters, the laser beam is applied to a first area of the raw ceramic sheet to be punched to form a first target hole penetrating the raw ceramic sheet; and based on the processing parameters, the laser beam is applied to a second area of the raw ceramic sheet to be punched to form a second target hole penetrating the raw ceramic sheet; the shape of the first target hole is different from the shape of the second target hole.
[0007] In some embodiments, when the shape of the second targeting hole includes a straight line segment, the shape of the second targeting hole includes an elliptical racetrack shape, a regular or irregular polygonal shape.
[0008] In some embodiments, the shape of the first target aperture comprises a circle; and the shape of the second target aperture comprises an elliptical racetrack shape.
[0009] In some embodiments, the diameter width of the first target hole in the second direction is greater than or equal to 0.01 mm; and the second direction is perpendicular to the first direction.
[0010] In some embodiments, the processing parameters of the laser beam also include: laser power, number of processing passes of the laser galvanometer, and marking speed; wherein the numerical range of the laser power is 5-10 watts, the numerical range of the number of processing passes is 30-40 times, and the numerical range of the marking speed is 200-400 mm / s.
[0011] In some embodiments, applying the laser beam to the green ceramic sheet to be punched includes: covering the surface of the green ceramic sheet to be punched with a polyester film; and applying the laser beam through the polyester film to the surface of the green ceramic sheet to be punched.
[0012] On the other hand, a green porcelain sheet is provided in an embodiment of the present disclosure, and the green porcelain sheet is prepared by the method described in the above embodiment of the present disclosure; wherein a target hole penetrating the green porcelain sheet is provided in the green porcelain sheet; the thickness of the green porcelain sheet in a first direction is greater than 1 mm; and / or the shape of the target hole includes a straight line segment; the first direction is perpendicular to the surface of the green porcelain sheet.
[0013] In some embodiments, the target holes include a first target hole located in a first area of the green ceramic sheet, and a second target hole located in a second area of the green ceramic sheet; wherein a shape of the second target hole includes a straight line segment.
[0014] In the disclosed embodiment, a raw ceramic sheet to be punched is formed by stacking a plurality of single-layer raw ceramic sheets; the thickness of the raw ceramic sheet to be punched and the shape of the target hole to be formed are obtained, and it is determined whether the thickness of the raw ceramic sheet to be punched is greater than 1 mm, and whether the shape of the target hole includes a straight line segment, so as to determine whether the processing parameters of the laser beam are set with a depth of focus compensation parameter, and then a better and more suitable laser parameter is selected to perform overall punching on the raw ceramic sheet to be punched, so as to obtain the desired target hole; wherein, by performing overall punching on the raw ceramic sheet to be punched, the difficulty of aligning the target holes in the plurality of single-layer raw ceramic sheets can be reduced, the appearance quality can be improved, and the yield effect of the entire raw ceramic sheet due to appearance deviation can be reduced, thereby improving production efficiency; further, by adding a depth of focus compensation parameter to the processing parameters of the laser beam, the raw ceramic sheet to be punched with a thickness exceeding 1 mm can be punched as a whole, and the problem of target holes not being punched through due to the difficulty in processing special-shaped holes (such as target holes including straight line segments) can be overcome, thereby improving the reliability of laser drilling. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 A schematic diagram of a process for laser drilling a green ceramic sheet according to an embodiment of the present disclosure;
[0016] Figure 2 A schematic diagram of the cross-sectional structure of a green ceramic sheet to be punched provided in one embodiment of the present disclosure;
[0017] Figure 3 A schematic diagram of the cross-sectional structure of a polyester film provided in one embodiment of the present disclosure;
[0018] Figure 4 A schematic diagram of placing a green ceramic sheet to be punched in a laser punching device according to an embodiment of the present disclosure;
[0019] Figure 5 A schematic diagram of a cross-sectional structure of a green ceramic sheet with a target hole on an XZ plane provided in an embodiment of the present disclosure;
[0020] Figure 6 A schematic diagram of the cross-sectional structure of a green ceramic sheet with target holes of various shapes on the XY plane provided in one embodiment of the present disclosure.
[0021] Reference numerals
[0022] 200 - raw ceramic sheet; 201 - single-layer raw ceramic sheet; 202 - raw ceramic sheet to be punched; 203 - polyester film; 204 - target hole; 2041 - first target hole; 2042 - second target hole.
[0023] In the above drawings (which are not necessarily drawn to scale), similar reference numerals may describe similar components in different views. Similar reference numerals with different letter suffixes may represent different examples of similar components. The accompanying drawings generally illustrate various embodiments discussed herein by way of example and not limitation. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present disclosure and the accompanying drawings to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0025] In the following description, a large number of specific details are given to provide a more thorough understanding of the present disclosure. However, it is obvious to those skilled in the art that the present disclosure can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present disclosure, some technical features known in the art are not described; that is, all features of actual embodiments are not described here, and well-known functions and structures are not described in detail.
[0026] In the drawings, the sizes of layers, regions, elements and their relative sizes may be exaggerated for clarity. Like reference numerals denote like elements throughout.
[0027] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not indicate that the present disclosure necessarily has the first element, component, region, layer or part.
[0028] Spatially relative terms such as "under", "beneath", "below", "under", "above", "above", etc., may be used here for convenience of description to describe the relationship between an element or feature shown in the figure and other elements or features. It should be understood that in addition to the orientation shown in the figure, the spatial relationship terms are intended to also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is turned over, then the elements or features described as "under other elements" or "under it" or "under it" will be oriented as "on" other elements or features. Therefore, the exemplary terms "under" and "under" may include both upper and lower orientations. The device can be oriented otherwise (rotated 90 degrees or other orientations) and the spatial descriptors used herein are interpreted accordingly.
[0029] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be a limitation of the present disclosure. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0030] In order to thoroughly understand the present disclosure, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present disclosure. The preferred embodiments of the present disclosure are described in detail below, but in addition to these detailed descriptions, the present disclosure may also have other implementations.
[0031] The principle of laser drilling is to use a laser drilling device to place the focal position of the laser beam on the surface of the sample (such as a raw porcelain piece) during laser drilling. By adjusting the processing parameters of the laser beam, the focal position reaches a molten state, and then vaporizes to form a circular pit. The laser beam moves under the control of the host (such as a computer, etc.), so that the multiple circular pits formed partially overlap, thereby forming a target hole (or a through hole); wherein, the raw porcelain debris cut off by the laser beam is adsorbed into the waste box by a vacuum adsorption device to ensure that the surface of the raw porcelain piece is clean and tidy. In the laser drilling process, the preparation of target holes of different shapes / sizes is mainly achieved by adjusting the processing parameters of the laser beam.
[0032] It should be noted that laser drilling devices are widely used due to their fast speed, high precision, flexibility, etc. When using laser drilling devices for laser drilling, it is necessary to select appropriate laser parameters according to different workpiece materials and drilling requirements, and reasonably design the laser drilling path to achieve good processing results.
[0033] In some embodiments, the laser drilling device includes a laser source, a laser beam transmission system, a scanning system, a control system and a sample placement position; wherein the laser source is generally a semiconductor laser or a solid-state laser. The laser source is used to generate a high-energy, continuous or pulsed laser beam. The laser beam transmission system can be used to adjust and focus the output of the laser beam. In some embodiments, the laser beam transmission system includes a lens and an optical fiber, which are used to focus the laser beam to a certain position on the surface of the sample (such as a raw ceramic sheet), thereby achieving a high-energy density drilling effect. In the embodiment of the present disclosure, a laser galvanometer is also provided in the laser beam transmission system, and the laser galvanometer includes an XY optical scanning head, an electronic drive amplifier and an optical reflective lens; wherein the signal provided by the host drives the optical scanning head through the drive amplifier circuit, thereby controlling the deflection of the laser beam in the XY plane.
[0034] The scanning system includes a scanning head and a scanning mirror. The scanning system is used to control the movement trajectory of the laser beam on the surface of the sample (such as a raw ceramic sheet) to achieve accurate drilling position and shape. The control system can usually include two parts: a hardware system and a software system. The control system controls the switch of the laser light source, the adjustment of the laser beam and the movement of the scanning system to achieve accurate control of the laser drilling process. In actual operation, the laser drilling device can obtain the size of the sample (such as a raw ceramic sheet), such as length, width, thickness, etc., through the scanning system. The sample placement position is used to place samples, such as raw ceramic sheets to be punched.
[0035] In some embodiments, the preparation process of the HTCC device includes first forming a plurality of thin single-layer green ceramic sheets, then using a laser punching device to punch holes in the plurality of thin single-layer green ceramic sheets one by one, and stacking the punched single-layer green ceramic sheets to form a multi-layer green ceramic sheet and a target hole located in the multi-layer green ceramic sheet, and then filling the target hole with a conductive paste to achieve interconnection between the multi-layer green ceramic sheets.
[0036] Considering that the alignment quality of the target hole in the multi-layer green ceramic sheet and the appearance deviation of each single-layer green ceramic sheet may affect the reliability of the HTCC device, a method for punching holes in the multi-layer green ceramic sheet as a whole is proposed in the embodiment of the present disclosure to improve the alignment quality of the target hole and reduce the influence of the appearance deviation of each single-layer green ceramic sheet on the reliability of the HTCC device. The specific operation includes: first forming a plurality of thin single-layer green ceramic sheets, stacking the plurality of single-layer green ceramic sheets to form a multi-layer green ceramic sheet, and then using a laser punching device to punch holes in the multi-layer green ceramic sheet as a whole to form a target hole in the multi-layer green ceramic sheet, and then filling the target hole with a conductive paste to achieve interconnection between the multi-layer green ceramic sheets.
[0037] In this way, by punching holes in a multilayer raw ceramic sheet composed of multiple single-layer raw ceramic sheets as a whole, the appearance quality of the product can be greatly improved, and the problem of poor appearance caused by the stacking deviation of multiple single-layer raw ceramic sheets can be reduced; a new processing method can be provided for some products with strict requirements on appearance quality; and a good foundation can be laid for through-hole metallization, thereby improving the appearance quality of device wall hanging; the problem of ceramic sheet stratification caused by slurry accumulation in the wall hanging holes when a single layer is hung on the wall can be reduced; in addition, since the time for punching holes in multiple single-layer raw ceramic sheets as a whole is less than the total time for punching holes in multiple single-layer raw ceramic sheets one by one, the production efficiency can also be improved.
[0038] However, in the process of overall drilling of the multi-layer green ceramic sheet using a laser drilling device, due to the influence of factors such as the thickness of the multi-layer green ceramic sheet and the shape of the target hole to be formed, the multi-layer green ceramic sheet is not drilled through, that is, the target hole cannot penetrate the multi-layer green ceramic sheet, thereby reducing the drilling yield and drilling efficiency of the multi-layer green ceramic sheet, affecting the interconnection and reliability of the HTCC device.
[0039] Based on one or more of the above problems, a laser drilling method for a raw ceramic sheet is proposed in the embodiment of the present disclosure. Figure 1 , Figure 1 The present invention is a schematic flow chart of a laser drilling method for a green ceramic sheet according to an embodiment of the present invention, wherein the method comprises the following steps:
[0040] Step S101: forming a plurality of single-layer green ceramic sheets.
[0041] Step S102: stacking a plurality of single-layer green ceramic sheets in sequence in a first direction to form a green ceramic sheet to be punched; the first direction is perpendicular to the surface of the single-layer green ceramic sheet.
[0042] Step S103: obtaining the thickness of the green ceramic sheet to be punched in the first direction.
[0043] Step S104: obtaining the shape of the target hole to be formed in the green ceramic sheet to be punched.
[0044] Step S105: When it is determined that the thickness is greater than 1 mm and / or the shape of the target hole includes a straight line segment, the processing parameters of the laser beam include a depth of focus compensation parameter.
[0045] Step S106: Based on the processing parameters, a laser beam is applied to the green ceramic sheet to be punched to form a target hole penetrating the green ceramic sheet.
[0046] It should be understood that Figure 1 The steps shown in the operation are not exclusive, and other steps may be performed before, after or between any steps in the operation shown; Figure 1The steps shown in the figure can be adjusted in order according to actual needs. Before introducing the content of the present disclosure in detail, various directions that may be used in the following description are defined. In the present disclosure, the direction in which multiple single-layer raw ceramic sheets are stacked and pressed is defined as a first direction (i.e., the Z-axis direction). In a plane perpendicular to the Z-axis direction, a second direction (i.e., the X-axis direction) and a third direction (i.e., the Y-axis direction) that intersect are defined. In some embodiments, the X-axis direction, the Y-axis direction, and the Z-axis direction can be perpendicular to each other.
[0047] refer to Figure 2 , perform step S101 and step S102 to form a plurality of single-layer raw ceramic sheets 201, and stack the plurality of single-layer raw ceramic sheets 201 in sequence along the Z-axis direction to form a raw ceramic sheet 202 to be punched. The raw ceramic sheet to be punched mentioned here can be understood as the multi-layer raw ceramic sheet mentioned in the above embodiment. It should be noted that the material of the single-layer / multi-layer raw ceramic sheet or the raw ceramic sheet to be punched includes but is not limited to insulating materials, such as aluminum oxide (Al2O3), aluminum nitride (AlN), etc.
[0048] The method of forming the single-layer green ceramic sheet 201 includes but is not limited to the tape casting method. Exemplarily, the specific method of forming the alumina green ceramic sheet may include: mixing ceramic powder, adhesive, plasticizer and solvent evenly to form a green ceramic slurry, and then tape casting and cutting the green ceramic slurry to obtain multiple single-layer green ceramic sheets by the tape casting method. Here, the ceramic powder may include but is not limited to a mixed powder of alumina powder and glass powder; the adhesive may include but is not limited to polyvinyl butyral; the plasticizer may include but is not limited to dibutyl phthalate; the solvent may include but is not limited to ethanol, isopropanol and ethyl acetate, etc.
[0049] The thickness of each single-layer green ceramic sheet 201 in the plurality of single-layer green ceramic sheets 201 in the Z-axis direction may be the same or different. Figure 2 The thickness of the multiple single-layer green ceramic sheets 201 in the Z-axis direction is the same. It should be understood that the thickness of the green ceramic sheet 202 to be punched in the Z-axis direction is the sum of the thicknesses of the multiple single-layer green ceramic sheets 201 in the Z-axis direction. Figure 2 The thickness of the green ceramic sheet 202 to be punched in the Z-axis direction is H2, the thickness of each single-layer green ceramic sheet 201 in the Z-axis direction is H1, and the green ceramic sheet 202 to be punched includes 8 single-layer green ceramic sheets 201, that is, H2=8*H1. Exemplarily, the thickness H2 of the green ceramic sheet 202 to be punched in the Z-axis direction is 1.0-1.5 millimeters (mm).
[0050] It should be understood that the number of single-layer green ceramic sheets included in the green ceramic sheets to be punched 202 can be set according to actual needs, and only eight layers are used as an example for illustrative description.
[0051] refer to Figure 3Before executing step S103, the method further includes: covering the surface of the green ceramic sheet 202 to be punched with a polyester film 203. The polyester film 203 is used to protect the green ceramic sheet 202 to be punched during the laser punching process. Here, the material of the polyester film 203 can be a plastic film material made of polyester resin, which has the characteristics of high transparency, good mechanical strength, high chemical stability, etc. Exemplarily, the polyester film 203 includes but is not limited to polyethylene terephthalate (PET), polycarbonate (PC board), and ethylene-vinyl acetate polymer (EVA).
[0052] In some embodiments, the thickness H3 of the polyester film 203 in the Z-axis direction is less than the thickness H2 of the raw ceramic sheet 202 to be punched in the Z-axis direction, that is, H3 < H2. In other embodiments, the thickness H3 of the polyester film 203 in the Z-axis direction is less than the thickness H1 of a single-layer raw ceramic sheet 201 in the Z-axis direction, that is, H3 < H1.
[0053] refer to Figure 4 , Figure 4 A partial structural schematic diagram of a laser drilling device provided in an embodiment of the present disclosure; wherein the method further comprises: placing a raw ceramic sheet 202 to be drilled covered with a polyester film 203 in a sample placement position of the laser drilling device.
[0054] Execute step S103: the laser drilling device is configured to obtain the thickness H2 of the raw ceramic sheet 202 to be punched in the Z-axis direction; and judge the obtained thickness H2 of the raw ceramic sheet 202 to be punched in the Z-axis direction to determine whether the thickness H2 of the raw ceramic sheet 202 to be punched in the Z-axis direction is greater than 1 mm. Judgment result 1 is that the thickness H2 of the raw ceramic sheet 202 to be punched in the Z-axis direction is greater than 1 mm; judgment result 2 is that the thickness H2 of the raw ceramic sheet 202 to be punched in the Z-axis direction is less than or equal to 1 mm. It should be noted that when the thickness H2 of the raw ceramic sheet 202 to be punched in the Z-axis direction is greater than 1 mm, problems such as difficulty in punching or incomplete punching may be encountered.
[0055] It should be understood that the 1 mm mentioned here is a preset value, which can also be set according to actual needs; in other embodiments, the preset value can also be 0.6 mm, 0.8 mm or 1.2 mm, etc.
[0056] Step S104 is executed, and the laser drilling device is configured to obtain the shape of the target hole to be formed in the green ceramic sheet 202 to be drilled; and judge the obtained shape of the target hole to determine whether the shape contour of the target hole includes a straight line segment. Judgment result three is that the shape contour of the target hole includes a straight line segment; judgment result four is that the shape contour of the target hole does not include a straight line segment.
[0057] Among them, if the shape contour of the target hole includes a straight line segment, it means that at least one segment of the laser path during the laser drilling process is a straight line. It should be noted that under the same processing parameters, the system (drilling) of a straight line segment is more difficult than that of an arc segment (such as a circular arc). In other words, the difficulty of making a special-shaped hole is higher than that of making a circular hole. Under the same processing parameters, there may also be problems such as difficulty in drilling or impermeable drilling when making a special-shaped hole.
[0058] In some specific embodiments, when the shape of the target hole includes a straight line segment, the shape of the target hole can be an elliptical track shape, a regular or irregular polygonal shape; here, the regular or irregular polygonal shape is such as a rectangle, square, triangle, parallelogram, fan, etc.
[0059] Step S105 is executed to perform a laser drilling operation on the raw ceramic sheet to be punched based on the above judgment result. Specifically: when the judgment result of the laser drilling device determines that the thickness H2 of the raw ceramic sheet to be punched in the Z-axis direction is greater than 1 mm (i.e., judgment result 1), when laser drilling is performed, the processing parameters of the laser beam include a depth of focus compensation parameter. And / or, when the judgment result of the laser drilling device determines that the shape of the target hole includes a straight line segment (i.e., judgment result 3), when laser drilling is performed, the processing parameters of the laser beam include a depth of focus compensation parameter.
[0060] It should be noted that when executing step S105, only at least one of the above judgment results 1 and 3 can be satisfied, and the processing parameters of the laser beam can be set to include the depth of focus compensation parameters during the laser drilling process. In other words, when the above judgment result 1 is satisfied, even if the shape of the target hole to be formed does not include a straight line segment, such as the shape of the target hole is circular, in the laser drilling process, the processing parameters of the laser beam still include the depth of focus compensation parameters. That is, when the above judgment result 3 is satisfied, even if the thickness H2 of the raw ceramic sheet 202 to be drilled in the Z-axis direction is less than or equal to 1 mm, in the laser drilling process, the processing parameters of the laser beam still include the depth of focus compensation parameters.
[0061] In some embodiments, the depth of focus compensation parameter is 0.01 mm / 10 times, i.e., 0.01 / 10 mm / time, 0.05 mm / 10 times, i.e., 0.05 / 10 mm / time. It should be noted that 0.01 mm / 10 times means that during laser drilling, the laser focus drops 0.01 mm in the depth direction for every 10 times of processing. The depth direction mentioned here can be understood as the direction from the surface of the green ceramic sheet to be drilled to the bottom surface of the green ceramic sheet to be drilled.
[0062] In other embodiments, the depth of focus compensation parameter may also be other values, which will not be described in detail here.
[0063] It should be noted that during the laser drilling process, after multiple processing, as the depth of the target hole decreases, the focus of the laser will become out of focus as the depth decreases. Therefore, setting the depth of focus compensation parameter in the laser beam processing parameters helps the laser beam focus on the raw ceramic sheet to be punched. It can also be understood that the depth of focus compensation parameter can refocus the laser beam, thereby improving the reliability and yield of laser drilling. On the other hand, for special-shaped holes, increasing the depth of focus compensation can also reduce the difficulty of drilling, overcome problems such as difficult or impermeable drilling, and thus improve the drilling yield.
[0064] Execute step S106, refer to Figure 5 Based on the above processing parameters, a laser beam is applied to the green ceramic sheet 202 to be punched to form a target hole 204 penetrating the green ceramic sheet 202. In this way, a green ceramic sheet 200 having a target hole 204 can be formed. Figure 5 Schematic diagram of the cross-sectional structure of the green ceramic sheet 200 with the target hole on the XZ plane is shown in FIG.
[0065] In some embodiments, applying the laser beam to the green ceramic sheet to be punched includes applying the laser beam to the surface of the green ceramic sheet to be punched 202 through a polyester film 203. As mentioned above, the polyester film 203 includes but is not limited to PET, PC board, EVA, and the like.
[0066] It should be noted that after the laser drilling device determines the judgment result, when the above judgment result 2 and judgment result 4 are satisfied at the same time, the processing parameters of the laser beam may not include the depth of focus compensation parameter.
[0067] In some embodiments, the processing parameters of the laser beam also include: laser power, the number of processing passes of the laser galvanometer, and the marking speed.
[0068] It should be noted that the larger the laser power value, the greater the energy of the laser beam and the larger the pulse, and too high a laser power may cause device burning, affecting the reliability and yield of the device. In the disclosed embodiment, the laser power value range is 5-10 watts (W); preferably, the laser power value range is 6-9W.
[0069] The working principle of the laser galvanometer is to make the laser beam incident on two reflectors (scanning mirrors), and use a computer to control the reflection angle of the reflectors. The two reflectors can scan along the X and Y axes respectively to achieve the deflection of the laser beam, so that the laser focus with a certain power density moves along a specific trajectory on the workpiece material, thereby leaving a permanent mark on the surface of the material. The number of processing passes of the laser galvanometer can be understood as the number of times the laser galvanometer scans the workpiece during the drilling / processing process. In the embodiment of the present disclosure, the numerical range of the number of processing passes of the laser galvanometer is 30-40 times; preferably, the numerical range of the number of processing passes of the laser galvanometer is 35 times.
[0070] The marking speed can be understood as the speed at which the laser beam is output to scratch / mark a line on the workpiece. The slower the speed, the longer the laser beam stays at the same position, and the deeper the hole punched on the workpiece. In the disclosed embodiment, the numerical range of the marking speed is 200-400 millimeters per second (mm / s); preferably, the numerical range of the marking speed is 300 mm / s.
[0071] In some specific embodiments, the laser drilling device used is a 20W ultraviolet nanosecond laser with a laser wavelength of 355nm and a laser frequency range of 50-100kHz.
[0072] In the disclosed embodiment, by punching holes in the raw ceramic sheets to be punched, which are composed of a plurality of single-layer raw ceramic sheets, the appearance quality of the product can be greatly improved, and the problem of poor appearance caused by the stacking deviation of the plurality of single-layer raw ceramic sheets can be reduced, thereby providing a new processing method for some products with strict requirements on appearance quality; it can lay a good foundation for through-hole metallization and improve the appearance quality of the device hanging on the wall; it can reduce the problem of ceramic sheet stratification caused by slurry accumulation in the wall hanging holes when a single layer is hung on the wall; the time for punching holes in the plurality of single-layer raw ceramic sheets as a whole is less than the total time for punching holes in the plurality of single-layer raw ceramic sheets one by one, and therefore the production efficiency can also be improved. Furthermore, by obtaining the thickness of the raw ceramic sheet to be punched and the shape of the target hole to be formed, and judging whether the thickness of the raw ceramic sheet to be punched is greater than 1 mm, and whether the shape of the target hole includes a straight line segment, it is determined whether the processing parameters of the laser beam are set with a depth of focus compensation parameter, and then a better and more suitable laser parameter is selected to perform overall drilling on the raw ceramic sheet to be punched, so as to obtain the desired target hole; in this way, the raw ceramic sheet to be punched with a thickness exceeding 1 mm can be punched as a whole, and the problem of target holes not being punched through due to the difficulty in processing special-shaped holes can be overcome, thereby improving the reliability of laser drilling.
[0073] In some embodiments, when multiple (such as two) target holes of different shapes need to be set in the same raw ceramic sheet to be punched, the laser punching device can judge according to the thickness of the raw ceramic sheet to be punched and the shapes of multiple target holes (such as the first target hole and the second target hole) to determine the processing parameters of the laser beam when performing the laser punching operation. Specifically, when executing step S106, the method specifically includes: determining the processing parameters based on the judgment result of the laser punching device, based on the processing parameters, applying the laser beam to the first area of the raw ceramic sheet to be punched to form a first target hole that penetrates the raw ceramic sheet to be punched; and based on the processing parameters, applying the laser beam to the second area of the raw ceramic sheet to be punched to form a second target hole that penetrates the raw ceramic sheet to be punched; the shape of the first target hole is different from the shape of the second target hole.
[0074] In some embodiments, the shape of the first target hole does not include a straight line segment; the shape of the second target hole includes a straight line segment. In some specific embodiments, the shape of the second target hole includes an elliptical racetrack shape, a regular or irregular polygonal shape.
[0075] Exemplary, reference Figure 6 , Figure 6 2041 is a schematic diagram of a cross-sectional structure of a green ceramic sheet with target holes of different shapes on an XY plane; wherein the shape of the first target hole 2041 includes a circle; and the shape of the second target hole 2042 includes an elliptical racetrack shape.
[0076] In some embodiments, a diameter width L of the first target hole in the X-axis direction is greater than or equal to 0.01 mm.
[0077] Exemplary, reference Figure 6 The range of the diameter width L of the first target hole 2041 in the X-axis direction is: 0.01mm≤L≤0.35mm.
[0078] It should be noted that the diameter width of the circular target hole formed by the method described in the above embodiment of the present disclosure can reach 0.01 mm, so that the demand for tiny holes in different application scenarios of raw ceramic sheets can be met. In addition, the shape of the second target hole can be understood as the shape of a special-shaped hole. In other words, the method described in the above embodiment of the present disclosure can form a special-shaped hole based on the same processing parameters as the circular target hole, and based on the depth of focus compensation parameters in the processing parameters, overcome the problem of the target hole not being penetrated due to the difficulty of processing the special-shaped hole, and improve the yield and reliability of laser drilling.
[0079] In order to more clearly understand the present disclosure, the processing parameters of laser drilling are described in detail below in conjunction with specific embodiments.
[0080] Embodiment 1
[0081] The thickness H2 of the green ceramic sheet to be punched in the Z-axis direction is 1.5 mm; the laser power is 6 W; the number of processing passes of the laser galvanometer is 35 times; and the marking speed is 300 mm / s. Under the above processing parameters, a circular hole is formed in the first area of the green ceramic sheet to be punched, and a runway hole (i.e., a special-shaped hole) in the shape of an elliptical runway is formed in the second area of the green ceramic sheet to be punched. The punching results show that neither the circular hole nor the runway hole is punched through.
[0082] Embodiment 2
[0083] The thickness H2 of the green ceramic sheet to be punched in the Z-axis direction is 1mm; the laser power is 6W; the number of processing passes of the laser galvanometer is 35 times; and the marking speed is 300mm / s. Under the above processing parameters, circular holes are formed in the first area of the green ceramic sheet to be punched, and runway holes (i.e., special-shaped holes) in the shape of an elliptical runway are formed in the second area of the green ceramic sheet to be punched. The punching results show that the circular holes are punched through, while the runway holes are not punched through.
[0084] Embodiment 3
[0085] The thickness H2 of the green ceramic sheet to be punched in the Z-axis direction is 1mm; the laser power is 6W; the number of processing passes of the laser galvanometer is 35 times; the marking speed is 300mm / s; the depth of focus compensation parameter is 0.01 / 10mm / time. Under the above processing parameters, a circular hole is formed in the first area of the green ceramic sheet to be punched, and a runway hole (i.e., a special-shaped hole) in the shape of an elliptical runway is formed in the second area of the green ceramic sheet to be punched. The punching results show that both the circular hole and the runway hole are punched through.
[0086] Embodiment 4
[0087] The thickness H2 of the green ceramic sheet to be punched in the Z-axis direction is 1mm; the laser power is 9W; the number of processing passes of the laser galvanometer is 35 times; the marking speed is 300mm / s; the depth of focus compensation parameter is 0.05 / 10mm / time. Under the above processing parameters, a circular hole is formed in the first area of the green ceramic sheet to be punched, and a runway hole (i.e., a special-shaped hole) in the shape of an elliptical runway is formed in the second area of the green ceramic sheet to be punched. The punching results show that both the circular hole and the runway hole are punched through.
[0088] Based on the above-mentioned first and second embodiments, it can be known that under the same processing parameters, when the thickness of the green ceramic sheet to be punched exceeds 1 mm, both the circular holes and the irregular holes cannot be punched through; when the thickness is 1 mm, the circular holes can be punched through, but the irregular holes cannot be punched through.
[0089] Based on the above-mentioned second and third embodiments, it can be known that when the thickness is 1 mm, after adding the depth of focus compensation parameter in the processing parameters, the irregular-shaped hole is also punched through. In other words, adding the depth of focus compensation parameter helps to improve the punching yield of the irregular-shaped hole.
[0090] Based on the above-mentioned Embodiment 3 and Embodiment 4, it can be known that by changing the depth of the depth of focus compensation parameter and changing the laser power, it is helpful to improve the yield of the drilling of special-shaped holes. It should be understood that the laser power cannot be increased indefinitely. Excessive power may cause device burning, affecting the reliability and yield of the device. By adjusting the depth of focus compensation parameter and the laser power, the yield of the target hole and the yield of the HTCC device can be further guaranteed.
[0091] Based on the above-mentioned laser drilling method for raw porcelain sheets, the embodiments of the present disclosure further provide a raw porcelain sheet, which is prepared by the method described in the above-mentioned embodiments of the present disclosure; wherein a target hole penetrating the raw porcelain sheet is provided in the raw porcelain sheet; the thickness of the raw porcelain sheet in the first direction is greater than 1 mm; and / or the shape of the target hole includes a straight line segment; the first direction is perpendicular to the surface of the raw porcelain sheet.
[0092] In some embodiments, the target holes include: a first target hole located in a first area of the green ceramic sheet, and a second target hole located in a second area of the green ceramic sheet; the first target hole and the second target hole have different shapes.
[0093] In some embodiments, the shape of the second targeting aperture includes straight line segments.
[0094] In some embodiments, the shape of the first target hole includes a circle; the shape of the second target hole includes an elliptical racetrack shape, a regular or irregular polygonal shape.
[0095] It should be understood that "one embodiment" or "an embodiment" mentioned throughout the specification means that specific features, structures or characteristics related to the embodiment are included in at least one embodiment of the present disclosure. Therefore, "in one embodiment" or "in an embodiment" appearing throughout the specification does not necessarily refer to the same embodiment. In addition, these specific features, structures or characteristics can be combined in one or more embodiments in any suitable manner. It should be understood that in the various embodiments of the present disclosure, the size of the serial number of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present disclosure. The serial numbers of the embodiments of the present disclosure are for description only and do not represent the advantages and disadvantages of the embodiments.
[0096] The above description is only a preferred embodiment of the present disclosure, and does not limit the patent scope of the present disclosure. All equivalent structural changes made by using the contents of the present disclosure and the drawings under the inventive concept of the present disclosure, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present disclosure.
Claims
1. A method for laser drilling of raw ceramic sheets, It is characterized in that The method comprises: forming a plurality of single-layer green ceramic sheets; stacking a plurality of the single-layer green ceramic sheets in sequence in a first direction to form a green ceramic sheet to be punched; the first direction is perpendicular to the surface of the single-layer green ceramic sheet; Obtaining the thickness of the green ceramic sheet to be punched in the first direction; Acquiring the shape of a target hole to be formed in the green ceramic sheet to be punched; When it is determined that the thickness is greater than 1 mm, and / or the shape of the target hole includes a straight line segment, the processing parameters of the laser beam include a depth of focus compensation parameter; Based on the processing parameters, the laser beam is applied to the green ceramic sheet to be punched to form the target hole penetrating the green ceramic sheet to be punched.
2. The method according to claim 1, It is characterized in that The focal depth compensation parameters include 0.01 mm / 10 times and 0.05 mm / 10 times.
3. The method according to claim 1, It is characterized in that Based on the processing parameters, the laser beam is applied to the green ceramic sheet to be punched to form the target hole penetrating the green ceramic sheet, including: Based on the processing parameters, applying the laser beam to a first area of the green ceramic sheet to be punched to form a first target hole penetrating the green ceramic sheet to be punched; and Based on the processing parameters, the laser beam acts on a second area of the green ceramic sheet to be punched to form a second target hole penetrating the green ceramic sheet to be punched; A shape of the first targeting hole is different from a shape of the second targeting hole.
4. The method according to claim 3, It is characterized in that When the shape of the second target hole includes a straight line segment, the shape of the second target hole includes an elliptical racetrack shape, a regular or irregular polygonal shape.
5. The method according to claim 4, It is characterized in that The shape of the first target hole includes a circle; the shape of the second target hole includes an elliptical racetrack shape.
6. The method according to claim 5, It is characterized in that The diameter width of the first target hole in the second direction is greater than or equal to 0.01 mm; and the second direction is perpendicular to the first direction.
7. The method according to claim 1, It is characterized in that The processing parameters of the laser beam also include: laser power, the number of processing passes of the laser galvanometer, and the marking speed; Wherein, the numerical range of the laser power is 5-10 watts, the numerical range of the processing times is 30-40 times, and the numerical range of the marking speed is 200-400 mm / s.
8. The method according to claim 1, It is characterized in that The step of applying the laser beam to the green ceramic sheet to be punched comprises: A polyester film is covered on the surface of the green ceramic sheet to be punched; and the laser beam passes through the polyester film and acts on the surface of the green ceramic sheet to be punched.
9. A raw porcelain sheet, It is characterized in that The green porcelain sheet is prepared by the method according to any one of claims 1 to 8; The raw porcelain sheet is provided with a target hole penetrating the raw porcelain sheet; the thickness of the raw porcelain sheet in a first direction is greater than 1 mm; and / or the shape of the target hole includes a straight line segment; and the first direction is perpendicular to the surface of the raw porcelain sheet.
10. The green ceramic sheet according to claim 9, It is characterized in that The target holes include: a first target hole located in a first area of the green ceramic sheet, and a second target hole located in a second area of the green ceramic sheet; Wherein, the shape of the second target hole includes a straight line segment.
Citation Information
Patent Citations
Ceramic substrate porous array picosecond laser galvanometer scanning drilling system and method
CN111590197A
Method suitable for laser processing of through hole of green ceramic chip
CN114682932A
Ceramic material high-quality laser drilling method based on sandwich structure
CN118543996A
Method for manufacturing multilayer ceramic electronic component
JP2010177508A
Laser drilling method for green ceramic sheet
WO2024021199A1
Cited By
Method for improving cracks in fiber laser ceramic cutting process
CN121156540A
Method for rapidly processing micropore array optical elements with inclined channels on multiple transparent glass substrates in batches
CN121514729A