Proton-type polyion liquid, preparation method thereof and application of proton-type polyion liquid as water-based tackifying and lubricating additive

CN118994474AActive Publication Date: 2024-11-22YANTAI ADVANCED MATERIALS & GREEN MFG SHANDONG PROVINCIAL LAB +1

Patent Information

Application Number
CN202411087918.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

Smart Images

  • Figure BDA0004985692030000021
    Figure BDA0004985692030000021
  • Figure BDA0004985692030000022
    Figure BDA0004985692030000022
  • Figure BDA0004985692030000023
    Figure BDA0004985692030000023
Patent Text Reader

Abstract

The invention provides proton type polyion liquid, a preparation method thereof and application of the proton type polyion liquid as a water-based tackifying and lubricating additive, and belongs to the technical field of lubricants. The cation of the proton type polyion liquid is a copolymer of N-vinyl pyrrolidone and dimethylaminoethyl methacrylate, and the anion of the proton type polyion liquid is an alkyl carboxylate anion or a dibutyl phosphate anion. The active nitrogen element in the molecular structure can generate a friction chemical reaction with a friction pair interface which slides mutually to generate a friction chemical protective film, so that not only can the antifriction and antiwear properties of the water-based lubricating liquid be improved, but also the extreme pressure bearing performance of the water-based lubricating liquid can be improved. Alkyl carboxylate anions or dibutyl phosphate anions can be adsorbed to a metal friction pair interface to form a layer of physical adsorption film, so that the lubricating property of the lubricating liquid is remarkably improved. The proton type polyion liquid aqueous solution has high viscosity, and has good film-forming ability on the surface of a friction pair. The physical adsorption film, the viscous solution film and the friction chemical reaction film have a synergistic effect, so that the antifriction and antiwear properties and the bearing property of the water-based lubricating liquid are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lubricants, and in particular to a proton type polyionic liquid and a preparation method thereof and application thereof as a water-based viscosity increasing lubricating additive. Background Art

[0002] According to statistics, energy consumption caused by friction accounts for about 1 / 2 to 1 / 3 of the total energy consumption in the world. At the same time, about 80% of damaged parts are caused by various forms of wear. Therefore, controlling friction and wear is an important measure to save energy and protect mechanical parts. Compared with oil-based lubricants that are prone to environmental pollution, water-based lubrication technology has attracted widespread attention due to its wide source, flame retardancy, high specific heat capacity and thermal conductivity, green and pollution-free, and good cleaning effect. However, water-based lubricants still have disadvantages, such as poor lubrication performance, low viscosity, poor film-forming and anti-corrosion performance, and the addition of water-based lubricant additives can significantly improve their physical and chemical properties and lubrication performance. Therefore, it is of great significance to develop water-based lubricant additives with high viscosity, good anti-corrosion performance and excellent anti-friction and anti-wear properties.

[0003] Ionic liquids are organic molten salts composed of organic cations and organic or inorganic anions with a melting point below 100°C. They have the advantages of low vapor pressure, high thermal and chemical stability, and flame retardancy. However, when ionic liquids are used as water-based lubricant additives, they cannot significantly increase the viscosity and film-forming properties of water-based lubricants. Polyionic liquids are a type of ionic polymer formed by the polymerization of monomers containing ionic liquid structures as repeating units. Polyionic liquids not only have the excellent lubrication properties of ionic liquids, but also have the high viscosity characteristics of polymers. However, the viscosity of water-based lubricants prepared with polyionic liquids in the prior art is still relatively low, the friction coefficient and wear volume are still relatively high, and the corrosion resistance needs to be further improved. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a proton type polyionic liquid and a preparation method thereof and an application thereof as a water-based thickening lubricating additive. When the proton type polyionic liquid provided by the present invention is used as a water-based lubricating fluid additive, it can significantly increase the kinematic viscosity of the water-based lubricating fluid, reduce the friction coefficient and wear volume of the water-based lubricating fluid, and has excellent corrosion resistance.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a proton type polyionic liquid, comprising cations and anions, wherein the cations are copolymers of N-vinyl pyrrolidone and dimethylaminoethyl methacrylate, and the anions are alkyl carboxylate anions and / or dibutyl phosphate anions;

[0007] The cation has a structure shown in Formula I:

[0008]

[0009] In formula I, m:n=5:1 to 1:5.

[0010] Preferably, the alkyl carboxylate anion has a structure shown in Formula II:

[0011]

[0012] In formula II, x is any integer from 1 to 11.

[0013] Preferably, the alkyl carboxylate anion includes one or more of acetate anion, butyrate anion, caproate anion, octanoate anion and laurate anion.

[0014] Preferably, the dibutyl phosphate anion has a structure shown in Formula III:

[0015]

[0016] The present invention provides a method for preparing the above-mentioned proton type polyionic liquid, comprising the following steps:

[0017] Dimethylaminoethyl methacrylate, anion raw material and solvent are mixed to perform a proton exchange reaction to obtain a proton exchange reaction solution; the anion raw material is an alkyl carboxylic acid and / or dibutyl phosphate;

[0018] The proton exchange reaction liquid, N-vinyl pyrrolidone and an initiator are mixed to carry out a polymerization reaction to obtain a proton type polyionic liquid.

[0019] Preferably, the molar ratio of dimethylaminoethyl methacrylate to anion raw material is 1 to 2:1;

[0020] The molar ratio of N-vinyl pyrrolidone to dimethylaminoethyl methacrylate is 5:1 to 1:5.

[0021] Preferably, the initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate;

[0022] The mass of the initiator is 0.003-1% of the total mass of dimethylaminoethyl methacrylate and anion raw materials.

[0023] Preferably, the polymerization reaction temperature is 50 to 90° C. and the time is 1 to 36 hours.

[0024] The present invention provides the use of the proton type polyionic liquid as a water-based viscosity increasing lubricating additive.

[0025] The present invention provides a water-based lubricant product, comprising a water-based basic lubricating liquid and the above-mentioned proton-type polyionic liquid;

[0026] The water-based lubricating fluid includes one or more of water, a water-ethylene glycol mixture, a water-glycerin mixture, and a water-ethylene glycol-glycerin mixture;

[0027] The mass concentration of the proton type polyionic liquid in the water-based lubricant product is 0.1-40wt%.

[0028] The present invention provides a proton type polyionic liquid, comprising cations and anions, wherein the cations are copolymers of N-vinyl pyrrolidone and dimethylaminoethyl methacrylate, and the anions are alkyl carboxylate anions and / or dibutyl phosphate anions; the cations have a structure shown in Formula I. The present invention uses the copolymer of N-vinyl pyrrolidone and dimethylaminoethyl methacrylate as the cation, wherein the molecule contains a tertiary amine and has a certain alkalinity, and the carboxyl functional group in the alkyl carboxylic acid or the hydroxyl functional group in the molecular structure of dibutyl phosphate has a certain acidity, and the two can be obtained by a simple proton exchange reaction to obtain an ionic monomer [dimethylaminoethyl methacrylate] [alkyl carboxylic acid] or [dimethylaminoethyl methacrylate] [dibutyl phosphate salt], and the ionic monomer is copolymerized with N-vinyl pyrrolidone to obtain a proton type polyionic liquid, and the proton type polyionic liquid has good solubility in a water-based lubricating fluid. The alkyl carboxylate anions or dibutyl phosphate anions can be effectively adsorbed on the interface of the metal friction pair to form a physical adsorption film, which can significantly improve the lubrication performance of the water-based lubricating fluid. In addition, the physical adsorption film can effectively isolate the metal surface from the water-based lubricant, greatly improving the metal's corrosion resistance. At the same time, the proton-type polyionic liquid aqueous solution provided by the present invention has a high viscosity and has good film-forming ability on the friction pair surface.

[0029] In addition, the active nitrogen element in the molecular structure of the polymer of the present invention can react tribochemically with the friction pair sliding against each other to form a tribochemical protective film. The physical adsorption film, the viscous liquid film and the tribochemical reaction film work synergistically to effectively improve the friction reduction and anti-wear performance and load-bearing performance of the water-based lubricant.

[0030] The present invention provides a method for preparing the above-mentioned proton type polyionic liquid. The proton type polyionic liquid of the present invention can be obtained by one-step polymerization. The preparation method is simple, does not require complex steps such as ion exchange, and is easy to mass produce. DETAILED DESCRIPTION

[0031] The present invention provides a proton type polyionic liquid, comprising cations and anions, wherein the cations are copolymers of N-vinyl pyrrolidone and dimethylaminoethyl methacrylate, and the anions are alkyl carboxylate anions and / or dibutyl phosphate anions;

[0032] The cation has a structure shown in Formula I:

[0033]

[0034] In Formula I, m:n=5:1 to 1:5, and specifically preferably 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4 or 1:5.

[0035] In the present invention, the alkyl carboxylate anion has a structure shown in Formula II:

[0036]

[0037] In formula II, x is any integer from 1 to 11, preferably from 3 to 10, more preferably from 5 to 8, and specifically preferably 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or 11.

[0038] In the present invention, the alkyl carboxylate anion preferably includes one or more of acetate anion, butyrate anion, caproate anion, octanoate anion and laurate anion.

[0039] In the present invention, the dibutyl phosphate anion has a structure shown in Formula III:

[0040]

[0041] Polyvinyl pyrrolidone (PVP) has good water solubility. The present invention uses polyvinyl pyrrolidone as a repeating unit of a polyionic liquid to significantly improve the solubility and viscosity of the polymer. In addition, PVP has very low toxicity, good physiological compatibility, and low price. At the same time, it contains active nitrogen elements, which makes it easier to generate a tribochemical reaction film. Dimethylaminoethyl methacrylate in the cation is used to provide an alkaline tertiary amine functional group for preparing a proton-type polyionic liquid. In addition, the structure of dimethylaminoethyl methacrylate also contains active nitrogen elements. The present invention uses a copolymer of N-vinyl pyrrolidone and dimethylaminoethyl methacrylate as a cation, and an alkyl carboxylate anion and / or dibutyl phosphate anion as an anion. The active nitrogen element in its molecular structure can react tribochemically with the interface of the friction pair that slides against each other to generate a tribochemical protective film, which can not only improve the friction reduction and anti-wear performance of the water-based lubricant, but also greatly improve its extreme pressure bearing performance. Alkyl carboxylate anions or dibutyl phosphate anions can be effectively adsorbed on the interface of the metal friction pair to form a physical adsorption film, which can significantly improve the lubrication performance of the lubricant. The proton-type polyionic liquid aqueous solution has a high viscosity and good film-forming ability on the friction pair surface. The physical adsorption film, the viscoelastic liquid film and the tribochemical reaction film work synergistically, effectively improving the friction reduction and anti-wear performance and load-bearing performance of the water-based lubricant.

[0042] The present invention provides a method for preparing the above-mentioned proton type polyionic liquid, comprising the following steps:

[0043] Dimethylaminoethyl methacrylate, anion raw material and solvent are mixed to perform a proton exchange reaction to obtain a proton exchange reaction solution; the anion raw material is an alkyl carboxylic acid and / or dibutyl phosphate;

[0044] The proton exchange reaction liquid, N-vinyl pyrrolidone and an initiator are mixed to carry out a polymerization reaction to obtain a proton type polyionic liquid.

[0045] Unless otherwise specified, the raw materials used in the present invention are all commercially available.

[0046] The present invention mixes dimethylaminoethyl methacrylate, anion raw materials and solvent, performs proton exchange reaction, and obtains a proton exchange reaction liquid. In the present invention, the anion raw materials are alkyl carboxylic acids and / or dibutyl phosphate. In the present invention, the alkyl carboxylic acids are preferably one or more of acetic acid, butyric acid, caproic acid, caprylic acid and lauric acid.

[0047] In the present invention, the molar ratio of dimethylaminoethyl methacrylate to the anion raw material is preferably 1 to 2:1, more preferably 1.5:1.

[0048] In the present invention, the solvent is preferably water, a water-ethylene glycol mixture or ethylene glycol. The present invention has no special requirements for the volume ratio of water to ethylene glycol in the water-ethylene glycol mixture. In the present invention, the volume ratio of the amount of dimethylaminoethyl methacrylate to the solvent is preferably 0.05mol:30-150g, preferably 0.05mol:60g, specifically preferably 0.05mol:30g, 0.05mol:40g, 0.05mol:50g, 0.05mol:60g, 0.05mol:70g, 0.05mol:80g, 0.05mol:90g, 0.05mol:100g, 0.05mol:110g, 0.05mol:120g, 0.05mol:130g, 0.05mol:140g or 0.05mol:150g.

[0049] In the present invention, the temperature of the proton exchange reaction is preferably room temperature, and the time is 10 to 180 min, preferably 20 to 120 min, and more preferably 30 min.

[0050] After obtaining the proton exchange reaction liquid, the present invention mixes the proton exchange reaction liquid, N-vinyl pyrrolidone and an initiator to perform a polymerization reaction to obtain a proton type polyionic liquid. In the present invention, the molar ratio of N-vinyl pyrrolidone to dimethylaminoethyl methacrylate is preferably 5:1 to 1:5, and more preferably 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4 or 1:5.

[0051] In the present invention, the initiator preferably includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate; the mass of the initiator is preferably 0.003-1% of the total mass of dimethylaminoethyl methacrylate and the anion raw material, more preferably 0.01-0.1%, specifically preferably 0.003%, 0.005%, 0.008%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95% or 1%.

[0052] After the proton exchange reaction solution, N-vinyl pyrrolidone and initiator are mixed, the obtained mixed solution is preferably deoxygenated. In the present invention, the deoxygenation is preferably bubbling deoxygenation, and the deoxygenation time is preferably 20 to 120 minutes, more preferably 30 minutes.

[0053] In the present invention, the polymerization reaction temperature is preferably 50-90°C, more preferably 60-80°C; the time is preferably 1-36h, more preferably 5-30h, further preferably 10-25h, further preferably 15-20h. In the present invention, the polymerization reaction is preferably carried out under stirring.

[0054] In the present invention, after the polymerization reaction, the present invention preferably removes the solvent to obtain a proton-type polyionic liquid. Alternatively, the present invention uses a water-based lubricating liquid as a solvent, and after the polymerization reaction, the present invention does not remove the solvent, and directly obtains a proton-type polyionic liquid in situ in the water-based lubricating liquid.

[0055] The present invention provides the use of the above-mentioned proton-type polyionic liquid as a water-based thickening lubricant additive. In the present invention, the water-based lubricant preferably includes one or more of water, a water-ethylene glycol mixture, a water-glycerol mixture, and a water-ethylene glycol-glycerol mixture; in the present invention, the mass ratio of water to other components in the water-ethylene glycol mixture, the water-glycerol mixture, and the water-ethylene glycol-glycerol mixture is independently preferably 0.5:1 to 2:1, more preferably 0.8:1 to 1.5:1, and further preferably 1:1.

[0056] In the present invention, the amount of the protic polyionic liquid added to the water-based lubricating fluid is preferably 0.1 to 40 wt %, more preferably 0.5 to 30 wt %, more preferably 1 to 20 wt %, and even more preferably 5 to 15 wt %.

[0057] The present invention provides a water-based lubricant product, comprising a water-based base lubricant and the above-mentioned proton-type polyionic liquid. In the present invention, the water-based base lubricant preferably comprises one or more of water, a water-ethylene glycol mixture, a water-glycerol mixture, and a water-ethylene glycol-glycerol mixture; in the present invention, the mass ratio of water to other components in the water-ethylene glycol mixture, the water-glycerol mixture, and the water-ethylene glycol-glycerol mixture is independently preferably 0.5:1 to 2:1, and more preferably 1:1.

[0058] In the present invention, the mass concentration of the protic polyionic liquid in the water-based lubricant product is preferably 0.1-40 wt %, more preferably 0.5-30 wt %, more preferably 1-20 wt %, and further preferably 5-15 wt %.

[0059] The proton type polyionic liquid provided by the present invention, its preparation method and its application as a water-based thickening lubricant additive are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0060] Example 1

[0061] Synthesis of protic polyionic liquids:

[0062] 7.8695g (0.05mol) of dimethylaminoethyl methacrylate and 7.2105g (0.05mol) of n-octanoic acid were added to a 250mL three-necked flask containing 60g of deionized water to dissolve and perform proton exchange. After 0.5h, 2.7785g (0.025mol) of N-vinyl pyrrolidone and 0.04g of initiator ammonium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30min. The system was placed in a 70℃ oil bath pot and continuously mechanically stirred and heated for 8h. After the reaction, the solvent was removed and vacuum dried to obtain the additive PNM-CA1.

[0063] The lubrication performance of the synthesized polyionic liquid as a water lubricant additive was evaluated using an SRV-V vibration friction and wear tester produced by Optimol, Germany. Water or water-ethylene glycol (mass ratio 1:1) was selected as the control sample, and the mass concentration of the polyionic liquid additive was 5wt%. The test conditions selected in the tribological test are as follows: load 100N, temperature 25℃, frequency 25Hz, amplitude 1mm, test time 30min; the upper test ball in the test is a Φ10mm AISI 52100 steel ball; in the steel / steel friction pair, the lower sample is a Φ24mm, 7.9mm thick AISI 52100 steel block with a hardness of 700-750HV; the wear volume of the lower sample is measured by a MicroXAM-800 non-contact three-dimensional surface profiler. The average friction coefficient and average wear volume of different base lubricants and base lubricants containing polyionic liquid lubricant additives are shown in Table 1.

[0064] Table 1 Average friction coefficient and average wear volume of PNM-CA1 at a concentration of 5wt% in different base lubricants

[0065] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> water 0.328 322.5 Water+5%PNM-CA1 0.075 28.5 Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-CA1 0.072 19.7

[0066] Example 2

[0067] Synthesis of protic polyionic liquids:

[0068] 7.8695g (0.05mol) dimethylaminoethyl methacrylate and 7.2105g (0.05mol) n-octanoic acid were added to a 250mL three-necked flask containing 60g of deionized water to dissolve and perform proton exchange. After 0.5h, 5.557g (0.05mol) N-vinyl pyrrolidone and 0.04g initiator potassium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30min. The system was placed in a 70℃ oil bath pot and continuously mechanically stirred and heated for 8h. After the reaction, the solvent was removed and vacuum dried to obtain the additive PNM-CA2.

[0069] PNM-CA2 was dissolved in water or water-ethylene glycol (mass ratio 1:1) solution to prepare a solution with a concentration of 5 wt%. The tribological properties of the obtained PNM-CA2 in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 2.

[0070] Table 2 Average friction coefficient and average wear volume of PNM-CA2 at a concentration of 5wt% in different base lubricants

[0071] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> water 0.328 322.5 Water + 5% PNM-CA2 0.082 38.5 Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-CA2 0.079 23.7

[0072] Example 3

[0073] Synthesis of protic polyionic liquids:

[0074] 7.8695g (0.05mol) of dimethylaminoethyl methacrylate and 5.8079g (0.05mol) of n-hexanoic acid were added to a 250mL three-necked flask containing 60g of deionized water to dissolve and perform proton exchange. After 0.5h, 2.7785g (0.025mol) of N-vinyl pyrrolidone and 0.04g of initiator ammonium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30min. The system was placed in a 70℃ oil bath pot and continuously mechanically stirred and heated for 8h. After the reaction, the solvent was removed and vacuum dried to obtain the additive PNM-HA.

[0075] PNM-HA was dissolved in water or water-ethylene glycol (mass ratio 1:1) solution to prepare a solution with a concentration of 5 wt%. The tribological properties of the obtained PNM-HA in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 3.

[0076] Table 3 Average friction coefficient and average wear volume of PNM-HA with a concentration of 5wt% in different base lubricants

[0077] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> water 0.328 322.5 Water + 5% PNM-HA 0.088 43.1 Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-HA 0.082 26.9

[0078] Example 4

[0079] Synthesis of protic polyionic liquids:

[0080] 7.8695g (0.05mol) of dimethylaminoethyl methacrylate and 4.4055g (0.05mol) of n-butyric acid were added to a 250mL three-necked flask containing 60g of deionized water to dissolve and perform proton exchange. After 0.5h, 2.7785g (0.025mol) of N-vinyl pyrrolidone and 0.04g of initiator sodium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30min. The system was placed in a 70℃ oil bath pot and continuously mechanically stirred and heated for 8h. After the reaction, the solvent was removed and vacuum dried to obtain the additive PNM-BA.

[0081] PNM-BA was dissolved in water or water-ethylene glycol (mass ratio 1:1) solution to prepare a solution with a concentration of 5 wt%. The tribological properties of the obtained PNM-BA in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 4.

[0082] Table 4 Average friction coefficient and average wear volume of PNM-BA with a concentration of 5wt% in different base lubricants

[0083] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> water 0.328 322.5 Water+5%PNM-BA 0.128 80.1 Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-BA 0.115 31.9

[0084] Example 5

[0085] Synthesis of proton-type polyionic liquid: 7.8695g (0.05mol) dimethylaminoethyl methacrylate and 10.5105g (0.05mol) dibutyl phosphate were added to a 250mL three-necked flask containing 60g of deionized water to dissolve and perform proton exchange. After 0.5h, 2.7785g (0.025mol) N-vinyl pyrrolidone and 0.04g initiator ammonium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30min. The system was placed in a 70℃ oil bath pot and heated for continuous mechanical stirring for 8h. After the reaction, the solvent was removed and vacuum dried to obtain the additive PNM-DBP.

[0086] PNM-DBP was dissolved in water or water-ethylene glycol (mass ratio 1:1) solution to prepare a solution with a concentration of 5 wt%. The tribological properties of the obtained PNM-DBP in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 5.

[0087] Table 5 Average friction coefficient and average wear volume of PNM-DBP at a concentration of 5 wt% in different water-ethylene glycol based lubricants

[0088] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> water 0.328 322.5 Water + 5% PNM-DBP 0.120 70.2 Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-DBP 0.112 28.9

[0089] Example 6

[0090] Synthesis of proton-type polyionic liquid: 7.8695g (0.05mol) dimethylaminoethyl methacrylate, 5.7685g (0.04mol) n-octanoic acid and 2.1021g (0.01mol) dibutyl phosphate were added to a 250mL three-necked flask containing 60g deionized water to dissolve and perform proton exchange. After 0.5h, 2.7785g (0.025mol) N-vinyl pyrrolidone and 0.04g initiator ammonium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30min. The system was placed in a 70℃ oil bath pot and continuously mechanically stirred and heated for 8h. After the reaction, the solvent was removed and vacuum dried to obtain the additive PNM-CP.

[0091] PNM-CP was dissolved in water or water-ethylene glycol (mass ratio 1:1) solution to prepare a solution with a concentration of 5 wt%. The tribological properties of the obtained PNM-CP in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 6.

[0092] Table 6 Average friction coefficient and average wear volume of PNM-CP with a concentration of 5wt% in different base lubricants

[0093] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> water 0.328 322.5 Water + 5% PNM-CP 0.077 40.5 Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-CP 0.075 24.6

[0094] Example 7

[0095] Synthesis of protic polyionic liquids:

[0096] 7.8695 g (0.05 mol) of dimethylaminoethyl methacrylate and 10.0159 g (0.05 mol) of lauric acid were added to a 250 mL three-necked flask containing 60 g of a water-ethylene glycol mixed solution (mass ratio 1:1) to dissolve and perform proton exchange. After 0.5 h, 2.7785 g (0.025 mol) of N-vinyl pyrrolidone and 0.04 g of initiator ammonium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30 min. The system was placed in an 80 ° C oil bath pot and continuously mechanically stirred and heated for reaction for 6 h. The lubricating liquid water-ethylene glycol + PNM-LA was obtained by in-situ reaction.

[0097] The water-ethylene glycol + PNM-LA obtained by the reaction was diluted with a water-ethylene glycol solution to an additive solution with a solid content of 5 wt%. The tribological properties of the obtained water-ethylene glycol + PNM-LA in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 7:

[0098] Table 7 Average friction coefficient and average wear volume of PNM-LA water-ethylene glycol solution with a concentration of 5wt%

[0099] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-LA 0.068 17.9

[0100] Example 8

[0101] Synthesis of protonic polyionic liquid: 7.8695 g (0.05 mol) of dimethylaminoethyl methacrylate and 7.2105 g (0.05 mol) of octanoic acid were added to a 250 mL three-necked flask containing 60 g of a water-ethylene glycol (mass ratio 1:1) mixed solution to dissolve and perform proton exchange. After 0.5 h, 2.7785 g (0.025 mol) of N-vinyl pyrrolidone and 0.04 g of initiator ammonium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30 min. The system was placed in an 80 ° C oil bath with continuous mechanical stirring and heating for 6 h. The lubricating liquid water-ethylene glycol + PNM-CA3 was obtained by in-situ reaction.

[0102] The water-ethylene glycol + PNM-CA3 obtained by the reaction was diluted with a water-ethylene glycol solution to an additive solution with a solid content of 5 wt%. The tribological properties of the obtained water-ethylene glycol + PNM-CA3 in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 8.

[0103] Table 8 Average friction coefficient and average wear volume of PNM-CA3 water-ethylene glycol solution with a concentration of 5wt%

[0104] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-CA3 0.071 19.9

[0105] Example 9

[0106] Synthesis of protic polyionic liquids:

[0107] 7.8695 g (0.05 mol) of dimethylaminoethyl methacrylate and 7.2105 g (0.05 mol) of n-octanoic acid were added to a 250 mL three-necked flask containing 60 g of ethylene glycol to dissolve and perform proton exchange. After 0.5 h, 2.7785 g (0.025 mol) of N-vinyl pyrrolidone and 0.04 g of initiator sodium persulfate were added to the reaction bottle to dissolve, and bubbling deoxygenation was performed for 30 min. The system was placed in an 80 ° C oil bath pot with continuous mechanical stirring and heating for 6 h to obtain an ethylene glycol solution of the additive PNM-CA4 by in-situ reaction.

[0108] The ethylene glycol solution of PNM-CA4 obtained by the reaction was diluted with water to a water-ethylene glycol (mass ratio 1:1) solution with a solid content of 5 wt%. The tribological properties of the obtained water-ethylene glycol + PNM-CA4 in the base lubricating fluid were evaluated according to the method in Example 1. The test conditions were the same as in Example 1. The test results are shown in Table 9.

[0109] Table 9 Average friction coefficient and average wear volume of PNM-CA4 water-ethylene glycol solution with a concentration of 5wt%

[0110] Basic lubricant Average friction coefficient <![CDATA[Average wear volume (×10 -5 / mm 3 )]]> Water-ethylene glycol 0.191 63.3 Water-ethylene glycol + 5% PNM-CA4 0.072 20.1

[0111] Test Example 1 Anti-corrosion Performance Test

[0112] The polyionic liquid prepared in Examples 1 to 9 was formulated into a basic lubricating solution with a concentration of 1 wt%, and the corrosion resistance test was carried out according to the standard of GB6144-85, with water and water-ethylene glycol (mass ratio 1:1) as the control group. Cast iron sheets of the same specifications were immersed in water, water-ethylene glycol, and the additive solution prepared in Examples 1 to 9 at 55±2°C, respectively, and taken out after 24 hours, ultrasonically cleaned in acetone, dried with high-speed gas, and the surface of the cast iron sheet was observed under an optical microscope, and the corrosion conditions of the cast iron sheets in the above different aqueous solutions were analyzed, and the corrosion grade was obtained by comparing with the corrosion colorimetric card. The results are shown in Table 10.

[0113] Table 10 Corrosion resistance test results of ionic liquids obtained in Examples 1 to 9

[0114] sample Corrosion level water D Water-ethylene glycol D Water+5%PNM-CA1 A Water-ethylene glycol + 5% PNM-CA1 A Water + 5% PNM-CA2 A Water-ethylene glycol + 5% PNM-CA2 A Water + 5% PNM-HA B Water-ethylene glycol + 5% PNM-HA B Water+5%PNM-BA B Water-ethylene glycol + 5% PNM-BA B Water + 5% PNM-DBP B Water-ethylene glycol + 5% PNM-DBP B Water + 5% PNM-CP A Water-ethylene glycol + 5% PNM-CP A Water-ethylene glycol + 5% PNM-LA A Water-ethylene glycol + 5% PNM-CA3 A Water-ethylene glycol + 5% PNM-CA4 A

[0115] In Table 10, A means no rust and bright as new; B means no rust but slightly tarnished; C means light rust and slight tarnished; D means heavy rust or serious tarnished.

[0116] It can be seen from the experimental results in Table 10 that the proton type polyionic liquid provided by the present invention can significantly improve the anti-corrosion performance of the water-based lubricating fluid when used as an additive for the water-based lubricating fluid.

[0117] Test Example 2: Viscosity Test

[0118] The polyionic liquids prepared in Examples 1 to 9 were formulated into aqueous solutions or water-ethylene glycol solutions (mass ratio 1:1) with a concentration of 5 wt%. The kinematic viscosities of deionized water, water-ethylene glycol, and the additive solutions prepared in Examples 1 to 9 at 25°C and 40°C were measured using a Pinnacle viscometer. The experimental results are shown in Table 11.

[0119] Table 11 Kinematic viscosity of deionized water and 5 wt% polyionic liquid solution at 25°C and 40°C

[0120]

[0121] It can be seen from the experimental results in Table 11 that the proton-type polyionic liquid prepared in the present invention, when used as a water-based lubricant additive, can significantly increase the kinematic viscosity of the water-based lubricant and enhance the film-forming ability of the water-based lubricant at the friction interface.

[0122] According to the above embodiments and test examples, the proton type polyionic liquid lubricating additive provided by the present invention can greatly improve the corrosion resistance, viscosity performance and friction reduction and anti-wear performance of water-based lubricating fluid. In addition, the proton type polyionic liquid lubricating additive provided by the present invention has a simple synthesis process, is green and pollution-free, has a low synthesis cost, and has broad application prospects as a water-based lubricating additive.

[0123] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A proton-type polyionic liquid comprising cations and anions, characterized in that: The cation is a copolymer of N-vinyl pyrrolidone and dimethylaminoethyl methacrylate, and the anion is an alkyl carboxylate anion and / or a dibutyl phosphate anion; The cation has a structure shown in Formula I: In formula I, m:n=5:1 to 1:

5.

2. The protic polyionic liquid according to claim 1, characterized in that The alkyl carboxylate anion has a structure shown in Formula II: In formula II, x is any integer from 1 to 11.

3. The protic polyionic liquid according to claim 1 or 2, characterized in that: The alkyl carboxylate anion includes one or more of acetate anion, butyrate anion, caproate anion, octanoate anion and laurate anion.

4. The protic polyionic liquid according to claim 1, characterized in that The dibutyl phosphate anion has a structure shown in Formula III:

5. The method for preparing the protic polyionic liquid according to any one of claims 1 to 4, comprising the following steps: Dimethylaminoethyl methacrylate, anion raw material and solvent are mixed to perform a proton exchange reaction to obtain a proton exchange reaction solution; the anion raw material is an alkyl carboxylic acid and / or dibutyl phosphate; The proton exchange reaction liquid, N-vinyl pyrrolidone and an initiator are mixed to carry out a polymerization reaction to obtain a proton type polyionic liquid.

6. The preparation method according to claim 5, characterized in that: The molar ratio of dimethylaminoethyl methacrylate to the anion raw material is 1 to 2:1; The molar ratio of N-vinyl pyrrolidone to dimethylaminoethyl methacrylate is 5:1 to 1:

5.

7. The preparation method according to claim 5 or 6, characterized in that: The initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate; The mass of the initiator is 0.003-1% of the total mass of dimethylaminoethyl methacrylate and the anion raw material.

8. The preparation method according to claim 5, characterized in that: The polymerization reaction temperature is 50-90° C. and the reaction time is 1-36 hours.

9. Use of the proton type polyionic liquid according to any one of claims 1 to 4 or the proton type polyionic liquid prepared by the preparation method according to any one of claims 5 to 8 as a water-based viscosity increasing lubricant additive.

10. A water-based lubricant product, comprising a water-based base lubricating liquid and the proton-type polyionic liquid according to any one of claims 1 to 4 or the proton-type polyionic liquid prepared by the preparation method according to any one of claims 5 to 8; The water-based lubricating fluid includes one or more of water, a water-ethylene glycol mixture, a water-glycerin mixture, and a water-ethylene glycol-glycerin mixture; The mass concentration of the proton type polyionic liquid in the water-based lubricant product is 0.1-40wt%.

Citation Information

Patent Citations

  • Water-soluble polyionic liquid lubricating additive and application

    CN110964587A

  • Polyionic liquid, preparation method and application thereof, lubricating and tackifying additive and supramolecular gel lubricant

    CN114656588A

  • Polymer-based ionic water-based lubricating additive as well as preparation method and application thereof

    CN114874386A

  • Use of water-based lubricants for textile machines

    WO2011131331A1

Cited By

  • Environment-friendly water-based trace lubricant as well as preparation method and application thereof

    CN122357208A