Impact-resistant heat-resistant polypropylene composite material and preparation process thereof

By introducing cage adamantane into polypropylene to form chemical bonds, the problem of insufficient wear, mechanical and heat resistance of polypropylene materials is solved, and higher impact and heat resistance are achieved, which enhances the Interaction forces and thermal stability of materials.

CN118994783AInactive Publication Date: 2024-11-22GUANGDONG BINGXIN NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411222288.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In actual applications, existing polypropylene materials have problems such as poor wear resistance, poor mechanical properties, easy aging and low heat resistance. The existing modification methods often reduce the rigidity and tensile strength of the material, or cause The agglomeration of inorganic nanoparticles has poor interface binding force.

Method used

By introducing rigid, highly symmetric cage-shaped adamantane into polypropylene, the isocyanate group in its structure uses chemical bonding to the hydroxyl group on the surface of nanosilicon dioxide to inhibit nanoparticle agglomeration, increase material compatibility, and Functionalized polypropylene materials are introduced to improve impact and heat resistance.

Benefits of technology

It significantly improves the impact resistance and heat resistance of polypropylene composite materials, enhances the interaction force between nano-silica and polypropylene, delays the thermal decomposition speed, and broadens the application range of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005023378210000051
    Figure BDA0005023378210000051
  • Figure BDA0005023378210000052
    Figure BDA0005023378210000052
  • Figure BDA0005023378210000101
    Figure BDA0005023378210000101
Patent Text Reader

Abstract

The invention relates to the technical field of polypropylene materials, and discloses an impact-resistant heat-resistant polypropylene composite material and a preparation process, double bonds of an imide group in a functionalized polypropylene material can be subjected to initiated polymerization with polypropylene, and an isocyanate group in the structure of the functionalized polypropylene material and hydroxyl on the surface of nano silicon dioxide form chemical bonding; the compatibility with polypropylene is increased, and adsorption bonding between the two is facilitated; the high-symmetry cage-shaped adamantane has rigidity and three-dimensional size stability, and is introduced into a polypropylene side chain to facilitate transmission of external stress, so that a larger load is borne, and the impact strength of the polypropylene composite material is improved; the polyhedral oligomeric adamantane and imide five-membered ring structure is excellent in high temperature resistance, rotation of a polypropylene chain can be hindered in the heating process, and movement of the material becomes difficult, so that the composite material has good heat resistance, and the application range of the polypropylene material is further widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polypropylene materials, in particular to an impact-resistant and heat-resistant polypropylene composite material and a preparation process. Background Art

[0002] Polypropylene (PP) is one of the five general-purpose plastics and has been widely used in various fields such as industry, agriculture, medical care, hygiene, packaging and daily life. It is widely used in various fields due to its low specific gravity, good performance, easy processing and molding, and low price. However, pure PP has defects such as poor wear resistance, poor mechanical properties, easy aging, and low heat resistance in practical applications. Some modifiers used in the prior art will reduce the impact performance of polypropylene materials, and the thermal decomposition temperature of the modified PP material is not high, and the heat resistance is poor. Therefore, it is urgent to develop a polypropylene composite material with excellent impact resistance and heat resistance.

[0003] The traditional method of toughening polypropylene is to add rubber elastomer to PP, but this will lead to a decrease in the rigidity and tensile strength of the material; although the use of inorganic nanomaterials to modify the polymer can improve the strength, due to the polarity difference between inorganic particles and polymer materials, inorganic nanoparticles are prone to agglomeration; therefore, it is necessary to modify the surface of the inorganic nanoparticles to promote their uniform dispersion in the polymer matrix and improve the interfacial interaction force; the invention patent CN111793277B pre-mixes polypropylene imine-modified nano-silica and polypropylene grafted maleic anhydride with polypropylene resin, and then obtains modified polypropylene by extrusion granulation. The polypropylene resin has good transparency, tensile strength and impact strength, but the improvement in heat resistance is limited, and there are many added components, which is not suitable for industrial production.

[0004] There are unsaturated Si-O bonds and hydroxyl groups on the surface of nano-silica, which can both toughen and strengthen PP, becoming a hot spot for PP modification. However, the polarity of silica and non-polar polypropylene materials is quite different, resulting in aggregation of silica nanoparticles, poor interface bonding, and heat resistance that needs to be further improved. Adamantane is a highly symmetrical and very stable compound. The present invention introduces rigid, highly symmetrical cage-like adamantane into the polypropylene chain segment, and utilizes the isocyanate group in its structure to produce chemical bonding with the hydroxyl group on the surface of nano-silica, which can inhibit the aggregation and bridging of nanoparticles, increase its compatibility with polypropylene, improve the impact resistance and heat resistance of polypropylene materials, and broaden the further application of polypropylene materials. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an impact-resistant and heat-resistant polypropylene composite material and a preparation process, thereby improving the heat resistance and impact resistance of the polypropylene material.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] An impact-resistant and heat-resistant polypropylene composite material comprises the following components in parts by weight: 100 parts of polypropylene, 3-15 parts of functionalized polypropylene material, 0.8-1.5 parts of antioxidant and 0.3-0.5 parts of light stabilizer.

[0008] The antioxidant is a hindered phenol antioxidant or a phosphite antioxidant.

[0009] The light stabilizer is a hindered amine light stabilizer.

[0010] The preparation process of functionalized polypropylene material is as follows: polypropylene particles and toluene are added into a high pressure reactor, after being stirred evenly, diisopropylbenzene peroxide and the structural formula The isocyanate-based adamantane, styrene and nano-silica are introduced with nitrogen, stirred and reacted at a speed of 600-800r / min. After the reaction is completed, they are dissolved in xylene, acetone is added for precipitation, and functionalized polypropylene material is obtained after drying.

[0011] Preferably, by weight, the polypropylene particles are 100 parts, the dicumyl peroxide is 3.5-6 parts, the isocyanate adamantane is 2-10 parts, the styrene is 3-5 parts, and the nano-silicon dioxide is 8-12 parts.

[0012] Preferably, the reaction temperature is 130-150° C., and the reaction time is 5-10 h.

[0013] Preferably, the preparation process of isocyanate-based adamantane is:

[0014] Step (1), under a nitrogen atmosphere, add 3-amino-1-adamantanol and toluene to a reaction flask, stir evenly, add maleic anhydride and triethylamine, stir to react, and after the reaction is completed, cool to room temperature, extract with dichloromethane and deionized water, concentrate the organic phase, purify by column chromatography, and dry to obtain maleimide adamantane alcohol.

[0015] Step (2), under a nitrogen atmosphere, add maleimide adamantane alcohol and N,N-dimethylformamide to a reaction flask, stir evenly, add 4-bromoisocyanate and sodium tert-butoxide, stir to react, after the reaction is completed, cool to room temperature, extract with ethyl acetate and deionized water, concentrate the organic phase, purify by column chromatography, and dry to obtain isocyanate adamantane.

[0016] Preferably, in step (1), the ratio of 3-amino-1-adamantanol, maleic anhydride and triethylamine is 1 mol: (1.05-1.2) mol: (1.3-1.5) mol.

[0017] Preferably, in step (1), the reaction temperature is 100-120° C. and the reaction time is 12-24 h.

[0018] Preferably, in step (2), the ratio of maleimide adamantane alcohol, 4-phenyl bromoisocyanate and sodium tert-butoxide is 1 mol: (1.1-1.3) mol: (1.5-2) mol.

[0019] Preferably, the reaction temperature is 60-80°C and the reaction time is 8-16h.

[0020] Preferably, 100 parts by weight of polypropylene, 3-15 parts by weight of functionalized polypropylene material, 0.8-1.5 parts by weight of antioxidant and 0.3-0.5 parts by weight of light stabilizer are added to a twin-screw extruder for melt mixing at a melt mixing temperature of 180-220° C. and a screw speed of 300-500 r / min. Extrusion, water cooling, pelletizing and injection molding are performed to obtain an impact-resistant and heat-resistant polypropylene composite material.

[0021] By adopting the above technical solution, the beneficial effects of the present invention are:

[0022] The invention firstly reacts 3-amino-1-adamantanol with maleic anhydride under the action of triethylamine to obtain maleimide adamantanol, and then reacts with 4-phenyl bromoisocyanate to obtain isocyanate-based adamantane, then utilizes the double bonds of the isocyanate-based adamantane to initiate polymerization with polypropylene and styrene, utilizes the isocyanate group of the isocyanate-based adamantane to bond with the hydroxyl group on the surface of silicon dioxide to obtain a functionalized polypropylene material, and finally blends and extrude with polypropylene and an antioxidant to obtain an impact-resistant and heat-resistant polypropylene composite material.

[0023] The double bond of the imide group in the functionalized polypropylene material can initiate polymerization with polypropylene, and the isocyanate group in its structure can chemically bond with the hydroxyl group on the surface of nano-silica to form a carbamate structure that can inhibit the agglomeration and bridging of nanoparticles and increase its compatibility with polypropylene, which is beneficial to the full adsorption and bonding of nano-silica and polypropylene, and enhances the interaction between the two; at the same time, the highly symmetrical cage-like diamond has rigidity and three-dimensional dimensional stability, and its introduction into the side chain of polypropylene is beneficial to the transmission of external stress, thereby bearing a larger load and improving the impact strength of the polypropylene composite material.

[0024] The thermal stability of nano-silicon dioxide is much higher than that of polypropylene, and it forms a chemical bond with the polypropylene matrix, forming a phase interface that limits the movement of the molecular chain, hindering the transfer of external heat to the polypropylene molecules, and slowing down the diffusion of gases produced by thermal decomposition from the matrix to the outside, thereby reducing the thermal decomposition rate; in addition, the functionalized polypropylene material contains cage-like adamantane and imide five-membered ring structures, which have excellent high temperature resistance. During the heating process, it will hinder the rotation of the polypropylene chain and make the movement of the material difficult, thereby making the polypropylene material have good heat resistance, further broadening the application range of polypropylene materials. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] 3-Amino-1-adamantanol, CAS number is 702-82-9.

[0027] 4-phenyl bromoisocyanate, CAS number is 2493-02-9.

[0028] Example 1

[0029] (1) Under nitrogen atmosphere, 65 mmol of 3-amino-1-adamantanol and 520 mL of toluene were added to a reaction flask, and after stirring, 75.4 mmol of maleic anhydride and 91 mmol of triethylamine were added, and the mixture was reacted at 110° C. for 16 h, cooled to room temperature, extracted with dichloromethane and deionized water, and the organic phase was concentrated and purified by column chromatography. The mobile system was ethyl acetate and petroleum ether in a volume ratio of 1:3, and dried to obtain maleimide adamantane alcohol. The preparation reaction formula is as follows:

[0030]

[0031] (2) Under nitrogen atmosphere, add 60 mmol of maleimide adamantane alcohol and 900 mL of N,N-dimethylformamide to the reaction flask, stir evenly, add 72 mmol of 4-bromoisocyanatophenyl ester and 99 mmol of sodium tert-butoxide, react at 70°C for 12 h, cool to room temperature, extract with ethyl acetate and deionized water, concentrate the organic phase, purify by column chromatography, the mobile system is methanol and dichloromethane with a volume ratio of 1:5, and dry to obtain isocyanate adamantane. The preparation reaction formula is as follows:

[0032]

[0033] (3) 100 g of polypropylene particles and 750 mL of toluene were added to a high-pressure reactor. After stirring evenly, 5 g of diisopropylbenzene peroxide, 2 g of isocyanate-based adamantane, 4 g of styrene and 10 g of nano-silica were added, nitrogen was introduced, and the mixture was reacted at a speed of 700 r / min and a temperature of 140°C for 8 h. After the reaction was completed, the mixture was dissolved in xylene, acetone was added for precipitation, and the functionalized polypropylene material was obtained after drying.

[0034] (4) 100 g of polypropylene, 3 g of functionalized polypropylene material, 1.2 g of hindered phenol antioxidant and 0.4 g of hindered amine light stabilizer were added into a twin-screw extruder for melt mixing. The melt mixing temperature was 200 °C and the screw speed was 450 r / min. The extrusion granulation was performed. The six-stage temperatures were 170 °C, 180 °C, 190 °C, 200 °C, 210 °C and 200 °C, respectively. The pelletization was performed by water cooling and injection molding. The temperatures of each stage were 165 °C, 180 °C, 200 °C and 195 °C, respectively, to obtain an impact-resistant and heat-resistant polypropylene composite material.

[0035] Example 2

[0036] (1) Under nitrogen atmosphere, 80 mmol of 3-amino-1-adamantanol and 400 mL of toluene were added to a reaction flask, and after stirring, 84 mmol of maleic anhydride and 104 mmol of triethylamine were added, and the mixture was reacted at 120° C. for 12 h. The mixture was cooled to room temperature, extracted with dichloromethane and deionized water, and the organic phase was concentrated with a mobile phase system of ethyl acetate and petroleum ether in a volume ratio of 1:3. After drying, maleimide adamantane alcohol was obtained.

[0037] (2) Under nitrogen atmosphere, 75 mmol of maleimide adamantane alcohol and 750 mL of N,N-dimethylformamide were added to a reaction flask, and after stirring, 82.5 mmol of 4-bromoisocyanatophenyl ester and 112.5 mmol of sodium tert-butoxide were added, and the mixture was reacted at 80° C. for 8 h. The mixture was cooled to room temperature, extracted with ethyl acetate and deionized water, and the organic phase was concentrated and purified by column chromatography using a mobile phase of methanol and dichloromethane in a volume ratio of 1:5. After drying, isocyanate adamantane was obtained.

[0038] (3) 100 g of polypropylene particles and 500 mL of toluene were added to a high-pressure reactor. After stirring evenly, 3.5 g of diisopropylbenzene peroxide, 4 g of isocyanate-based adamantane, 3 g of styrene and 8 g of nano-silica were added, nitrogen was introduced, and the mixture was reacted at a speed of 800 r / min and a temperature of 150°C for 5 h. After the reaction was completed, the mixture was dissolved in xylene, acetone was added for precipitation, and the functionalized polypropylene material was obtained after drying.

[0039] (4) 100 g of polypropylene, 6 g of functionalized polypropylene material, 0.8 g of phosphite antioxidant and 0.3 g of hindered amine light stabilizer were added into a twin-screw extruder for melt mixing. The melt mixing temperature was 220 °C and the screw speed was 500 r / min. The six-stage temperatures were 170 °C, 180 °C, 190 °C, 200 °C, 210 °C and 200 °C respectively. The pelletizing was carried out by water cooling and injection molding. The temperatures of each stage were 165 °C, 180 °C, 200 °C and 195 °C respectively. An impact-resistant and heat-resistant polypropylene composite material was obtained.

[0040] Example 3

[0041] (1) Under nitrogen atmosphere, 35 mmol of 3-amino-1-adamantanol and 350 mL of toluene were added to a reaction flask, and after stirring, 42 mmol of maleic anhydride and 52.5 mmol of triethylamine were added, and the mixture was reacted at 100° C. for 24 h. The mixture was cooled to room temperature, extracted with dichloromethane and deionized water, and the organic phase was concentrated and purified by column chromatography with a mobile phase of ethyl acetate and petroleum ether in a volume ratio of 1:3. Maleimide adamantane alcohol was obtained after drying.

[0042] (2) Under nitrogen atmosphere, 30 mmol of maleimide adamantane alcohol and 600 mL of N,N-dimethylformamide were added to a reaction flask, and after stirring, 39 mmol of 4-bromoisocyanatophenyl ester and 60 mmol of sodium tert-butoxide were added, and the mixture was reacted at 60° C. for 16 h. The mixture was cooled to room temperature, extracted with ethyl acetate and deionized water, and the organic phase was concentrated and purified by column chromatography. The mobile phase was methanol and dichloromethane in a volume ratio of 1:5. After drying, isocyanate adamantane was obtained.

[0043] (3) 100 g of polypropylene particles and 800 mL of toluene were added to a high-pressure reactor. After stirring evenly, 6 g of diisopropylbenzene peroxide, 6 g of isocyanate-based adamantane, 5 g of styrene and 12 g of nano-silica were added, nitrogen was introduced, and the mixture was reacted at a speed of 600 r / min and a temperature of 130°C for 10 h. After the reaction was completed, the mixture was dissolved in xylene, acetone was added for precipitation, and the functionalized polypropylene material was obtained after drying.

[0044] (4) Add 100 g of polypropylene, 9 g of functionalized polypropylene material, 1.5 g of hindered phenol antioxidant and 0.5 g of hindered amine light stabilizer into a twin-screw extruder for melt mixing at a melt mixing temperature of 180 ° C and a screw speed of 300 r / min. Extrusion granulation with six temperature sections of 170 ° C, 180 ° C, 190 ° C, 200 ° C, 210 ° C and 200 ° C respectively. Water-cooled pelletizing and injection molding with the temperature of each section of 165 ° C, 180 ° C, 200 ° C and 195 ° C respectively are performed to obtain an impact-resistant and heat-resistant polypropylene composite material.

[0045] Example 4

[0046] (1) Under nitrogen atmosphere, 42 mmol of 3-amino-1-adamantanol and 355 mL of toluene were added to a reaction flask, and after stirring, 48.3 mmol of maleic anhydride and 56.6 mmol of triethylamine were added, and the mixture was reacted at 115° C. for 15 h. The mixture was cooled to room temperature, extracted with dichloromethane and deionized water, and the organic phase was concentrated with a mobile phase system of ethyl acetate and petroleum ether in a volume ratio of 1:3. The mixture was dried to obtain maleimide adamantanol.

[0047] (2) Under nitrogen atmosphere, 35 mmol of maleimide adamantane alcohol and 630 mL of N,N-dimethylformamide were added to a reaction flask, and after stirring, 40.6 mmol of 4-bromoisocyanatophenyl ester and 56 mmol of sodium tert-butoxide were added, and the mixture was reacted at 65° C. for 12 h. The mixture was cooled to room temperature, extracted with ethyl acetate and deionized water, and the organic phase was concentrated and purified by column chromatography. The mobile phase was methanol and dichloromethane in a volume ratio of 1:5. After drying, isocyanate adamantane was obtained.

[0048] (3) 100 g of polypropylene particles and 650 mL of toluene were added to a high-pressure reactor. After stirring evenly, 5.5 g of diisopropylbenzene peroxide, 8 g of isocyanate-based adamantane, 4.5 g of styrene and 10 g of nano-silica were added, and nitrogen was introduced. The mixture was reacted at a speed of 700 r / min and a temperature of 135°C for 9 h. After the reaction was completed, the mixture was dissolved in xylene, acetone was added for precipitation, and the functionalized polypropylene material was obtained after drying.

[0049] (4) 100 g of polypropylene, 12 g of functionalized polypropylene material, 1.1 g of phosphite antioxidant and 0.35 g of hindered amine light stabilizer were added into a twin-screw extruder for melt mixing. The melt mixing temperature was 190 ° C and the screw speed was 450 r / min. The six-stage temperatures were extruded and granulated at 170 ° C, 180 ° C, 190 ° C, 200 ° C, 210 ° C and 200 ° C, respectively. Water-cooled pelletizing and injection molding were performed. The temperatures of each stage were 165 ° C, 180 ° C, 200 ° C and 195 ° C, respectively, to obtain an impact-resistant and heat-resistant polypropylene composite material.

[0050] Example 5

[0051] (1) Under nitrogen atmosphere, 25 mmol of 3-amino-1-adamantanol and 205 mL of toluene were added to a reaction flask, and after stirring, 29 mmol of maleic anhydride and 35.5 mmol of triethylamine were added, and the mixture was reacted at 120° C. for 16 h. The mixture was cooled to room temperature, extracted with dichloromethane and deionized water, and the organic phase was concentrated and purified by column chromatography. The dry mobile phase was ethyl acetate and petroleum ether in a volume ratio of 1:3. Maleimide adamantane alcohol was obtained after drying.

[0052] (2) Under nitrogen atmosphere, 20 mmol of maleimide adamantane alcohol and 320 mL of N,N-dimethylformamide were added to a reaction flask, and after stirring, 25 mmol of 4-bromoisocyanatophenyl ester and 33.6 mmol of sodium tert-butoxide were added, and the mixture was reacted at 75° C. for 12 h. The mixture was cooled to room temperature, extracted with ethyl acetate and deionized water, and the organic phase was concentrated and purified by column chromatography. The mobile phase was methanol and dichloromethane in a volume ratio of 1:5. After drying, isocyanate adamantane was obtained.

[0053] (3) 100 g of polypropylene particles and 700 mL of toluene were added to a high-pressure reactor. After stirring evenly, 5 g of diisopropylbenzene peroxide, 10 g of isocyanate-based adamantane, 5 g of styrene and 12 g of nano-silica were added, nitrogen was introduced, and the reaction was carried out at a speed of 720 r / min and a temperature of 145°C for 9 h. After the reaction was completed, it was dissolved in xylene, acetone was added for precipitation, and functionalized polypropylene material was obtained after drying.

[0054] (4) 100 g of polypropylene, 15 g of functionalized polypropylene material, 1.2 g of hindered phenol antioxidant and 0.5 g of hindered amine light stabilizer were added into a twin-screw extruder for melt mixing. The melt mixing temperature was 200 °C and the screw speed was 400 r / min. The six-stage temperatures of extrusion granulation were 170 °C, 180 °C, 190 °C, 200 °C, 210 °C and 200 °C, respectively. Water-cooled pelletizing and injection molding were performed. The temperatures of each stage were 165 °C, 180 °C, 200 °C and 195 °C, respectively, to obtain an impact-resistant and heat-resistant polypropylene composite material.

[0055] Comparative Example 1

[0056] (1) 100 g of polypropylene particles and 750 mL of toluene were added to a high-pressure reactor, and after being stirred evenly, 5 g of diisopropylbenzene peroxide, 2 g of isocyanate-based adamantane (prepared in Example 1), 4 g of styrene and 10 g of nano-silicon dioxide were added, and nitrogen was introduced. The reaction was carried out at a speed of 700 r / min and a temperature of 140° C. for 8 h. After the reaction was completed, the mixture was dissolved in xylene, acetone was added for precipitation, and the modified polypropylene material was obtained after drying.

[0057] (2) 100 g of polypropylene, 3 g of modified polypropylene material, 1.2 g of hindered phenol antioxidant and 0.4 g of hindered amine light stabilizer were added into a twin-screw extruder for melt mixing. The melt mixing temperature was 200 °C and the screw speed was 450 r / min. The six-stage temperatures of extrusion granulation were 170 °C, 180 °C, 190 °C, 200 °C, 210 °C and 200 °C, respectively. The pelletization was carried out by water cooling and injection molding. The temperatures of each stage were 165 °C, 180 °C, 200 °C and 195 °C, respectively, to obtain a polypropylene composite material.

[0058] Comparative Example 2

[0059] (1) 100 g of polypropylene particles and 750 mL of toluene were added to a high-pressure reactor, and after being stirred evenly, 5 g of diisopropylbenzene peroxide, 2 g of maleic anhydride, 4 g of styrene and 10 g of nano-silicon dioxide were added, and nitrogen was introduced. The reaction was carried out at a speed of 700 r / min and a temperature of 140° C. for 8 h. After the reaction was completed, the mixture was dissolved in xylene, acetone was added for precipitation, and the modified polypropylene material was obtained after drying.

[0060] (2) 100 g of polypropylene, 3 g of modified polypropylene material, 1.2 g of hindered phenol antioxidant and 0.4 g of hindered amine light stabilizer were added into a twin-screw extruder for melt mixing. The melt mixing temperature was 200 °C and the screw speed was 450 r / min. The six-stage temperatures of extrusion granulation were 170 °C, 180 °C, 190 °C, 200 °C, 210 °C and 200 °C, respectively. The pelletization was carried out by water cooling and injection molding. The temperatures of each stage were 165 °C, 180 °C, 200 °C and 195 °C, respectively, to obtain a polypropylene composite material.

[0061] Comparative Example 3

[0062] 100g of polypropylene, 1.2g of hindered phenol antioxidant and 0.4g of hindered amine light stabilizer were added into a twin-screw extruder for melt mixing. The melt mixing temperature was 200°C and the screw speed was 450r / min. The six-stage temperatures of extrusion granulation were 170°C, 180°C, 190°C, 200°C, 210°C and 200°C, respectively. The pelletizing was carried out by water cooling and injection molding. The temperatures of each stage were 165°C, 180°C, 200°C and 195°C, respectively, to obtain a polypropylene material.

[0063] Tensile performance test: The tensile strength test of polypropylene was carried out according to GB / T 1040-2006, and the tensile rate was 50 mm / min.

[0064] Impact strength test: refer to GB / T 1843-2008 polypropylene for impact performance test. When the specimen to be tested is broken or fractured under the action of impact load, the energy absorbed by the unit cross-sectional area is tested.

[0065] Table 1 Mechanical properties test

[0066]

[0067] It can be seen from the test results in the above table that as the content of functionalized polypropylene material increases, the mechanical properties of the polypropylene composite material gradually increase, and the impact strength in Example 5 reaches 65.17 kJ / m 2The tensile strength and tensile modulus are significantly increased. This is because the double bond of the imide group in the functionalized polypropylene material initiates polymerization with polypropylene, and the isocyanate group in its structure is chemically bonded with the hydroxyl group on the surface of the nano-silica to form a carbamate structure, which can inhibit the aggregation and bridging of the nanoparticles and increase its compatibility with polypropylene, which is beneficial to the full adsorption and bonding of nano-silica and polypropylene, and enhances the interaction between the two. At the same time, the highly symmetrical cage-like adamantane has rigidity and three-dimensional dimensional stability, which is introduced into the side chain of polypropylene, which is beneficial to the transmission of external stress, thereby bearing a larger load and improving the impact strength of the polypropylene composite material.

[0068] Comparative Example 1 does not contain an isocyanate group and cannot form a chemical bond with nano-silica, resulting in poor dispersion of the nanoparticles and affected mechanical properties; Comparative Example 2 does not contain a rigid adamantane structure, but the introduced maleic anhydride can form a bond with nano-silica, thereby improving the compatibility with the polypropylene material and improving the mechanical properties to a certain extent; Comparative Example 3 is a pure polypropylene material with poor impact resistance and the worst mechanical properties.

[0069] Thermal performance test: In a nitrogen atmosphere, the test was carried out using a thermogravimetric analyzer with a heating rate of 10°C / min and a test temperature range of 25-700°C.

[0070] Table 2 Heat resistance test

[0071]

[0072] It can be seen from the test results in the above table that with the increase of the content of the functionalized polypropylene material, the heat resistance of the polypropylene composite material is gradually enhanced. The initial decomposition temperature of Example 4 is 379.5°C, and the maximum rate decomposition temperature is 481.2°C, which is significantly improved compared with the comparative example. This is because, on the one hand, the thermal stability of nano-silicon dioxide is much higher than that of polypropylene, and chemical bonding is generated between the nano-silicon dioxide and the polypropylene matrix, forming a phase interface that limits the movement of the molecular chain, hindering the transfer of external heat to the polypropylene molecules, and slowing down the diffusion of gases generated by thermal decomposition from the matrix to the outside, so that the thermal decomposition rate is reduced; on the other hand, the functionalized polypropylene material contains cage-like adamantane and imide five-membered ring structure, which has excellent high temperature resistance. During the heating process, the rotation of the polypropylene chain will be hindered, making the movement of the material difficult, so that the polypropylene material has good heat resistance.

[0073] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. An impact-resistant and heat-resistant polypropylene composite material, characterized in that: The polypropylene composite material comprises the following components in parts by weight: 100 parts of polypropylene, 3-15 parts of functionalized polypropylene material, 0.8-1.5 parts of antioxidant and 0.3-0.5 parts of light stabilizer; The antioxidant is a hindered phenol antioxidant or a phosphite antioxidant; The light stabilizer is a hindered amine light stabilizer; The preparation process of the functionalized polypropylene material is as follows: adding polypropylene particles and toluene into a high-pressure reactor, stirring evenly, adding diisopropylbenzene peroxide and a structural formula of The isocyanate-based adamantane, styrene and nano-silica are introduced with nitrogen, stirred and reacted at a speed of 600-800r / min. After the reaction is completed, they are dissolved in xylene, acetone is added for precipitation, and functionalized polypropylene material is obtained after drying.

2. The impact-resistant and heat-resistant polypropylene composite material according to claim 1, characterized in that: In terms of weight, the polypropylene particles are 100 parts, the dicumyl peroxide is 3.5-6 parts, the isocyanate-based adamantane is 2-10 parts, the styrene is 3-5 parts, and the nano-silicon dioxide is 8-12 parts.

3. The impact-resistant and heat-resistant polypropylene composite material according to claim 1, characterized in that: The reaction temperature is 130-150° C., and the reaction time is 5-10 h.

4. The impact-resistant and heat-resistant polypropylene composite material according to claim 1, characterized in that: The preparation process of the isocyanate-based adamantane is as follows: Step (1), under a nitrogen atmosphere, add 3-amino-1-adamantanol and toluene to a reaction flask, stir evenly, add maleic anhydride and triethylamine, stir to react, and after the reaction is completed, cool to room temperature, extract with dichloromethane and deionized water, concentrate the organic phase, purify by column chromatography, and dry to obtain maleimide adamantanol; Step (2), under a nitrogen atmosphere, add maleimide adamantane alcohol and N,N-dimethylformamide to a reaction flask, stir evenly, add 4-bromoisocyanate and sodium tert-butoxide, stir to react, after the reaction is completed, cool to room temperature, extract with ethyl acetate and deionized water, concentrate the organic phase, purify by column chromatography, and dry to obtain isocyanate adamantane.

5. The impact-resistant and heat-resistant polypropylene composite material according to claim 4, characterized in that: In the step (1), the ratio of 3-amino-1-adamantanol, maleic anhydride and triethylamine is 1 mol: (1.05-1.2) mol: (1.3-1.5) mol.

6. The impact-resistant and heat-resistant polypropylene composite material according to claim 4, characterized in that: In the step (1), the reaction temperature is 100-120° C. and the reaction time is 12-24 h.

7. The impact-resistant and heat-resistant polypropylene composite material according to claim 4, characterized in that: In the step (2), the ratio of maleimide adamantane alcohol, 4-phenyl bromoisocyanate and sodium tert-butoxide is 1 mol: (1.1-1.3) mol: (1.5-2) mol.

8. The impact-resistant and heat-resistant polypropylene composite material according to claim 4, characterized in that: The reaction temperature is 60-80°C, and the reaction time is 8-16h.

9. A process for preparing the impact-resistant and heat-resistant polypropylene composite material according to any one of claims 1 to 8, characterized in that: 100 parts by weight of polypropylene, 3-15 parts by weight of functionalized polypropylene material, 0.8-1.5 parts by weight of antioxidant and 0.3-0.5 parts by weight of light stabilizer are added into a twin-screw extruder for melt mixing at a melt mixing temperature of 180-220° C. and a screw speed of 300-500 r / min. The product is extruded, water cooled, pelletized and injection molded to obtain an impact-resistant and heat-resistant polypropylene composite material.

Citation Information

Patent Citations

  • Silicon rubber / polyolefin thermoplastic elastomer with sliding cross-linked network

    CN109796767A

  • Impact-resistant and heat-resistant polypropylene composite material and preparation method thereof

    CN117946479A

  • Photocurable resin, photocurable resin composition, method of forming fine concave-convex pattern, transfer foil, optical article, and stamper

    JP2004059822A

  • Heat-resistant adhesive resin, heat-resistant adhesive composition, and adhesive, laminate, and bonding method employing the same

    JP2017122157A

Cited By

  • Toughened modified PBT (polybutylene terephthalate) and processing method thereof

    CN119286207A

  • High-flame-retardant automotive interior material and preparation method thereof

    CN120554760A

  • High-temperature-resistant polypropylene composite material and preparation method thereof

    CN121021972A

  • Synergistic modified photo-thermal aging resistant polypropylene composite material and preparation method thereof

    CN122608973A