Graphene composite kaolin powder as well as preparation method and application thereof

Through the composite preparation of graphene and kaolin, the problem of low mechanical strength of traditional thermally conductive ceramic materials is solved, and graphene composite kaolin powder with high thermal conductivity and high mechanical properties is achieved, which is suitable for areas with high efficiency thermal management and mechanical strength requirements.

CN118993696AActive Publication Date: 2024-11-22HUAQIAO UNIVERSITY

Patent Information

Application Number
CN202411128045.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

While traditional thermally conductive ceramic materials have high thermal conductivity, they also have problems such as high density, low mechanical strength and easy to break, making it difficult to meet the needs of efficient thermal management and mechanical properties.

Method used

The thermally conductive ceramic materials are prepared by composite graphene and kaolin. Through ultrasonic dispersion, modification of aminosilane coupling agent, high-temperature sintering and other steps, graphene composite kaolin powder with excellent thermal conductivity and mechanical properties is formed.

Benefits of technology

The thermal diffusion coefficient and thermal conductivity of the material are significantly improved, the mechanical properties are enhanced, and efficient thermal management and mechanical properties are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993696A_ABST
    Figure CN118993696A_ABST
Patent Text Reader

Abstract

The invention discloses graphene composite kaolin powder and a preparation method and application thereof.According to the preparation method, firstly, the surface of kaolin powder is subjected to graft modification through an amino silane coupling agent, so that the kaolin powder and graphene oxide have opposite electrical properties within a certain pH range, when the pH ranges from 2 to 3, the kaolin powder and the graphene oxide can be effectively self-assembled, and the graphene composite kaolin powder is prepared; the problems that two materials with negative electricity, namely graphene and kaolin powder, are difficult to uniformly mix and graphene is easy to agglomerate in a ceramic collective sintered by the kaolin powder are solved, so that the graphene composite kaolin heat-conducting ceramic material is relatively compact in microstructure and low in porosity, the graphene constructs a rapid heat conduction path in the ceramic, and the heat conduction efficiency is improved. And the thermal diffusion coefficient and the thermal conductivity of the composite material are increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal conductive ceramics, and in particular relates to a graphene composite kaolin powder and a preparation method and application thereof. Background Art

[0002] Thermally conductive ceramic material is a ceramic material with good thermal conductivity, which is widely used in the fields of electronic component radiators, high-voltage cable insulation layers, etc. At present, the commonly used thermally conductive ceramic materials are mostly aluminum oxide, silicon nitride, etc. Traditional thermally conductive ceramic materials have high density, low mechanical strength, and easy breakage while having high thermal conductivity. Therefore, it is of great significance to find a new type of thermally conductive ceramic material with high thermal conductivity and high mechanical strength. Graphene is a new type of carbon material with excellent thermal conductivity and mechanical properties, which can be used to prepare thermally conductive ceramic materials. Kaolin is a common ceramic raw material with good high temperature resistance and structural stability. The composite preparation of graphene and kaolin for preparing thermally conductive ceramic materials can give full play to the advantages of both and improve the thermal conductivity and mechanical properties of the material. For example, CN112707736A provides a method for preparing a graphene-modified ceramic composite material, wherein a pressure casting machine is used for a ceramic powder and a graphene nanosheet dispersion liquid, so that the graphene nanosheet dispersion liquid enters the cavity of the pressure casting machine and can be evenly mixed with the ceramic powder, and the formed composite material has excellent fracture toughness and good thermal conductivity. Multiphase thermal storage ceramics usually have good thermal shock resistance, high fracture toughness and strength, low thermal resistance, high thermal storage density and good high-temperature thermal performance. Therefore, the development of new high-temperature, high-efficiency and low-cost thermal storage ceramic materials is of great significance for improving the efficiency of thermal power generation technology and thermal utilization technology. Kaolin is an important solid thermal storage material. The main chemical components are SiO2 and Al2O3. Most kaolin also contains MgO and Fe2O3. The high content of Fe2O3 will promote the formation of liquid phase and make the sample dense. Since the high packing density corresponds to the high thermal storage density, this also provides a new idea for using kaolin to prepare solar thermal storage materials.

[0003] Compared with traditional ceramics, the advantages of graphene composite kaolin thermal conductive ceramic materials include improved thermal conductivity, thermal management efficiency, and potential excellent mechanical properties. Composite ceramic materials are widely used in electronics, aerospace, and automotive fields, especially in occasions that require efficient thermal management. Summary of the invention

[0004] The purpose of the present invention is to provide a graphene composite kaolin powder and a preparation method and application thereof. The graphene composite kaolin powder can be used to sinter a graphene composite kaolin thermal conductive ceramic material with good thermal conductivity and mechanical strength, and has broad application prospects.

[0005] The technical solution of the present invention is as follows:

[0006] A method for preparing graphene composite kaolin powder comprises the following steps:

[0007] (1) dispersing kaolin powder in an ethanol solution by ultrasonication, then adding an aminosilane coupling agent, mixing thoroughly and reacting, then washing to remove the residual aminosilane coupling agent, and drying to obtain a surface-modified kaolin powder, wherein the reaction temperature is 73-83° C., and the reaction time is 19-29 h;

[0008] The mass volume ratio of the kaolin powder and the aminosilane coupling agent is 1-1.5 g: 10-15 mL; the reaction time after mixing is 24 h ± 5

[0009] (2) dispersing the surface-modified kaolin powder in deionized water and adjusting the pH to 2-3 to obtain a kaolin dispersion;

[0010] (3) dispersing the graphene oxide aerogel in deionized water, adjusting the pH to 2-3, then adding the above-mentioned kaolin dispersion, mixing thoroughly and standing until the system is stratified, then taking the lower layer slurry and centrifuging and washing it to weak acidity, and finally drying to obtain the graphene oxide composite kaolin powder;

[0011] Wherein, the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel in the kaolin dispersion is 100:2.5-10;

[0012] (4) Using hydrazine hydrate as a reducing agent to reduce the above-mentioned graphene oxide composite kaolin powder to obtain graphene composite kaolin powder.

[0013] In some possible implementations, the preparation method of graphene oxide aerogel is: slowly pour concentrated sulfuric acid into graphite powder, then stir in an ice water bath to fully mix the graphite powder and concentrated sulfuric acid, slowly add potassium permanganate powder after the system temperature drops below 10°C, continue stirring and react at 45°C for 2h, slowly add distilled water to the system after the reaction is completed and control the system temperature not to exceed 100°C, then cool to room temperature, then add hydrogen peroxide dropwise until the system turns golden yellow, seal and stand until the system is separated, then take the lower layer of precipitate and wash it to neutrality, and then freeze-dry it to obtain graphene oxide aerogel;

[0014] The mass volume ratio of graphite powder, concentrated sulfuric acid and distilled water is 1 g:50 mL:75 mL, the mass ratio of graphite powder to potassium permanganate powder is 1:6, and the mass fraction of hydrogen peroxide is 30 wt%.

[0015] In the above steps, the main function of sealing is to prevent pollution, maintain the reaction conditions such as temperature and humidity of the system, prevent splashing, reduce the release of harmful gases and facilitate subsequent processing. Exemplarily, the mouth of the reaction container can be covered with plastic wrap and sealed.

[0016] In some possible implementations, the specific operation of step (4) is: dispersing graphene oxide composite kaolin powder in deionized water, adding hydrazine hydrate, and then reacting at 90-95° C. for 80-100 hours to obtain a black precipitate, washing and drying the black precipitate to obtain graphene composite kaolin powder;

[0017] The mass volume ratio of graphene oxide composite kaolin powder to hydrazine hydrate is 0.5 g:5 mL.

[0018] In some possible implementations, the size of the kaolin powder is 200 mesh, and the size of the graphite powder is 8000 mesh.

[0019] In some possible implementations, the aminosilane coupling agent is 3-aminopropylmethyldiethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethylsilane or aminoethylaminopropyltrimethoxysilane.

[0020] A graphene composite kaolin powder is prepared by the above preparation method.

[0021] A graphene composite kaolin thermal conductive ceramic material is obtained by shaping and sintering the graphene composite kaolin powder.

[0022] In some possible implementations, the sintering temperature is 1080-1400° C., and the sintering time is 180 min.

[0023] In some possible implementations, the sintering is performed under nitrogen or argon protection.

[0024] An application of the above graphene composite kaolin powder in the preparation of graphene composite kaolin thermal conductive ceramic material.

[0025] The present invention has at least the following beneficial effects:

[0026] 1. The present invention firstly grafts and modifies the surface of kaolin powder by using an aminosilane coupling agent, so that it has opposite electrical properties to graphene oxide within a certain pH range. When the pH is 2-3, the two can effectively self-assemble, thus overcoming the problem that graphene and kaolin powder, two negatively charged materials, are difficult to mix evenly and graphene is easy to agglomerate in the ceramic aggregate sintered by kaolin powder;

[0027] 2. In some possible implementations, the present application adopts the Hummers method to prepare graphene oxide aerogel, which is mixed with surface-modified kaolin powder and then subjected to a hydrazine hydrate reduction reaction to obtain graphene composite kaolin powder, which is then sintered at high temperature to obtain graphene composite kaolin thermal conductive ceramic material. The entire production process is safe, efficient, and easy to mass produce.

[0028] 3. The graphene composite kaolin thermal conductive ceramic material prepared by the present invention has a relatively dense microstructure and low porosity. Graphene constructs a fast heat conduction path inside the ceramic, thereby increasing the thermal diffusion coefficient and thermal conductivity of the ceramic material.

[0029] 4. Compared with pure phase kaolin ceramics, the graphene composite kaolin thermal conductive ceramic material prepared by the present invention has better mechanical properties; at the optimal addition amount, the thermal diffusion coefficient increases by 2.8 times and the thermal conductivity increases by 6 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The process diagram for preparing the graphene composite kaolin thermal conductive ceramic material of Example 1-12;

[0031] Figure 2 is the TG-DSC curve diagram of Example 1;

[0032] Figure 3 The figures are scanning electron microscope images of the graphene composite kaolin thermal conductive ceramic materials obtained in Examples 1-4; wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Example 4;

[0033] Figure 4 This is the XRD diffraction pattern of the graphene composite kaolin thermal conductive ceramic material prepared in Example 5-8. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further illustrated and described below through specific implementation methods.

[0035] In the following examples, the water used can be one or more of distilled water, purified water, and drinking water; unless otherwise specified, the detection methods in the following examples are conventional detection methods; the reagents in the following examples are purchased from commercial channels unless otherwise specified.

[0036] Example 1

[0037] (1) Dispersing 200 mesh kaolin powder in 200 mL ethanol by 200 W ultrasound for 1 hour to separate flakes, then adding kaolin powder with a mass ratio of 1:1 to 1:1 ultrasonic dispersion in ethanol solution, then adding 3-aminopropylmethyldiethoxysilane, stirring at 500 rpm for 10 minutes to fully mix, and then continuously stirring and condensing and reflux at 78 ° C for 24 hours. After the reaction is completed, the product is washed with deionized water and ethanol alternately centrifuged 3 to 5 times to remove excess 3-aminopropylmethyldiethoxysilane, and then dried at 60 ° C for 6 hours to obtain surface-modified kaolin powder;

[0038] (2) dispersing the surface-modified kaolin powder in deionized water and adjusting the pH to 2-3 to obtain a kaolin dispersion;

[0039] (3) Weigh 1 g of 8000 mesh graphite powder, slowly pour 50 mL of concentrated sulfuric acid into it, and then perform magnetic stirring in an ice water bath to fully mix the graphite powder and concentrated sulfuric acid. After the system temperature drops below 10°C, slowly add 6 g of potassium permanganate powder, continue stirring and react at 45°C for 2 h. After the reaction is completed, slowly add 75 mL of distilled water to the system and increase the magnetic stirring speed. During the reaction, the system temperature is controlled not to exceed 100°C, then cool to room temperature, and then add 30 wt% hydrogen peroxide until the system turns golden yellow. Seal with plastic wrap and let stand for 24 h, then remove the lower precipitate and wash it with deionized water until it is neutral, and then freeze-dry to obtain graphene oxide aerogel;

[0040] (4) Ultrasonic dispersion of graphene oxide aerogel for 2 hours to obtain graphene oxide dispersion. The graphene oxide dispersion is dispersed again in deionized water and the pH is adjusted to 3 with dilute hydrochloric acid, and then added dropwise to the above kaolin dispersion under ultrasonic vibration, ultrasonicated for 2 hours to fully mix, and then allowed to stand until the system is separated into layers, at which time the upper layer is a clear and transparent liquid and the lower layer is a slurry, the lower layer slurry is taken and washed until the pH is weakly acidic, and finally dried to obtain graphene oxide composite kaolin powder;

[0041] Wherein, the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel in the kaolin dispersion is 100:2.5;

[0042] (5) dispersing graphene oxide composite kaolin powder in deionized water, adding hydrazine hydrate after ultrasonic treatment for 2 hours, and then reacting at 90-95° C. for 80-100 hours to obtain a black precipitate, washing and drying the black precipitate to obtain graphene composite kaolin powder;

[0043] The mass volume ratio of graphene oxide composite kaolin powder to hydrazine hydrate is 0.5 g:5 mL.

[0044] (6) The graphene-composite kaolin powder is molded by oil pressure using a mold to obtain a ceramic green body, which is then placed in a tubular sintering furnace for sintering at a temperature of 1087° C. for 180 min to obtain a graphene-composite kaolin thermally conductive ceramic material.

[0045] Thermogravimetric analysis was performed on Example 1, and the results were as follows: Figure 2 As shown, the graphene composite kaolin thermal conductive ceramic material of Example 1 has a sintering weight loss of 20%.

[0046] Example 2

[0047] The difference between Example 2 and Example 1 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:5.

[0048] Example 3

[0049] The difference between Example 3 and Example 1 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:7.5.

[0050] Example 4

[0051] The difference between Example 4 and Example 1 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:10.

[0052] The scanning electron microscope images of the graphene composite kaolin thermal conductive ceramic materials prepared in Examples 1-4 are as follows: Figure 3 As shown, it can be seen that the microstructure of the graphene composite kaolin thermal conductive ceramic material is dense, the porosity is low, and the graphite flakes are evenly distributed in the matrix and wrapped around the grains, indicating that the addition of graphene enhances the microstructure of the sintered body.

[0053] Example 5

[0054] (1) Dispersing 200 mesh kaolin powder in 200 mL ethanol by 200 W ultrasound for 2 h to separate flakes, then adding kaolin powder with a mass ratio of 1:1 to 1:1 ultrasonic dispersion in ethanol solution, then adding 3-aminopropyltriethoxysilane, stirring at 500 rpm for 10 min to fully mix, then continuously stirring and condensing and reflux at 78 ° C for 24 h. After the reaction is completed, the product is washed with deionized water and ethanol alternately centrifuged 3 to 5 times to remove excess 3-aminopropyltriethoxysilane, and then dried at 60 ° C for 6 h to obtain surface-modified kaolin powder;

[0055] (2) dispersing the surface-modified kaolin powder in deionized water and adjusting the pH to 2-3 to obtain a kaolin dispersion;

[0056] (3) Weigh 2 g of 8000 mesh graphite powder, slowly pour 100 mL of concentrated sulfuric acid into it, and then perform magnetic stirring in an ice water bath to fully mix the graphite powder and concentrated sulfuric acid. After the system temperature drops below 10°C, slowly add 12 g of potassium permanganate powder, continue stirring and react at 45°C for 2 h. After the reaction is completed, slowly add 75 mL of distilled water to the system and increase the magnetic stirring speed. During the reaction, the system temperature is controlled not to exceed 100°C, then cool to room temperature, and then add 30 wt% hydrogen peroxide until the system turns golden yellow. Seal with plastic wrap and let stand for 24 h, then remove the lower precipitate and wash it with deionized water until it is neutral, and then freeze-dry to obtain graphene oxide aerogel;

[0057] (4) Ultrasonic dispersion of graphene oxide aerogel for 2 hours to obtain graphene oxide dispersion. The graphene oxide dispersion is dispersed again in deionized water and the pH is adjusted to 3 with dilute hydrochloric acid. It is added dropwise to the above kaolin dispersion under ultrasonic vibration, ultrasonicated for 2 hours to fully mix, and then allowed to stand until the system is separated into layers. At this time, the upper layer is a clear and transparent liquid, and the lower layer is a slurry. The lower layer slurry is taken and washed until the pH is neutral, and finally dried to obtain graphene oxide composite kaolin powder;

[0058] Wherein, the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel in the kaolin dispersion is 100:2.5;

[0059] (5) dispersing graphene oxide composite kaolin powder in deionized water, adding hydrazine hydrate after ultrasonic treatment for 2 hours, and then reacting at 90-95° C. for 80-100 hours to obtain a black precipitate, washing and drying the black precipitate to obtain graphene composite kaolin powder;

[0060] The mass volume ratio of graphene oxide composite kaolin powder to hydrazine hydrate is 0.5 g:5 mL.

[0061] (6) The graphene-composite kaolin powder is molded by oil pressure using a mold to obtain a ceramic green body, which is then placed in a tubular sintering furnace for sintering at a temperature of 1150° C. for 180 min to obtain a graphene-composite kaolin thermally conductive ceramic material.

[0062] Example 6

[0063] The difference between Example 6 and Example 5 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:5.

[0064] Example 7

[0065] The difference between Example 7 and Example 5 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:7.5.

[0066] Example 8

[0067] The difference between Example 8 and Example 5 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:10.

[0068] The XRD diffraction patterns of the graphene composite kaolin thermal conductive ceramic materials prepared in Examples 5-8 are as follows: Figure 4 shown.

[0069] Example 9

[0070] (1) Dispersing 200 mesh kaolin powder in 200 mL ethanol by 200 W ultrasound for 2 h to separate flakes, then adding kaolin powder with a mass ratio of 1:1 to 1:1 ultrasonic dispersion in ethanol solution, then adding 3-aminopropyltriethoxysilane, stirring at 500 rpm for 10 min to fully mix, then continuously stirring and condensing and reflux at 78 ° C for 24 h. After the reaction is completed, the product is washed with deionized water and ethanol alternately centrifuged 3 to 5 times to remove excess 3-aminopropyltriethoxysilane, and then dried at 60 ° C for 6 h to obtain surface-modified kaolin powder;

[0071] (2) dispersing the surface-modified kaolin powder in deionized water and adjusting the pH to 2-3 to obtain a kaolin dispersion;

[0072] (3) Weigh 2 g of 8000 mesh graphite powder, slowly pour 100 mL of concentrated sulfuric acid into it, and then perform magnetic stirring in an ice water bath to fully mix the graphite powder and concentrated sulfuric acid. After the system temperature drops below 10°C, slowly add 12 g of potassium permanganate powder, continue stirring and react at 45°C for 2 h. After the reaction is completed, slowly add 150 mL of distilled water to the system and increase the magnetic stirring speed. During the reaction, the system temperature is controlled not to exceed 100°C, then cool to room temperature, and then add 30 wt% hydrogen peroxide until the system turns golden yellow. Seal with plastic wrap and let stand for 24 h, then remove the lower precipitate and wash it with deionized water until it is neutral, and then freeze-dry to obtain graphene oxide aerogel;

[0073] (4) Ultrasonic dispersion of graphene oxide aerogel for 2 hours to obtain graphene oxide dispersion. The graphene oxide dispersion is dispersed again in deionized water and the pH is adjusted to 3 with dilute hydrochloric acid. It is added dropwise to the above kaolin dispersion under ultrasonic vibration, ultrasonicated for 2 hours to fully mix, and then allowed to stand until the system is separated into layers. At this time, the upper layer is a clear and transparent liquid, and the lower layer is a slurry. The lower layer slurry is taken and washed until the pH is neutral, and finally dried to obtain graphene oxide composite kaolin powder;

[0074] Wherein, the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel in the kaolin dispersion is 100:2.5;

[0075] (5) dispersing graphene oxide composite kaolin powder in deionized water, adding hydrazine hydrate after ultrasonic treatment for 2 hours, and then reacting at 90-95° C. for 80-100 hours to obtain a black precipitate, washing and drying the black precipitate to obtain graphene composite kaolin powder;

[0076] The mass volume ratio of graphene oxide composite kaolin powder to hydrazine hydrate is 0.5 g:5 mL.

[0077] (6) The graphene-composite kaolin powder is molded by oil pressure using a mold to obtain a ceramic green body, which is then placed in a tubular sintering furnace for sintering at a temperature of 1087° C. for 180 min to obtain a graphene-composite kaolin thermally conductive ceramic material.

[0078] Example 10

[0079] The difference between Example 10 and Example 9 is that in step (4), the mass ratio of the surface-modified kaolin powder to the graphene oxide aerogel is 100:5.

[0080] Embodiment 11

[0081] The difference between Example 11 and Example 9 is that in step (4), the mass ratio of the surface-modified kaolin powder to the graphene oxide aerogel is 100:7.5.

[0082] Example 12

[0083] The difference between Example 12 and Example 9 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:10.

[0084] Comparative Example 1

[0085] The difference between Comparative Example 1 and Example 5 is that in step (5), the graphene oxide composite kaolin powder is not reduced using hydrazine hydrate as a reducing agent, but the graphene oxide composite kaolin powder is reduced to graphene composite kaolin powder by high-temperature heat treatment.

[0086] The specific operation of high temperature heat treatment is: placing the graphene oxide composite kaolin powder in a high temperature tube furnace, adjusting the temperature and time, and controlling the heating rate between 5-10℃ / min to avoid thermal shock to the graphene oxide composite kaolin powder. Slowly heat to 1000℃ and then keep warm for 2 hours to ensure that the graphene oxide is effectively reduced. Then slowly cool the system to room temperature to avoid the impact of rapid temperature changes on the sample.

[0087] Comparative Example 2

[0088] The difference between Comparative Example 2 and Comparative Example 1 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:5.

[0089] Comparative Example 3

[0090] The difference between Comparative Example 3 and Comparative Example 1 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:7.5.

[0091] Comparative Example 4

[0092] The difference between Comparative Example 4 and Comparative Example 1 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:10.

[0093] Comparative Example 5

[0094] The difference between Comparative Example 5 and Comparative Example 1 is that the sintering temperature in step (6) is 1400°C.

[0095] Comparative Example 6

[0096] The difference between Comparative Example 6 and Comparative Example 5 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:5.

[0097] Comparative Example 7

[0098] The difference between Comparative Example 7 and Comparative Example 5 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:7.5.

[0099] Comparative Example 8

[0100] The difference between Comparative Example 8 and Comparative Example 5 is that in step (4), the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel is 100:10.

[0101] Comparative Example 9

[0102] The difference between Comparative Example 9 and Example 5 is that the kaolin used is not surface modified (specifications of kaolin: particle size 75±5 μm) and no graphene aerogel is added in step (4), and the sintering temperature in step (6) is 1087°C.

[0103] Comparative Example 10

[0104] The difference between Comparative Example 10 and Comparative Example 9 is that the sintering temperature in step (6) is 1150°C.

[0105] Comparative Example 11

[0106] The difference between Comparative Example 11 and Example 9 is that the surface-modified kaolin powder obtained in step (1) is replaced by unmodified kaolin, and the mass ratio of the unmodified kaolin to the above-mentioned graphene oxide aerogel is 100:2.5.

[0107] Comparative Example 12

[0108] The difference between Comparative Example 11 and Example 9 is that the kaolin used is not surface-modified (specifications of kaolin: particle size 75±5 μm), and the mass ratio of the unmodified kaolin to the above-mentioned graphene oxide aerogel is 100:5.

[0109] Comparative Example 13

[0110] The difference between Comparative Example 13 and Example 9 is that the kaolin used is not surface-modified (specifications of kaolin: particle size 75±5 μm), and the mass ratio of the unmodified kaolin to the above-mentioned graphene oxide aerogel is 100:7.5.

[0111] Comparative Example 14

[0112] The difference between Comparative Example 14 and Example 9 is that the kaolin used is not surface-modified (specifications of kaolin: particle size 75±5 μm), and the mass ratio of the unmodified kaolin to the above-mentioned graphene oxide aerogel is 100:10.

[0113] Performance Testing

[0114] The thermal diffusivity and thermal conductivity in the following performance tests are all tested in the vertical direction.

[0115] (1) The thermal conductivity of Examples 5-12 and Comparative Examples 1-10 was tested at 25° C. The results are shown in Table 1.

[0116] Table 1 Thermal conductivity of Examples 5-12 and Comparative Examples 1-10

[0117]

[0118]

[0119] As can be seen from Table 1, Examples 5-12, by adding graphene aerogel to the raw materials of the ceramic material, have a thermal diffusion coefficient and thermal conductivity that are improved by about 0.5-1 times compared to Comparative Examples 1-8 in which the graphene oxide composite kaolin powder is reduced by high-temperature heat treatment; the thermal diffusion coefficient and thermal conductivity are about twice that of Comparative Examples 11-14 using kaolin without surface modification; and the thermal diffusion coefficient and thermal conductivity are greatly improved compared to Comparative Examples 9 and 10 in which only kaolin without surface modification is used and no graphene aerogel is added.

[0120] (2) The thermal physical properties of the graphene composite kaolin thermal conductive ceramic material prepared in Example 9 (graphene aerogel: surface modified kaolin powder = 2.5wt%, sintering temperature 1087°C) were tested as samples. The results are shown in Table 2

[0121] Table 2 Thermophysical properties of Example 9

[0122] Test temperature / ℃ <![CDATA[Specific heat capacity / (J·g -1 ·K -1 )]]> <![CDATA[Thermal diffusivity / (mm 2 / s)]]> Thermal conductivity / (W / mk) 25 1.85 3.42 13.65 100 1.95 3.02 12.62 200 2.11 2.68 12.11

[0123] It can be seen from Table 2 that as the temperature increases, the specific heat capacity of the graphene composite kaolin thermal conductive ceramic material prepared in Example 9 gradually increases, and the thermal diffusion coefficient and thermal conductivity gradually decrease, but it still maintains good thermal conductivity at 200°C.

[0124] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing graphene composite kaolin powder, characterized in that: The steps include: (1) dispersing kaolin powder in an ethanol solution by ultrasonication, then adding an aminosilane coupling agent, mixing thoroughly and reacting, then washing to remove the residual aminosilane coupling agent, and drying to obtain a surface-modified kaolin powder, wherein the reaction temperature is 73-83° C., and the reaction time is 19-29 h; The mass volume ratio of the kaolin powder and the aminosilane coupling agent is 1-1.5 g: 10-15 mL; the reaction time after mixing is 24 h ± 5 (2) dispersing the surface-modified kaolin powder in deionized water and adjusting the pH to 2-3 to obtain a kaolin dispersion; (3) dispersing the graphene oxide aerogel in deionized water, adjusting the pH to 2-3, then adding the above-mentioned kaolin dispersion, mixing thoroughly and standing until the system is stratified, then taking the lower layer slurry and centrifuging and washing it to weak acidity, and finally drying to obtain the graphene oxide composite kaolin powder; Wherein, the mass ratio of the surface modified kaolin powder to the graphene oxide aerogel in the kaolin dispersion is 100:2.5-10; (4) Using hydrazine hydrate as a reducing agent to reduce the above-mentioned graphene oxide composite kaolin powder to obtain graphene composite kaolin powder.

2. The preparation method according to claim 1, characterized in that The preparation method of the graphene oxide aerogel is as follows: slowly pouring concentrated sulfuric acid into graphite powder, then stirring in an ice water bath to fully mix the graphite powder and the concentrated sulfuric acid, slowly adding potassium permanganate powder after the system temperature drops below 10°C, continuously stirring and reacting at 45°C for 2h, slowly adding distilled water to the system after the reaction is completed and controlling the system temperature not to exceed 100°C, then cooling to room temperature, then dripping hydrogen peroxide until the system turns golden yellow, sealing and standing until the system delaminates, then taking the lower precipitate and washing it to neutrality, and then freeze-drying it to obtain the graphene oxide aerogel; The mass volume ratio of the graphite powder, the concentrated sulfuric acid and the distilled water is 1 g:50 mL:75 mL, the mass ratio of the graphite powder to the potassium permanganate powder is 1:6, and the mass fraction of the hydrogen peroxide is 30 wt%.

3. The preparation method according to claim 1 or 2, characterized in that: The specific operation of step (4) is: dispersing the graphene oxide composite kaolin powder in deionized water, adding hydrazine hydrate, and then reacting at 90-95° C. for 80-100 minutes to obtain a black precipitate, and washing and drying the black precipitate to obtain the graphene composite kaolin powder; The mass volume ratio of the graphene oxide composite kaolin powder to the hydrazine hydrate is 0.5 g:5 mL.

4. The preparation method according to claim 3, characterized in that: The size of the kaolin powder is 200 mesh, and the size of the graphite powder is 8000 mesh.

5. The preparation method according to claim 1, characterized in that: The aminosilane coupling agent is 3-aminopropylmethyldiethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethylsilane or aminoethylaminopropyltrimethoxysilane.

6. A graphene-composite kaolin powder, characterized in that: Prepared by the preparation method described in any one of claims 1 to 5.

7. A graphene composite kaolin thermal conductive ceramic material, characterized in that: The graphene-composite kaolin powder according to claim 6 is formed and sintered to obtain the same.

8. The graphene-composite kaolin thermally conductive ceramic material according to claim 7, characterized in that: The sintering temperature is 1080-1400° C., and the sintering time is 180 min.

9. The graphene-composite kaolin thermally conductive ceramic material according to claim 8, characterized in that: The sintering is performed under the protection of nitrogen or argon.

10. Use of the graphene-composite kaolin powder according to claim 6 in preparing a graphene-composite kaolin thermal conductive ceramic material.

Citation Information

Patent Citations

  • Preparation method of graphene kaolin composite nanometer rubber fillers

    CN103275524A

  • Graphene oxide preparation process

    CN106744928A

  • Graphene coated alumina ceramic powder as well as preparation method and application thereof

    CN107353017A

  • Manufacturing method of graphene-ceramic composites with excellent fracture toughness

    KR1020150075503A

Cited By

  • High-strength high-temperature-resistant ceramic material and preparation method thereof