Method for improving glossiness and ink color fastness of printed color film and application
By adopting three-layer composite structure and surface modification treatment on the BOPP film, combined with water-based ink printing, the problem of poor surface performance of BOPP film is solved, and the gloss and ink color fastness of the printed color film is significantly improved. It is suitable for high-end cigarettes Package.
Patent Information
- Application Number
- CN202411110872.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-14
AI Technical Summary
BOPP film has poor surface hydrophilicity, adhesion and dyeability in printing color film applications, which are prone to oxidation and degradation, resulting in poor gloss and haze performance, which limits its application in the field of tobacco packaging.
Three-layer composite BOPP film is adopted, the surface layer, core layer and inner layer contain hydrogenated petroleum resin, and low-temperature plasma surface activation and corona treatment are carried out, and the surface modification coating is prepared by combining aqueous silane coupling agent and solid acid to improve the surface. Modification properties, printed using water-based color ink.
It significantly improves the gloss and ink fastness of the printed color film, maintains transparency and wear resistance, and has good performance after a year of natural aging. It is suitable for tobacco packaging films.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tobacco, and particularly relates to a method and application for improving the glossiness and oil black fastness of a printed color film. Background Art
[0002] The cigarette packaging film is generally BOPP film. BOPP film undergoes biaxial stretching during the production process, so BOPP film has high tensile strength and high impact strength. It has excellent rigidity, toughness and transparency, outstanding tensile strength and impact strength, high stiffness and high transparency. BOPP film is colorless, odorless, tasteless and non-toxic, and is a commonly used packaging material in the tobacco industry.
[0003] Due to the characteristics of BOPP film such as light weight, non-toxicity, high mechanical strength, good dimensional stability and good transparency, it is widely used in the packaging of candies, cigarettes, textiles, food, etc. However, some characteristics of BOPP film limit its application: (1). Biaxially oriented polypropylene film is a non-polar polymer with mainly methyl groups exposed on the surface, so its surface free energy is extremely low, resulting in poor surface hydrophilicity, printability, adhesion and dyeability, which greatly limits its scope of application and makes its adhesion and printing and dyeing properties relatively poor; (2) The tertiary carbon atoms and methyl groups in the biaxially oriented polypropylene film molecules carry active H elements, which are prone to oxidative degradation reactions under the action of external oxygen and other conditions, which is not conducive to its long-term storage and use.
[0004] Printed color films are currently widely used for decorative packaging of high-end cigarette products. Gloss and haze are two important indicators of the optical properties of BOPP film. Films with low haze and high gloss will make cigarettes look more upscale and bring bright visual effects to cigarette packages. Compared with traditional unprinted cigarette films, printed color films require large-area printing of multiple colors, and the printing process of printed color films is complicated. If organic solvents are used in printing, they will corrode the macromolecular chains of the printed color film (the cigarette film is generally BOPP); therefore, water-based inks are generally used, and the drying process for printing is about 40°C, which causes a certain degree of loss in the physical indicators of the printed color film, especially the loss of performance indicators such as gloss.
[0005] Water-based inks need to dry quickly and have good resolubility. Generally, quick-drying inks have poor resolubility. Inks with good resolubility have poor water resistance, dry slowly, and cannot be driven at high speeds. Water-based back printing inks require good bonding strength with the composite glue, and must not bubble or debond. The back printing ink layer is in direct contact with the glue and the printing surface cannot be corroded by the glue. The back printing equipment has a high speed and requires high quick drying of the ink, generally more than 180 meters per minute.
[0006] In addition, the gloss and haze of BOPP film tend to deteriorate over time. Therefore, it is necessary to develop a new anti-blocking masterbatch and apply it to BOPP film, while optimizing the film formula and improving the optical properties and stability of the BOPP film.
[0007] The present invention is proposed for this purpose. Summary of the invention
[0008] The invention provides a method for improving the glossiness of a printed color film. The obtained printed color film is used as a tobacco packaging film and has good light transmittance and glossiness and high ink color fastness.
[0009] The technical solution of the present invention is as follows:
[0010] The first aspect of the present invention discloses a method for improving the glossiness and color fastness of a printed color film, wherein the printed color film is a composite BOPP film, and the method comprises the following steps:
[0011] (1) Pre-treating the outer surface and inner surface of the composite BOPP film;
[0012] (2) coating the outer surface and inner surface of the composite BOPP film with a surface modification coating agent and drying at high temperature;
[0013] (3) Printing the outer surface of the composite BOPP film with water-based color ink, and obtaining the printed color film after drying.
[0014] Preferably, the composite BOPP film is a three-layer film, the surface layer is a blended film of copolymer PP, silicon dioxide, phenyl-modified silicone and hydrogenated petroleum resin; the core layer is a blended film of homopolymer PP, antistatic agent and hydrogenated petroleum resin; the inner layer is a blended film of copolymer PP, phenyl-modified silicone and hydrogenated petroleum resin.
[0015] Preferably, the silicon dioxide content in the surface layer is not higher than 0.08wt%, the phenyl modified silicone content is 0.05-0.10wt%, and the hydrogenated petroleum resin content is 3.0-5.0wt%; the antistatic agent in the core layer is a mixture of alkyl diethanolamine and monoglyceride, the antistatic agent content is 0.35%-0.45wt%, and the hydrogenated petroleum resin content is 10.0-15.0wt%; the phenyl modified silicone content in the inner layer is 0.10-0.20wt%, and the hydrogenated petroleum resin content is 1.0-2.0wt%.
[0016] Preferably, in step (1), the outer surface of the composite BOPP film is pretreated by low-temperature plasma surface activation treatment, and the gas used is CO2; the inner surface of the composite BOPP film is treated by corona treatment, and the voltage of the corona treatment is 10 to 20 kV and the frequency is 2 to 5 kHz.
[0017] Preferably, the surface modification coating composition of step (2) comprises: water-based silane coupling agent, tetraethyl orthosilicate, solid acid and water, and the mass ratio thereof is (5-10):(50-100):(5-10):(300-400).
[0018] Preferably, the water-based silane coupling agent is one of methyltrichlorosilane (MTS) or aminosilane; and the solid acid is ethylenediaminetetraacetic acid.
[0019] Preferably, the preparation of the surface modification coating comprises the following steps: adding a water-based silane coupling agent and a solid acid into water to dissolve them, then adding tetraethyl orthosilicate dropwise under high-speed stirring, and obtaining the surface modification coating after the reaction is completed.
[0020] Preferably, the surface modification coating in step (2) is applied by spraying; the drying temperature is 80-100°C.
[0021] Preferably, the drying temperature after printing in step (3) is 40-50°C.
[0022] The second aspect of the present invention discloses the use of the high-printing color film obtained by the method as a tobacco packaging film to improve the glossiness and ink color fastness of the printed color film.
[0023] Beneficial effects of the present invention:
[0024] 1. The method of the present invention can improve the glossiness of the printed color film, while the haze and transparency are not affected or slightly improved, and the ink color fastness is high. It is used for tobacco packaging film and has good machine suitability. Note: Haze refers to the ratio of the scattered light flux that deviates from the direction of the incident light through the sample to the transmitted light flux, expressed as a percentage. Glossiness wearable capability refers to the ability of the surface of the film to withstand damage under the action of external friction; it is generally expressed by the change in haze value, that is, the difference between the haze value of the film after it has been rubbed with a certain pressure, speed and number of times and the original haze value before friction; the smaller the difference, the better the glossiness and the higher the ink color fastness, and vice versa.
[0025] 2. The method for improving the glossiness of printed color film of the present invention adopts a three-layer composite BOPP film; the surface layer, core layer and inner layer all contain hydrogenated petroleum resin. The refractive index of hydrogenated petroleum resin is about 1.51, which is very close to the refractive index of BOPP (about 1.49). Both are non-polar materials with similar structures and good compatibility; hydrogenated petroleum resin is an amorphous oligomer, and PP is a semi-crystalline polymer. The addition of hydrogenated petroleum resin expands the amorphous area of the mixed material, significantly changes the aggregate structure of the PP polymer chain, partially dissolves the crystal structure of PP, reduces the melting point of PP (from 161-162°C to 140-150°C), and refines the crystalline particles of PP, thereby improving the transparency of PP and keeping the haze unchanged or reduced. In addition, the surface layer and the inner layer also contain phenyl-modified silicone, wherein the kinematic viscosity of the phenyl-modified silicone is 100-280mm 2 / s, which has a refractive index closer to that of PP, which improves the glossiness of the BOPP film surface and makes it more transparent.
[0026] 3. In order to improve the bonding performance between the surface modification coating and the surface of the composite BOPP film, the method of the present invention performs low-temperature plasma surface activation treatment on the outer surface of the composite BOPP film, and the gas used is CO2; the inner surface of the composite BOPP film is subjected to corona treatment, and the voltage of the corona treatment is 2 to 100 kV and the frequency is 2 to 10 kHz. Since the surface layer of the composite BOPP film of the present invention is a blended film of copolymerized PP, silicon dioxide, phenyl-modified silicone and hydrogenated petroleum resin, after the CO2 low-temperature plasma surface activation treatment, the surface modification coating has a greater bonding ability with it, and after printing with water-based color ink, the color film has a higher glossiness and improved wear resistance. The inner layer is a blended film of copolymerized PP, hydrogenated petroleum resin and phenyl modified silicone. After corona treatment with a voltage of 10-20kV and a frequency of 2-5kHz, the surface modification coating has a good ability to bind to it, and the coating formed later has a high peeling strength and will not have a "grinding" phenomenon; at the same time, because many active points will be formed on the surface after corona treatment, these active points are tightly combined with the surface modification coating, and the entire BOPP surface is almost gapless, so the gas barrier property is improved. Through the analysis of the CO2 low-temperature plasma surface activation treatment of the composite BOPP film, polar groups such as -COOH and -OH were successfully introduced on the outer surface of the composite BOPP film, which significantly improved the surface free energy and improved the interface bonding ability between the outer surface of the composite BOPP film and the surface modification coating; the glossiness of the outer surface of the composite BOPP film can be significantly improved.
[0027] 4. The surface modification coating of the present invention first dissolves the water-based silane coupling agent and the solid acid in water, and then adds ethyl orthosilicate dropwise under high-speed stirring (the speed is generally 1000-5000 rpm) to prepare a surface modification coating with good transparency and glossiness for the first time. According to analysis, the particles in the surface modification coating are about 30 nm and the particle size is uniform.
[0028] 5. After the outer surface of the composite BOPP film of the present invention is treated with CO2 low-temperature plasma surface activation and then coated with a surface modification coating, the outer surface of the composite BOPP film is printed with water-based color ink, and the wear quality is small and the glossiness is improved. This is because the polar groups such as -COOH and -OH generated on the outer surface after the CO2 low-temperature plasma surface activation treatment have good hydrophilicity, so that they have good bonding performance with the surface modification coating, and the coating is uniform; the printed color film obtained by printing the outer surface of the composite BOPP film with water-based color ink is firmly bonded to the surface modification coating, and the ink color fastness is high.
[0029] 6. The composite BOPP film prepared by the preparation method of the present invention still has good gloss performance and ink color fastness after natural aging for one year. DETAILED DESCRIPTION
[0030] The following is described in conjunction with the embodiments, and it should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention. Other advantages, objectives and features of the present invention will be described in the subsequent embodiments, and to some extent are obvious to those skilled in the art, or those skilled in the art can be taught from the practice of the present invention.
[0031] In order to improve the glossiness of BOPP printed color film without losing its wear resistance, the present invention provides a method for improving the glossiness of printed color film, and the glossiness of the high-quality printed color film used for tobacco packaging film can be improved without losing its light transmittance and wear resistance.
[0032] The method for improving the glossiness of a printed color film of the present invention comprises the following steps: (1) pre-treating the outer surface and the inner surface of the composite BOPP film; the composite BOPP film is a three-layer film, the surface layer is a blended film of copolymerized PP, silicon dioxide, phenyl-modified silicone and hydrogenated petroleum resin, the silicon dioxide content in the surface layer is not higher than 0.08wt%, the phenyl-modified silicone content is 0.05-0.10wt%, and the hydrogenated petroleum resin content is 3-5wt%; the core layer is a blended film of homopolymerized PP and silicon dioxide, phenyl-modified silicone and hydrogenated petroleum resin; The invention discloses a blended film of an antistatic agent and a hydrogenated petroleum resin, wherein the antistatic agent in the core layer is a mixture of alkyl diethanolamine and monoglyceride, the content of the antistatic agent is 0.35%-0.45wt%, and the content of the hydrogenated petroleum resin is 10-15wt%; the inner layer is a blended film of copolymerized PP, phenyl modified silicone and hydrogenated petroleum resin, the content of the phenyl modified silicone in the inner layer is 0.10-0.20wt%, and the content of the hydrogenated petroleum resin is 1-2wt%; the outer surface of the composite BOPP film is pretreated by using a low temperature plasma surface active (1) treating the inner surface of the composite BOPP film with a corona treatment, wherein the voltage of the corona treatment is 10-20 kV and the frequency is 2-5 kHz; (2) coating the outer surface and the inner surface of the composite BOPP film with a surface modification coating, wherein the coating is sprayed and dried at 80-100° C.; the surface modification coating comprises: a water-based silane coupling agent, tetraethyl orthosilicate, a solid acid and water, wherein the mass ratio is (5-10): (50-100): (5-10): (3 00-400); the silane coupling agent is one of methyltrichlorosilane (MTS) and aminosilane; the solid acid is ethylenediaminetetraacetic acid; the preparation of the surface modification coating comprises the following steps: adding the water-based silane coupling agent and the solid acid into water to dissolve, then adding tetraethyl orthosilicate dropwise under high-speed stirring, and obtaining the surface modification coating after the reaction is completed; (3) using water-based color ink to print the outer surface of the composite BOPP film, and obtaining the printed color film after drying; the drying temperature after printing is 40-50°C.
[0033] Embodiment 1: Method for improving the glossiness of printed color film (shrink film).
[0034] The composite BOPP film has three layers: the surface layer is a blended film of copolymer PP, 0.05wt% silicon dioxide, 0.05wt% phenyl modified silicone and 4.0wt% hydrogenated petroleum resin; the core layer is a blended film of homopolymer PP, 0.40wt% antistatic agent (the mass ratio of alkyl diethanolamine and monoglyceride is 1:0.3) and 10.0wt% hydrogenated petroleum resin; the inner layer is a blended film of copolymer PP, 0.15wt% phenyl modified silicone and 1.5wt% hydrogenated petroleum resin;
[0035] The composition and preparation method of the modified coating: water-based silane coupling agent (aminosilane), tetraethyl orthosilicate, solid acid (ethylenediaminetetraacetic acid) and water, the mass ratio of which is 5:100:10:300. 5g of aminosilane and 10g of ethylenediaminetetraacetic acid are added to 300g (ml) of water to mix and dissolve, and 100g of tetraethyl orthosilicate is dripped dropwise at 3000rmp, and stirred for 10 minutes after the dripping is completed; a transparent and slightly viscous surface modified coating is obtained;
[0036] The outer surface of the composite BOPP film is pretreated by using CO2 low-temperature plasma surface activation treatment; then the surface modification coating is sprayed on the outer surface of the composite BOPP film, and after drying at 90° C., the outer surface of the composite BOPP film is printed with water-based color ink (commonly used in the market), and after drying at 50° C., the printed color film is obtained;
[0037] At the same time, the inner surface of the composite BOPP film was treated with 50 kV and 10 kHz corona treatment, and then the surface modification coating was sprayed on the outer surface of the composite BOPP film and dried at 90°C;
[0038] The glossiness and light transmittance of the printed color film were tested, and the printed color film was tested after natural aging for one year. The results are shown in Table 1 below:
[0039] The haze test shall be carried out in accordance with the provisions of GB / T2410 Transparent Plastics Transmittance and Haze Test Method.
[0040] The glossiness is tested in accordance with the provisions of GB / T8807 Plastic Mirror Gloss Test Method, with an incident angle of 45°. During the test, the plane formed by the incident and reflected light of the glossiness tester test window should be parallel to the longitudinal direction of the smoke film, the backing plate should be black and the glossiness should not exceed 0.2%.
[0041] Table 1 Test results of printed color film obtained in Example 1
[0042] Indicator name unit Industry average Standard requirements Example 1 After one year of natural aging Haze % 1.63 ≤1.5 1.35 1.34 Glossiness % 86.9 ≥88 91.2 91.2
[0043] As can be seen from Table 1, the glossiness of the composite BOPP film of the present invention is much higher than the industry average, and the haze is much lower than the industry average. After aging for one year, the glossiness and haze are almost unchanged. This fully demonstrates that the composite BOPP film obtained by the preparation method of the present invention has significantly improved glossiness and ink color fastness, and has good aging resistance.
[0044] Machine suitability: The cigarette film samples undergoing machine suitability test should be stored for 24 hours under environmental conditions of temperature 22.0-27.0℃ and relative humidity 60%±5% before being tested on the machine. During the process, the normal operation of the packaging machine will not be affected by cigarette film quality defects, the effective operation rate of the equipment will be improved, and there will be no defects such as loose packs and wrinkles that affect the quality of cigarette strips, boxes and packaging.
[0045] Embodiment 2: Method for improving the glossiness of printed color film (shrink film).
[0046] The composite BOPP film has three layers: the surface layer is a blended film of copolymer PP, 0.05wt% silicon dioxide, 0.05wt% phenyl modified silicone and 4.0wt% hydrogenated petroleum resin; the core layer is a blended film of homopolymer PP, 0.40wt% antistatic agent (the mass ratio of alkyl diethanolamine and monoglyceride is 1:0.3) and 10.0wt% hydrogenated petroleum resin; the inner layer is a blended film of copolymer PP, 0.15wt% phenyl modified silicone and 1.5wt% hydrogenated petroleum resin;
[0047] The composition and preparation method of the modified coating: water-based silane coupling agent (aminosilane), tetraethyl orthosilicate, solid acid (ethylenediaminetetraacetic acid) and water, the mass ratio of which is 5:50:5:300. Add 5g of aminosilane and 5g of ethylenediaminetetraacetic acid into 300g (ml) of water to mix and dissolve, and drip 50g of tetraethyl orthosilicate drop by drop at 3000rmp, and stir for 10min after dripping; thus, a transparent and slightly viscous surface modified coating is obtained;
[0048] The outer surface of the composite BOPP film is pretreated by using CO2 low-temperature plasma surface activation treatment; then the surface modification coating is sprayed on the outer surface of the composite BOPP film, and after drying at 90° C., the outer surface of the composite BOPP film is printed with water-based color ink (commonly used in the market), and after drying at 50° C., the printed color film is obtained;
[0049] At the same time, the inner surface of the composite BOPP film was treated with 50 kV and 10 kHz corona treatment, and then the surface modification coating was sprayed on the outer surface of the composite BOPP film and dried at 90°C;
[0050] Similar to Example 1, the glossiness and light transmittance of the printed color film were tested. The results are shown in Table 2 below:
[0051] Table 2 Test results of printed color film obtained in Example 2
[0052] Indicator name unit Industry average Standard requirements Example 2 After one year of natural aging Haze % 1.63 ≤1.5 1.29 1.28 Glossiness % 86.9 ≥88 91.5 91.3
[0053] The suitability for the machine is the same as that in Example 1.
[0054] Embodiment 3: Method for improving the glossiness of printed color film (micro-shrinkage film).
[0055] The composite BOPP film has three layers: the surface layer is a blended film of copolymer PP, 0.05wt% silicon dioxide, 0.05wt% phenyl modified silicone and 4.0wt% hydrogenated petroleum resin; the core layer is a blended film of homopolymer PP, 0.40wt% antistatic agent (the mass ratio of alkyl diethanolamine and monoglyceride is 1:0.3) and 10.0wt% hydrogenated petroleum resin; the inner layer is a blended film of copolymer PP, 0.15wt% phenyl modified silicone and 1.5wt% hydrogenated petroleum resin;
[0056] The composition and preparation method of the modified coating: water-based silane coupling agent (aminosilane), tetraethyl orthosilicate, solid acid (ethylenediaminetetraacetic acid) and water, the mass ratio of which is 10:50:10:400. Add 10g of aminosilane and 10g of ethylenediaminetetraacetic acid into 400g (ml) of water to mix and dissolve, and drip 50g of tetraethyl orthosilicate drop by drop at 3000rmp, and stir for 10min after dripping; a transparent and slightly viscous surface modified coating is obtained;
[0057] The outer surface of the composite BOPP film is pretreated by using CO2 low-temperature plasma surface activation treatment; then the surface modification coating is sprayed on the outer surface of the composite BOPP film, and after drying at 90° C., the outer surface of the composite BOPP film is printed with water-based color ink (commonly used in the market), and after drying at 50° C., the printed color film is obtained;
[0058] At the same time, the inner surface of the composite BOPP film was treated with 50 kV and 10 kHz corona treatment, and then the surface modification coating was sprayed on the outer surface of the composite BOPP film and dried at 90°C;
[0059] As in Example 1, the glossiness and light transmittance of the printed color film were tested, and the results are shown in Table 3 below:
[0060] Table 3 Test results of printed color film obtained in Example 3
[0061] Indicator name unit Industry average Standard requirements Example 3 After one year of natural aging Haze % 1.60 ≤1.5 1.30 1.29 Glossiness % 87.1 ≥88 91.5 91.4
[0062] The suitability for the machine is the same as that of Example 1.
[0063] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for improving the glossiness and color fastness of printed color films, characterized in that: The printed color film is a composite BOPP film, and the method comprises the following steps: (1) Pre-treating the outer and inner surfaces of the composite BOPP film; (2) coating the outer surface and inner surface of the composite BOPP film with a surface modification coating and drying at high temperature; (3) Printing the outer surface of the composite BOPP film with water-based color ink, and obtaining the printed color film after drying.
2. The method according to claim 1, characterized in that The composite BOPP film is a three-layer film, the surface layer is a blended film of copolymer PP, silicon dioxide, phenyl-modified silicone and hydrogenated petroleum resin; the core layer is a blended film of homopolymer PP, antistatic agent and hydrogenated petroleum resin; The inner layer is a blended film of copolymer PP, phenyl modified silicone and hydrogenated petroleum resin.
3. The method according to claim 2, characterized in that The silicon dioxide content in the surface layer is not higher than 0.08wt%, the phenyl modified silicone content is 0.05-0.10wt%, and the hydrogenated petroleum resin content is 3.0-5.0wt%; the antistatic agent in the core layer is a mixture of alkyl diethanolamine and monoglyceride, the antistatic agent content is 0.35%-0.45wt%, and the hydrogenated petroleum resin content is 10.0-15.0wt%; the phenyl modified silicone content in the inner layer is 0.10-0.20wt%, and the hydrogenated petroleum resin content is 1.0-2.0wt%.
4. The method according to claim 1, characterized in that: In step (1), the outer surface of the composite BOPP film is pretreated by low-temperature plasma surface activation treatment, and the gas used is CO2; the inner surface of the composite BOPP film is treated by corona treatment, and the voltage of the corona treatment is 10 to 20 kV and the frequency is 2 to 5 kHz.
5. The method according to claim 1, characterized in that The surface modification coating composition of step (2) includes: water-based silane coupling agent, tetraethyl orthosilicate, solid acid and water, and the mass ratio thereof is (5-10):(50-100):(5-10):(300-400).
6. The method according to claim 5, characterized in that The water-based silane coupling agent is one of methyltrichlorosilane (MTS) and aminosilane; and the solid acid is ethylenediaminetetraacetic acid.
7. The method according to claim 5, characterized in that The preparation of the surface modification coating comprises the following steps: adding a water-based silane coupling agent and a solid acid into water to dissolve them, then adding ethyl orthosilicate dropwise under high-speed stirring, and obtaining the surface modification coating after the reaction is completed.
8. The method according to claim 1, characterized in that The surface modification coating in step (2) is applied by spraying; the drying temperature is 80-100°C.
9. The method according to claim 1, characterized in that: The drying temperature after printing in step (3) is 40-50°C.
10. Use of the high-printing color film obtained by the method according to any one of claims 1 to 9 as a tobacco packaging film to improve the glossiness and ink color fastness of the printed color film.
Citation Information
Patent Citations
Multifunctional BOPP (Biaxially-oriented Polypropylene) cigarette packaging film and manufacture method thereof
CN102085735A
Stamping stay wire with embossed sense and production method of stamping stay wire
CN109398942A
Biaxially oriented polypropylene film with temperature change effect and preparation method thereof
CN111548565A
BOPP (Biaxially-oriented Polypropylene) film and preparation process thereof
CN116461180A
Electroless plating pretreatment composition for forming film
JP2013053329A
Cited By
Recoverable easy-to-rinse low-density label and recovery method thereof
CN119724022A
Recyclable easy-to-rinse low-density label and recycling method thereof
CN119724022B