Polyglycolide polymer material as well as preparation method and application thereof
Through the copolymerization reaction of starch and polyglycolide segments, a polyglycolide polymer material with high molecular weight and bimodal molecular weight distribution is prepared, which solves the problems of poor toughness and high energy consumption in traditional polyglycolide materials. It has achieved efficient improvement in processability and production efficiency of polyglycolide materials.
Patent Information
- Application Number
- CN202310555617.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
The molecular weight of traditional polyglycolide materials is low, resulting in poor toughness and high melt flowability, making them unable to be suitable for thin film products, and the production process consumes high energy and is large in carbon emissions, resulting in high production costs.
By copolymerizing starch with monomers that can form polyglylactide segments, a polyglylactide polymer material with high molecular weight and bimodal molecular weight distribution is prepared, which improves its strength and melt flow and is extruded on a twin screw Continuous preparation is achieved on-board out, shortening reaction time, reducing energy consumption and carbon emissions.
Improves the tensile strength and elongation of break of polyglycolide materials, improves its processability in casting and blown film applications, reduces production costs and energy consumption, has high production efficiency and promotion and application value .
Smart Images

Figure CN118994607A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and more particularly to a polyglycolide polymer material and a preparation method and application thereof. Background Art
[0002] Biodegradable polyester, as an environmentally friendly material, can partially replace existing petroleum-based polyester. Polyglycolide (PGA) has received widespread attention as a biodegradable material. PGA can be prepared by glycolic acid melt polycondensation or glycolide ring-opening polymerization. The obtained product has a small molecular weight, insufficient tensile strength and melt strength. In some fields, such as when used as fracture fixation, disposable tableware, etc., its strength is insufficient. The PGA prepared by the traditional method cannot be applied to film products due to its low molecular weight and high melt flow rate. In addition, the traditional method is an intermittent polymerization method with a long reaction cycle (reaction time 40 to 80 hours) and high energy consumption and carbon emissions, so the production cost is high.
[0003] Starch is a nutrient stored in seeds and tubers in plants, usually composed of amylose and amylopectin. Amylose is formed by glucose units connected by α-1,4 glycosidic bonds, and amylopectin is composed of α-1,4 glycosidic bonds and α-1,6 glycosidic bonds. Starch is a polyhydroxy compound, each glucose structural unit contains hydroxyl groups on the 2, 3, and 6 carbons, and is a completely biodegradable material. By introducing macromolecular starch, the molecular structure and molecular weight of PGA are changed, thereby changing some of the properties of PGA.
[0004] Therefore, it is necessary to study a polyglycolide polymer material, by grafting and modifying polyglycolide to improve its strength and reduce its melt fluidity, thereby improving its processability in applications such as casting and blown film, and can be applied to film products. Summary of the invention
[0005] In order to solve the technical problems existing in the prior art, the present invention provides a polyglycolide polymer material and a preparation method and application thereof.
[0006] The present invention uses starch and a monomer capable of generating a polyglycolide chain segment to copolymerize to prepare a polyglycolide polymer material, which overcomes the disadvantages of low molecular weight and poor toughness of the polyglycolide material in the prior art, has the characteristics of high molecular weight and bimodal molecular weight distribution, so that the polyglycolic acid has high strength and low melt fluidity at the same time, improves its processability in applications such as casting and blown film, and the obtained polyglycolide polymer material has high tensile strength and elongation at break. At the same time, the preparation method of the polyglycolide polymer material in the present invention has high production efficiency, can realize continuous preparation on a twin-screw extruder, greatly reduces reaction time, saves energy consumption and reduces carbon emissions.
[0007] One of the objects of the present invention is to provide a polyglycolide polymer material.
[0008] The polyglycolide polymer material includes starch-polyglycolide graft copolymer and polyglycolide homopolymer;
[0009] The structural formula of the starch-polyglycolide graft copolymer is:
[0010]
[0011] Wherein, R1, R2, and R3 are independently selected from hydrogen atoms or alkane groups or aromatic hydrocarbon groups with a molecular weight of 15 to 1000 g / mol, R a , R b are independently selected from a hydrogen atom or Where R x is R1, R2 or R3, p is an integer greater than 10, preferably an integer of 150 to 10000; n is greater than 50, preferably 60 to 10000; p1, p2, p3 are independently selected from integers greater than 10, preferably from 150 to 10000; if the starch used is amylopectin, amylopectin has a side chain branch at position 6 of the main chain, but its structural repeating unit is the same as the structural formula of Figure I; wherein the main chain or side chain end structure of the starch molecule is R1, R2, R3, R a or R b The starch and polyglycolide side chains of the starch-polyglycolide graft copolymer are linked by ester bonds, and the primary hydroxyl group at position 6 of the glucose repeating unit and secondary hydroxyl grafting at positions 2 and 3
[0012]
[0013] The structural formula of the polyglycolide homopolymer is:
[0014]
[0015] Among them, M1, M2, ..., M i are the same or different and are independently selected from imino, nitro or ether bonds; R is a hydrogen atom (when i=1) or an alkane or aromatic hydrocarbon group with a molecular weight of 15 to 1000 g / mol; n1, n2, ..., n i are all integers not equal to 0, and n1, n2, ..., n i The sum is not less than 50, preferably 50 to 3000; i is an integer of 1 to 20, preferably an integer of 2 to 6, for example 2, 3, 4, 5, 6.
[0016] The starch-polyglycolide graft copolymer is obtained by surface hydroxyl grafting, wherein the central particle is a starch particle, and the surface hydroxyl initiates the grafting of polyglycolide, and the copolymer structure is shown in the following formula:
[0017]
[0018] Wherein a, n, y, and z are all integers, preferably integers greater than 10.
[0019] In a preferred embodiment of the present invention,
[0020] The molecular weight distribution of the polyglycolide copolymer material is a bimodal molecular weight distribution, preferably comprising an ultra-high molecular weight starch-polyglycolide graft copolymer peak and a polyglycolide homopolymer peak;
[0021] Preferably,
[0022] The weight average molecular weight M of the ultra-high molecular weight starch-polyglycolide graft copolymer peak w1 5.0×10 5 ~3.0×10 6 g / mol, preferably 8.0×10 5 ~2.0×10 6 g / mol, the molecular weight distribution index is 1.0 to 2.0, preferably 1.0 to 1.5;
[0023] The weight average molecular weight M of the polyglycolide homopolymer peak w2 5.0×10 4 ~1.5×10 5 g / mol, preferably 1.0×10 5 ~1.5×10 5 g / mol; the molecular weight distribution index is 1.5 to 3.0, preferably 1.5 to 2.5;
[0024] The weight average molecular weight M of the polyglycolide polymer material w 1.0×10 5 ~2.0×10 6 g / mol, preferably 1.0×10 5 ~3.0×10 5 g / mol; the molecular weight distribution index is 1.5 to 15.0, preferably 1.5 to 4.0.
[0025] In a preferred embodiment of the present invention,
[0026] Taking the total mass of the polyglycolide polymer material as 100%, the mass content of the starch-polyglycolide graft copolymer is 1-50%, preferably 1-20%, and more preferably 4-15%; the mass content of the polyglycolide homopolymer is 50-99%, preferably 80-99%, and more preferably 85-96%.
[0027] In a preferred embodiment of the present invention,
[0028] The melt flow rate of the polyglycolide polymer material at 230° C. / 2.16 kg is not higher than 20 g / 10 min, preferably 3 to 20 g / 10 min.
[0029] The elongation at break of the polyglycolide copolymer material is at least 50% higher than that of the polyglycolide homopolymer, and the tensile strength of the polyglycolide copolymer material is at least 10 MPa higher than that of the polyglycolide homopolymer.
[0030] In a preferred embodiment of the present invention,
[0031] The polyglycolide polymer material comprises starch, which can be polymerized to obtain polyglycolide chain segments. The raw materials are prepared from monomers, small molecule co-initiators, and catalysts; preferably, the raw materials also include at least one of small molecule co-initiators and antioxidants; wherein the degree of polymerization p includes p1, p2, p3, n1, n2, ..., n i .
[0032] In a preferred embodiment of the present invention,
[0033] The starch is unmodified native starch or modified starch, preferably at least one of native corn starch, native cassava starch, native wheat starch, hydroxymethyl starch, and hydroxyethyl starch; the unmodified native starch includes at least one of amylose and amylopectin; preferably, the starch is amylose (molecular weight 5×10 5 ~2×10 6 g / mol), amylopectin (molecular weight 15×10 6 ~400×10 6 g / mol);
[0034] The polyglycolide chain segment can be obtained by polymerization The monomer is at least one of methyl glycolate, glycolic acid, and glycolide;
[0035] The catalyst is a salt compound of at least one metal selected from the group IIA-VA metal elements and transition metal elements or an organic guanidine catalyst. Preferably, the catalyst is a salt compound of at least one selected from the group consisting of Sn, Bi, Mg, Al, Ca, Fe, Mn, Ti and Zn, and more preferably a Sn salt, such as stannous octoate.
[0036] The antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant, that is, it can be a hindered phenol antioxidant and a phosphite antioxidant and any combination thereof, including but not limited to 2,6-di-tert-butyl-p-cresol, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 2,2'-methylenebis(6-tert-butyl-4-methylphenol), hexanediol bis[β-(3,5-dibutyl-4-hydroxyphenyl)propionate], tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol (such as BASF's antioxidant 1010), N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine (such as antioxidant 1024), N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine (such as antioxidant 1098), β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid n-octadecyl ester (such as BASF's antioxidant 1076), at least one of 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, triphenyl phosphite, tri(4-nonylphenyl)phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl di(2-ethylhexyl) phosphite, phenyl diisodecyl phosphite, tri(2-ethylhexyl) phosphite, triisodecyl phosphite, tri(dodecyl) phosphite, pentaerythritol diisodecyl phosphite, tris[2.4-di-tert-butylphenyl]phosphite (such as antioxidant 168), bis(2,4-dicumylphenyl)pentaerythritol diphosphite (such as antioxidant 686) and bis(2,4-di-tert-butylphenyl)propionate]pentaerythritol diphosphite (such as antioxidant 626);
[0037] The small molecule co-initiator is a small molecule substance containing hydroxyl or amino groups with a boiling point greater than 160° C. and a molecular weight less than 1000 g / mol, preferably at least one of ethylene glycol, butanediol, propylene glycol, serinol, leucinol, pentaerythritol, sorbitol, xylitol, amino acids, phenol, hydroquinone, resorcinol, benzyl alcohol, aniline, benzylamine, and p-phenylenediamine.
[0038] In a preferred embodiment of the present invention,
[0039] The polyglycolide chain segment can be obtained by polymerization The monomers are 100 parts by mass and include the following raw materials:
[0040]
[0041] The second object of the present invention is to provide a method for preparing a polyglycolide copolymer material, comprising:
[0042] The amount includes the polyglycolide chain segment that can be polymerized The raw materials of monomer, starch and small molecule co-initiator are subjected to melt polymerization reaction in the presence of a catalyst, and then cooled to obtain the polyglycolide polymer material; preferably, the raw materials also include at least one of a small molecule co-initiator and an antioxidant;
[0043] Preferably, the temperature of the melt polymerization is 140 to 250° C., preferably 200 to 240° C.; the reaction time is 0.5 to 60 min, preferably 1 to 20 min, and more preferably 3 to 6 min. During the melt polymerization reaction, if it is carried out in a twin-screw extruder, the feeding speed is 1 to 5 kg / h, preferably 1 to 3 kg / h.
[0044] In a preferred embodiment of the present invention,
[0045] The melt polymerization reaction is carried out in a continuous melt mixing device, which is a series combination of one or more of a kettle reactor, a tubular reactor, an internal mixer, a Farrel continuous mixer, a Banbury mixer, a single screw extruder, a multi-screw extruder and a reciprocating single screw extruder, preferably an internal mixer or a twin-screw extruder;
[0046] The melt polymerization reaction is preferably carried out in a continuous twin-screw extruder, more preferably in at least two continuous twin-screw extruders connected in series, such as 2, 3, 4, etc. For example, when the reaction is carried out in multiple continuous twin-screw extruders, the polymerization reaction can be carried out in the first twin-screw extruder, and the volatile components such as unreacted monomers and small molecular products generated by the degradation of polymers at high temperature are removed in the second (or second + third) twin-screw extruder, and various additives can also be added to the second (or second + third) twin-screw extruder;
[0047] Preferably, the processing conditions of the continuous twin-screw extruder include:
[0048] The processing temperature is 140-250°C, preferably 200-240°C;
[0049] The screw speed is 5 to 300 rpm, preferably 40 to 150 rpm;
[0050] The aspect ratio is 25-80, preferably 25-70.
[0051] The melt polymerization reaction can also be carried out in an internal mixer; preferably, the internal mixer temperature is 180-250°C, preferably 200-230°C, the rotation speed is 5-150 rpm, preferably 20-80 rpm, and the reaction time is 1-30 min, preferably 3-15 min.
[0052] The continuous twin-screw extruder equipment applicable to the present invention includes twin-screw extruders of different designs, such as the HAAKE Eurolab16 desktop parallel co-rotating twin-screw extruder produced by Thermo Fisher in the United States, the ZSK Mcc18 or ZSK 40 co-rotating parallel twin-screw extruders produced by Coperion in Germany, etc. The internal mixer equipment applicable to the present invention includes internal mixers of different designs, such as the PolyLab HAAKE produced by Thermo Fisher in the United States TM Rheomex OS 567-1000 internal mixer module, etc.
[0053] The third object of the present invention is to provide a polyglycolide polymer material obtained by the above preparation method.
[0054] A fourth object of the present invention is to provide an application of a polyglycolide polymer material in a plastic product, wherein the plastic product is preferably an injection molded product, a blown film product or a cast film product.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] The polyglycolide polymer material prepared by the invention has the characteristics of higher molecular weight and bimodal molecular weight distribution, so that the polyglycolic acid has high strength and low melt fluidity at the same time, and improves its processability in applications such as casting and film blowing.
[0057] At the same time, the preparation method of the polyglycolide polymer material in the present invention has high production efficiency, can realize continuous preparation on a twin-screw extruder, greatly reduces the reaction time, and shortens it from several hours in the existing technology to within a few minutes, significantly saves energy consumption and reduces carbon emissions, overcomes the defects of high production cost and energy consumption caused by the slow polymerization reaction of polyglycolic acid in the existing technology, and has extremely high promotion and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 The GPC charts of the polyglycolide polymer materials prepared in Example 1 and Comparative Example 1;
[0059] Depend on Figure 1It can be seen that the PGA obtained without adding native starch has a unimodal molecular weight distribution, and the LogMW is less than 5.25, while Example 1 has a bimodal molecular weight distribution, with a peak with a LogMW greater than 6.0 (ultra-high molecular weight peak) and a peak with a LogMW less than 5.25 (high molecular weight peak). DETAILED DESCRIPTION
[0060] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.
[0061] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0062] The raw materials used in the present invention are all commercially available;
[0063] Glycolide (GA), purchased from Shenzhen Boli Biomaterials Co., Ltd., purity ≥99.5%;
[0064] Corn starch, purchased from Aladdin, is native corn starch;
[0065] Stannous octoate and 1,4-butanediol were purchased from Sinopharm Chemical Reagent Co., Ltd. The purity of stannous octoate was AR grade, and the purity of 1,4-butanediol was CP grade;
[0066] Antioxidant 1010 was purchased from BASF (China) Co., Ltd., and antioxidant 626 (THP-24) was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., with a purity of ≥95%.
[0067] The present invention performs performance measurement according to the following method:
[0068] Gel Permeation Chromatography (GPC): The test instrument was PL-GPC50 gel permeation chromatograph from Angilent, USA, and the processing software was GPC offline. During the test, the mobile phase was hexafluoroisopropanol containing 5mmol / L sodium trifluoroacetate, the flow rate was 1mL / min, the column temperature was 40℃, the injection volume was 100μL, the standard sample was PMMA, and the sample concentration was 1mg / mL.
[0069] Melt flow index (MFR): Melt flow index measurement: The test was conducted on a CEAST MF20 melt flow rate tester from Instron, USA. The test temperature was 230°C, the load weight was 2.16 kg, and the preheating time was 4 minutes.
[0070] Injection molding processing method and tensile test: The samples were injection molded into 5A tensile specimens (thickness: 2 mm) on a HAAKE MiniJet micro-injection molding machine according to GB / T 1040.2-2006. The barrel temperature and mold temperature were 240°C and 50°C, respectively, the injection pressure and time were 400 bar and 5 s, respectively, and the holding pressure and time were 100 bar and 10 s, respectively. Then, the tensile test was carried out on a 3344 material testing machine of Instron Company of the United States, with a tensile rate of 50 mm / min and a clamp spacing of 50 mm.
[0071] [Example 1]
[0072] The above-mentioned glycolide (GA), corn starch, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed in a mass ratio of 1000:1:0.5:5:5:1, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000 g / hr. The temperatures of sections 2-11 of the extruder are 160°C, 200°C, 220°C, 220°C, 220°C, 220°C, 225°C, 230°C and 235°C, respectively, and the screw speed is set at 100 rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 300 seconds on average, and the reaction time can be considered to be about 300 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0073] The obtained polyglycolide polymer material includes starch-polyglycolide graft copolymer and polyglycolide homopolymer; the structural formula of starch-polyglycolide graft copolymer is:
[0074]
[0075] Wherein R1, R2, and R3 are independently selected from hydrogen atoms or alkane groups with a molecular weight of 92 g / mol, R a , R b are independently selected from a hydrogen atom or Where R x is R1, R2 or R3.
[0076] The structural formula of polyglycolide homopolymer is:
[0077]
[0078] [Example 2]
[0079] The above-mentioned glycolide (GA), corn starch, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:0.8:0.5:5:5:1, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 2000 g / hr. The temperatures of sections 2-11 of the extruder are: 160°C, 200°C, 220°C, 220°C, 220°C, 220°C, 220°C, 225°C, 230°C and 230°C, respectively, and the screw speed is set at 100 rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 200 seconds on average, and the reaction time can be considered to be about 200 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0080] The obtained polyglycolide polymer material includes starch-polyglycolide graft copolymer and polyglycolide homopolymer; the structural formulas of starch-polyglycolide graft copolymer and polyglycolide homopolymer are the same as those in Example 1.
[0081] [Example 3]
[0082] The above-mentioned glycolide (GA), corn starch, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:0.1:0.5:5:5:1, and the polymer was extruded and granulated using a HAAKE EuroLab 16 desktop co-rotating twin-screw extruder (screw diameter 16mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000g / hr. The temperatures of sections 2-11 of the extruder are: 180℃, 200℃, 210℃, 210℃, 220℃, 220℃, 220℃, 220℃, 220℃ and 220℃, respectively, and the screw speed is set at 100rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 200 seconds on average, and the reaction time can be considered to be about 200 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0083] The obtained polyglycolide polymer material includes starch-polyglycolide graft copolymer and polyglycolide homopolymer; the structural formulas of starch-polyglycolide graft copolymer and polyglycolide homopolymer are the same as those in Example 1.
[0084] [Example 4]
[0085] The above-mentioned glycolide (GA), corn starch, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:0.01:0.1:15:15:2, and the polymer was extruded and granulated using a HAAKE EuroLab 16 desktop co-rotating twin-screw extruder (screw diameter 16mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000g / hr. The temperatures of sections 2-11 of the extruder are: 180℃, 200℃, 210℃, 210℃, 220℃, 220℃, 220℃, 220℃, 220℃ and 220℃, respectively, and the screw speed is set at 100rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 200 seconds on average, and the reaction time can be considered to be about 200 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0086] The obtained polyglycolide polymer material includes starch-polyglycolide graft copolymer and polyglycolide homopolymer; the structural formulas of starch-polyglycolide graft copolymer and polyglycolide homopolymer are the same as those in Example 1.
[0087] [Example 5]
[0088] The above-mentioned glycolide (GA), corn starch, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:2:2:5:5:0.2, and the polymer was extruded and granulated using a HAAKE EuroLab 16 desktop co-rotating twin-screw extruder (screw diameter 16mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000g / hr. The temperatures of sections 2-11 of the extruder are: 180℃, 200℃, 210℃, 210℃, 220℃, 220℃, 220℃, 220℃, 220℃ and 220℃, respectively, and the screw speed is set at 100rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 200 seconds on average, and the reaction time can be considered to be about 200 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample strip is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, which are collected, dried and packaged for use. The obtained polyglycolide polymer material includes starch-polyglycolide graft copolymer and polyglycolide homopolymer; the structural formula of starch-polyglycolide graft copolymer and polyglycolide homopolymer is the same as that of Example 1.
[0089] [Example 6]
[0090] The above-mentioned glycolide (GA), corn starch, antioxidant 1010, antioxidant 626, and stannous octoate are fully premixed according to the mass ratio of 1000:1:5:5:0.2, and the polymer is extruded and granulated using a HAAKE EuroLab 16 desktop co-rotating twin-screw extruder (screw diameter 16mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw, and the feed rate is 1000g / hr. The temperatures of sections 2-11 of the extruder are: 180℃, 200℃, 210℃, 210℃, 220℃, 220℃, 220℃, 220℃, 220℃ and 220℃, respectively, and the screw speed is set at 100rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 200 seconds on average, and the reaction time can be considered to be about 200 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0091] The obtained polyglycolide polymer material includes starch-polyglycolide graft copolymer and polyglycolide homopolymer; the structural formulas of starch-polyglycolide graft copolymer and polyglycolide homopolymer are the same as those in Example 1.
[0092] [Comparative Example 1]
[0093] The above-mentioned glycolide (GA), 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:1.5:5:5:1, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000 g / hr. The temperatures of sections 2-11 of the extruder are: 180°C, 200°C, 220°C, 220°C, 220°C, 220°C, 230°C, 235°C and 240°C, and the screw speed is set at 100 rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 300 seconds on average, and the reaction time can be considered to be about 300 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and air-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0094] The obtained product is a polyglycolide homopolymer.
[0095] [Comparative Example 2]
[0096] Commercially available pure PGA, GMP grade glycolide homopolymer, brand: PURASORB PG S.
[0097] Table 1 shows the molecular weight and molecular weight distribution of the polyglycolide polymers of Examples 1 to 6 and Comparative Examples 1 to 2, the mass ratio of the graft copolymer to the homopolymer, and the polymerization degree of the graft copolymer. As can be seen from Table 1, the polyglycolide polymer materials prepared in Examples 1 to 6 have the characteristics of a relatively high molecular weight and a bimodal molecular weight distribution.
[0098] Figure 1 The GPC diagram of the polyglycolide polymer material prepared in Example 1 and Comparative Example 1 is shown in FIG. Figure 1 It can be seen that the PGA obtained without adding native starch has a unimodal molecular weight distribution, and the LogMW is less than 5.25, while Example 1 has a bimodal molecular weight distribution, with a peak with a LogMW greater than 6.0 (starch-polyglycolide graft copolymer) and a peak with a LogMW less than 5.25 (polyglycolide homopolymer), which also proves that the polyglycolide polymer material has a higher molecular weight and a bimodal molecular weight distribution.
[0099] Table 1 Molecular weight and distribution of polyglycolide polymers in Examples 1 to 6 and Comparative Examples 1 to 2 The mass ratio of graft copolymer to homopolymer and the degree of polymerization of graft copolymer
[0100]
[0101] * Calculated from the GPC curve integral area ratio. (The ordinate and abscissa of the GPC curve are related to the mass and molecular weight of the polymer, respectively. Therefore, the corresponding component mass can be obtained by integrating the curve. That is, the ratio of the integral area to the total integral area is the corresponding mass ratio, M n is the number average molecular weight, M w is the weight average molecular weight.)
[0102] **Polymerization degree n is the statistical average of polymerization degrees p1, p2, and p3. The high molecular weight fraction X% obtained by integrating the GPC curve and the cellulose fraction Y (glycolide is 1000) at the initial feed are calculated according to the following formula: 162*10*X / (58*Y). As shown in Table 1, multimodal molecular weight distribution appears in all the examples, and the M of the ultrahigh molecular weight peak is w Greater than 5×10 5 g / mol, and the proportion of this part is about 1 to 15wt%.
[0103] Table 2 shows the melt flow rate test results of the polyglycolide polymers of Examples 1 to 2, 4, and Comparative Examples 1 to 2. As can be seen from Table 2, the melt flow rates of Examples 1 to 2, 4 are significantly lower than those of Comparative Examples 1 to 2, proving that the polyglycolide polymer material prepared by the present invention has a high molecular weight and thus has low melt fluidity, while the melt strength and melt toughness are significantly improved, which improves its processability in applications such as casting and blown film, and is beneficial to its application in the fields of casting and blown film processing.
[0104] Table 2 Melt flow rate test results of some embodiments and comparative examples
[0105]
[0106] Table 3 shows the mechanical property test results of Examples 1, 3, and Comparative Examples 1-2. It can be seen from Table 3 that the tensile strength of Example 1, Example 3 and Comparative Example 2 is equivalent, but the elongation at break is significantly improved; compared with Comparative Example 1, the elongation at break and the tensile strength of Examples 1 and 3 are significantly increased, which proves that the mechanical properties of the polyglycolide polymer material obtained by the present invention are significantly improved compared with the polyglycolide homopolymer.
[0107] Table 3 Mechanical properties test results of some embodiments and comparative examples
[0108]
[0109] The preparation method of the polyglycolic acid polymer material in the present invention has high production efficiency, can realize continuous preparation on a twin-screw extruder, greatly reduces the reaction time, and shortens it from several hours in the prior art to within a few minutes, significantly saves energy consumption and reduces carbon emissions, overcomes the defects of high production cost and energy consumption caused by the slow polymerization reaction of polyglycolic acid in the prior art, and has extremely high promotion and application value.
Claims
1. A polyglycolide polymer material comprising a starch-polyglycolide graft copolymer and a polyglycolide homopolymer; The structural formula of the starch-polyglycolide graft copolymer is: in, R1, R2, and R3 are independently selected from hydrogen atoms or alkyl or aromatic hydrocarbon groups with a molecular weight of 15 to 1000 g / mol. a , R b are independently selected from a hydrogen atom or Where R x is R1, R2 or R3, p is an integer greater than 10, preferably an integer of 150 to 10000; n is greater than 50, preferably 60 to 10000; p1, p2, p3 are independently selected from integers greater than 10, preferably selected from integers of 150 to 10000; the starch and the polyglycolic acid side chains of the starch-polyglycolide graft copolymer are linked by ester bonds; The structural formula of the polyglycolide homopolymer is: Among them, M1, M2, ..., M i are the same or different, and are independently selected from imino, nitro or ether bonds, and R is a hydrogen atom or an alkane or aromatic hydrocarbon group with a molecular weight of 15 to 1000 g / mol; n1, n2, ..., n i are all integers not equal to 0, and n1, n2, ..., n i The sum is not less than 50, preferably 50-3000; i is an integer of 1-20, preferably an integer of 2-6.
2. The polyglycolide polymer material according to claim 1, characterized in that: The molecular weight distribution of the polyglycolide polymer material is a bimodal molecular weight distribution, preferably comprising an ultra-high molecular weight starch-polyglycolide graft copolymer peak and a polyglycolide homopolymer peak; Preferably, The weight average molecular weight M of the ultra-high molecular weight starch-polyglycolide graft copolymer peak w1 5.0×10 5 ~3.0×10 6 g / mol, preferably 8.0×10 5 ~2.0×10 6 g / mol; a molecular weight distribution index of 1.0 to 2.0, preferably 1.0 to 1.5; and / or, The weight average molecular weight M of the polyglycolide homopolymer peak w2 5.0×10 4 ~1.5×10 5 g / mol, preferably 1.0×10 5 ~1.5×10 5 g / mol; a molecular weight distribution index of 1.5 to 3.0, preferably 1.5 to 2.5; and / or, The weight average molecular weight M of the polyglycolide polymer material w 1.0×10 5 ~2.0×10 6 g / mol, preferably 1.0×10 5 ~3.0×10 5 g / mol; the molecular weight distribution index is 1.5 to 15.0, preferably 1.5 to 4.
0.
3. The polyglycolide polymer material according to claim 1, characterized in that: Taking the total mass of the polyglycolide polymer material as 100%, the mass content of the starch-polyglycolide graft copolymer is 1-50%, preferably 1-20%, and more preferably 4-15%; the mass content of the polyglycolide homopolymer is 50-99%, preferably 80-99%, and more preferably 85-96%.
4. The polyglycolide polymer material according to claim 1, characterized in that: The melt flow rate of the polyglycolide polymer material at 230° C. / 2.16 kg is not higher than 20 g / 10 min, preferably 3 to 20 g / 10 min.
5. The polyglycolide polymer material according to claim 1, characterized in that: The polyglycolide polymer material comprises starch, which can be polymerized to obtain polyglycolide chain segments. The raw materials are prepared from raw materials including monomers and catalysts; preferably, the raw materials also include at least one of a small molecule co-initiator and an antioxidant.
6. The polyglycolide polymer material according to claim 5, characterized in that: The starch is unmodified native starch or modified starch, preferably at least one of native corn starch, native cassava starch, native wheat starch, hydroxymethyl starch and hydroxyethyl starch; and / or, The polyglycolide chain segment can be polymerized The monomer is at least one of methyl glycolate, glycolic acid and glycolide; and / or, The catalyst is a salt compound of at least one metal of Group IIA-VA metal elements and transition metal elements or an organic guanidine catalyst, preferably, the catalyst is a salt compound of at least one of Sn, Bi, Mg, Al, Ca, Fe, Mn, Ti and Zn; and / or, The antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant; and / or, The small molecule co-initiator is a small molecule substance containing hydroxyl or amino groups with a boiling point greater than 160° C. and a molecular weight less than 1000 g / mol, preferably at least one of ethylene glycol, butanediol, propylene glycol, serinol, leucinol, pentaerythritol, sorbitol, xylitol, amino acids, phenol, hydroquinone, resorcinol, benzyl alcohol, aniline, benzylamine, and p-phenylenediamine.
7. The polyglycolide polymer material according to claim 5, characterized in that: The polyglycolide chain segment can be obtained by polymerization The monomers are 100 parts by mass and include the following raw materials:
8. A method for preparing the polyglycolide polymer material according to any one of claims 1 to 7, comprising: The amount includes the polyglycolide chain segment that can be polymerized The monomers and starch raw materials are subjected to melt polymerization reaction in the presence of a catalyst, and then cooled to obtain the polyglycolide polymer material; preferably, the raw materials also include at least one of a small molecule co-initiator and an antioxidant; Preferably, the temperature of the melt polymerization is 140 to 250° C., preferably 200 to 240° C.; the reaction time is 0.5 to 60 min, preferably 1 to 20 min, more preferably 3 to 6 min.
9. The preparation method according to claim 8, characterized in that: The melt polymerization reaction is carried out in a continuous melt mixing device; the melt polymerization reaction is preferably carried out in a continuous twin-screw extruder, more preferably in at least two continuous twin-screw extruders connected in series; Preferably, the processing conditions of the continuous twin-screw extruder include: The processing temperature is 140 to 250°C, preferably 200 to 240°C; and / or, The screw speed is 5 to 300 rpm, preferably 40 to 150 rpm; and / or, The aspect ratio is 25-80, preferably 25-70.
10. A polyglycolide polymer material obtained according to the preparation method of claim 8 or 9.
11. Use of the polyglycolide polymer material according to any one of claims 1 to 7 and 10 in plastic products, wherein the plastic products are preferably injection molded products, blown film products or cast film products.
Citation Information
Cited By
Method for preparing high molecular weight starch grafted polyester copolymer through reactive extrusion
CN120157850A