Optical pressure-sensitive adhesive for polycarbonate type diffusion plate and preparation method of optical pressure-sensitive adhesive
Through the preparation of solvent-free polycarbonate optical pressure-sensitive adhesive, the problems of low light transmittance and insufficient bonding fastness in OLED products are solved, and high light transmittance and good adhesive performance are achieved. Suitable for assembly of functional PC diffusion plates.
Patent Information
- Application Number
- CN202411266357.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing pressure-sensitive adhesives are low in light transmittance, insufficient fit fastness, and many bubble defects in OLED products, which cannot meet the requirements for the use of polycarbonate diffusion plates, especially in the case of increasing assembly demand for functional PC diffusion plates. Down.
The preparation method of solvent-free polycarbonate type optical pressure-sensitive adhesive is adopted, and the ultraviolet light is irradiated with butyl acrylate, isooctyl acrylate, methyl methacrylate, hydroxyl-containing functional monomer, internal crosslinking monomer and photoinitiator under ultraviolet light. The polymerization reaction was carried out to form a prepolymer with high light transmittance and high viscosity, and the optical pressure-sensitive adhesive for polycarbonate diffusion plate was obtained by cross-linking and curing.
It achieves a light transmittance of more than 90%, has good initial viscosity, peeling force and retention force, and has good weather resistance and high and low temperature resistance. It is suitable for the bonding application of polycarbonate diffusion plates.
Smart Images

Figure BDA0005037586980000011 
Figure BDA0005037586980000021 
Figure BDA0005037586980000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of synthesis of acrylic ester pressure-sensitive adhesives, in particular to an optical pressure-sensitive adhesive for a polycarbonate type diffusion plate and a preparation method thereof. Background Art
[0002] In order to better meet the energy-saving and environmental protection concepts and visual effect innovation advocated by social development, the product update and iteration speed in the field of high-definition and high-color OLED has accelerated, which in turn puts forward higher requirements for the materials used in OLED. Traditional polymer materials such as polyethylene terephthalate (PET) and polystyrene (PS) can no longer meet the performance requirements of existing OLED products. The emergence of polycarbonate (PC) diffuser plates provides a new idea for the development of OLED. However, with the upgrading of products, the demand for functionalized PC diffuser plates is increasing, and it is necessary to assemble diffuser plates with different functions together to give composite materials more functions. Using pressure-sensitive adhesive to bond PC diffuser plates with different functions together is a good solution. However, the existing pressure-sensitive adhesive has problems such as low transmittance, insufficient bonding fastness, and many bubble defects during use. The pressure-sensitive adhesive currently produced in China cannot meet the use requirements of PC diffusion films. Therefore, the development of a solvent-free, green and environmentally friendly optical pressure-sensitive adhesive for polycarbonate diffuser plates that can be fully localized and its preparation method is a technical problem that needs to be solved at present. Summary of the invention
[0003] The object of the present invention is to provide an optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof, so as to solve the above technical problems.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides an optical pressure-sensitive adhesive for a polycarbonate diffuser plate, which is prepared from raw materials containing the following parts by mass:
[0006]
[0007]
[0008] Furthermore, the hydroxyl functional monomer comprises hydroxyethyl acrylate and / or hydroxyethyl methacrylate.
[0009] Furthermore, the internal crosslinking monomer comprises 1,6-hexanediol diacrylate and / or ethoxylated trimethylolpropane triacrylate.
[0010] Furthermore, the photoinitiator comprises one or more of 1-hydroxycyclohexyl benzophenone, 2-hydroxy-2-methyl-1-phenylpropanone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0011] Furthermore, the active amine monomer comprises one or more of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone and 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone.
[0012] The present invention also provides a method for preparing an optical pressure-sensitive adhesive for a polycarbonate diffuser plate, comprising the following steps:
[0013] 1) mixing butyl acrylate, isooctyl acrylate, methyl methacrylate, acrylic acid, hydroxyl functional monomer, internal crosslinking monomer, part of photoinitiator and active amine monomer under the protection of nitrogen to obtain a mixture;
[0014] 2) subjecting the mixture to a polymerization reaction under ultraviolet light to obtain a prepolymer;
[0015] 3) The prepolymer and the remaining photoinitiator are mixed and cross-linked and cured under light to obtain an optical pressure-sensitive adhesive for a polycarbonate diffuser plate.
[0016] Furthermore, the part of the photoinitiator accounts for 40-50% of the total amount of the photoinitiator.
[0017] Furthermore, the conditions of the ultraviolet irradiation are: the irradiation wavelength is 245 to 380 nm, the irradiation distance is 1 to 10 cm, and the irradiation time is 3 to 8 min.
[0018] Furthermore, in step 3), the main wavelength of the illumination is 365 nm, and the intensity of the illumination is 20 to 30 mW / cm 2 The illumination time is 20 to 30 seconds.
[0019] Beneficial effects of the present invention:
[0020] The optical pressure-sensitive adhesive of the present invention has a simple synthesis process, is a solvent-free green environmentally friendly adhesive, has a light transmittance of more than 90%, is simple and easy to use, has good initial adhesion, peeling force and holding force, and also has good weather resistance, high and low temperature resistance, etc. DETAILED DESCRIPTION
[0021] The present invention provides an optical pressure-sensitive adhesive for a polycarbonate diffuser plate, which is prepared from raw materials containing the following parts by mass:
[0022]
[0023] In the present invention, the content of butyl acrylate is preferably 38 to 52 parts by mass, more preferably 40 to 50 parts, and even more preferably 42 to 48 parts.
[0024] In the present invention, the content of isooctyl acrylate is preferably 25 to 35 parts by mass, more preferably 28 to 32 parts, and even more preferably 30 parts.
[0025] In the present invention, the content of methyl methacrylate is preferably 8 to 12 parts by mass, more preferably 9 to 11 parts, and even more preferably 10 parts.
[0026] In the present invention, the content of the acrylic acid is preferably 3 to 5 parts by mass, and more preferably 4 parts by mass.
[0027] In the present invention, the content of the hydroxyl functional monomer is preferably 2 parts by mass.
[0028] In the present invention, the content of the internal crosslinking monomer is preferably 0.2 to 0.8 parts by mass, more preferably 0.4 to 0.6 parts, and more preferably 0.5 parts.
[0029] In the present invention, the content of the photoinitiator is preferably 0.5 to 2.0 parts by mass, more preferably 0.8 to 1.8 parts, and more preferably 1.0 to 1.5 parts.
[0030] In the present invention, the content of the active amine monomer is preferably 0.5 to 2.2 parts by mass, more preferably 1.0 to 2.0 parts, and more preferably 1.2 to 1.8 parts.
[0031] In the present invention, the hydroxyl functional monomer comprises hydroxyethyl acrylate and / or hydroxyethyl methacrylate, preferably hydroxyethyl acrylate.
[0032] In the present invention, the internal crosslinking monomer comprises 1,6-hexanediol diacrylate and / or ethoxylated trimethylolpropane triacrylate, preferably 1,6-hexanediol diacrylate.
[0033] In the present invention, the photoinitiator comprises one or more of 1-hydroxycyclohexyl benzophenone, 2-hydroxy-2-methyl-1-phenylpropanone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide, preferably 2-hydroxy-2-methyl-1-phenylpropanone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide are compounded in a mass ratio of 1:1.
[0034] In the present invention, the active amine monomer comprises one or more of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone and 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, preferably 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone.
[0035] The present invention also provides a method for preparing an optical pressure-sensitive adhesive for a polycarbonate diffuser plate, comprising the following steps:
[0036] 1) mixing butyl acrylate, isooctyl acrylate, methyl methacrylate, acrylic acid, hydroxyl functional monomer, internal crosslinking monomer, part of photoinitiator and active amine monomer under the protection of nitrogen to obtain a mixture;
[0037] 2) subjecting the mixture to a polymerization reaction under ultraviolet light to obtain a prepolymer;
[0038] 3) The prepolymer and the remaining photoinitiator are mixed and cross-linked and cured under light to obtain an optical pressure-sensitive adhesive for a polycarbonate diffuser plate.
[0039] In the present invention, the part of the photoinitiator accounts for 40-50% of the total amount of the photoinitiator, preferably 50%.
[0040] In the present invention, the conditions of ultraviolet irradiation are: irradiation wavelength is 245-380nm, irradiation distance is 1-10cm, and irradiation time is 3-8min.
[0041] In the present invention, in step 3), the main wavelength of the illumination is 365nm, and the intensity of the illumination is 20-30mW / cm 2 , preferably 20 mW / cm 2 The illumination time is 20 to 30 seconds, preferably 25 seconds.
[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] Example 1
[0044] An optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof, comprising the following steps:
[0045] (1) 55 parts of butyl acrylate, 20 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 3 parts of acrylic acid, 3 parts of 2-hydroxyethyl acrylate, 1 part of 1,6-diacrylate, 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 15 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 180 r / min.
[0046] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 245nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 8cm. The irradiation time is controlled to be 5min. When the system viscosity reaches 2500cps (25°C), the prepolymer preparation is completed.
[0047] (3) After the prepolymer is prepared, add 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, stir evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500μm), control the thickness of the dry glue to 25μm, and then laminate it with a polycarbonate diffusion film (thickness is 100μm), and use a high-pressure mercury lamp at a main wavelength of 365nm and an intensity of 20mW / cm 2 Irradiate for 20 s to make the colloid cross-link and solidify again.
[0048] Example 2
[0049] An optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof, comprising the following steps:
[0050] (1) 54 parts of butyl acrylate, 21 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 3 parts of acrylic acid, 3 parts of 2-hydroxyethyl methacrylate, 1 part of 1,6-diacrylate, 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part of 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl) were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 10 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 160 r / min.
[0051] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 380nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 9cm. The irradiation time is controlled to be 7min. When the system viscosity reaches 2500cps (25°C), the prepolymer preparation is completed.
[0052] (3) After the prepolymer is prepared, add 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, stir evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500μm), control the thickness of the dry glue to 25μm, and then laminate it with a polycarbonate diffusion film (thickness is 100μm), and use a high-pressure mercury lamp at a main wavelength of 365nm and an intensity of 20mW / cm 2 Irradiate for 25 seconds to make the colloid cross-link and solidify again.
[0053] Example 3
[0054] An optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof, comprising the following steps:
[0055] (1) 53 parts of butyl acrylate, 23 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 3 parts of acrylic acid, 3 parts of 2-hydroxyethyl methacrylate, 1 part of ethoxylated trimethylolpropane triacrylate, 0.8 parts of 2-hydroxy-2-methyl-1-phenylpropanone and 1.2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 10 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 160 r / min.
[0056] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 365nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 8cm. The irradiation time is controlled to be 6min. When the system viscosity reaches 2500cps (25°C), the prepolymer preparation is completed.
[0057] (3) After the prepolymer is prepared, add 1 part of 2-hydroxy-2-methyl-1-phenylacetone, stir evenly and put into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500 μm), control the thickness of the dry glue to 25 μm, and then laminate it with a polycarbonate diffusion film (thickness is 100 μm), and use a high-pressure mercury lamp at a main wavelength of 365 nm and an intensity of 20 mW / cm 2Irradiate for 25 seconds to make the colloid cross-link and solidify again.
[0058] Example 4
[0059] An optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof, comprising the following steps:
[0060] (1) 53 parts of butyl acrylate, 23 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 3 parts of acrylic acid, 3 parts of 2-hydroxyethyl methacrylate, 1 part of ethoxylated trimethylolpropane triacrylate, 0.8 parts of 1-hydroxycyclohexyl benzophenone and 1.2 parts of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 10 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 160 r / min.
[0061] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 280nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 8cm. The irradiation time is controlled to be 6min. When the system viscosity reaches 2500cps (25°C), the prepolymer preparation is completed.
[0062] (3) After the prepolymer is prepared, add 1 part of 1-hydroxycyclohexyl benzophenone, stir evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500 μm), control the thickness of the dry glue to 25 μm, and then laminate it with a polycarbonate diffusion film (thickness is 100 μm), and use a high-pressure mercury lamp at a main wavelength of 365 nm and an intensity of 20 mW / cm 2 Irradiate for 25 seconds to make the colloid cross-link and solidify again.
[0063] Example 5
[0064] An optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof, comprising the following steps:
[0065] (1) 55 parts of butyl acrylate, 20 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 3 parts of acrylic acid, 3 parts of 2-hydroxyethyl methacrylate, 1 part of ethoxylated trimethylolpropane triacrylate, 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 15 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 180 r / min.
[0066] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 320nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 8cm. The irradiation time is controlled to be 5min. When the system viscosity reaches 2500cps (25°C), the prepolymer preparation is completed.
[0067] (3) After the prepolymer is prepared, add 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, stir evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500μm), control the thickness of the dry glue to 25μm, and then laminate it with a polycarbonate diffusion film (thickness is 100μm), and use a high-pressure mercury lamp at a main wavelength of 365nm and an intensity of 20mW / cm 2 Irradiate for 20 s to make the colloid cross-link and solidify again.
[0068] Example 6
[0069] An optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof, comprising the following steps:
[0070] (1) 50 parts of butyl acrylate, 25 parts of isooctyl acrylate, 13 parts of methyl methacrylate, 4 parts of acrylic acid, 4 parts of 2-hydroxyethyl acrylate, 1 part of 1,6-diacrylate, 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 15 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 180 r / min.
[0071] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 245nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 7cm. The irradiation time is controlled to be 8min. When the system viscosity reaches 3000cps (25°C), the prepolymer preparation is completed.
[0072] (3) After the prepolymer is prepared, add 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, stir evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500μm), control the thickness of the dry glue to 25μm, and then laminate it with a polycarbonate diffusion film (thickness is 100μm), and use a high-pressure mercury lamp at a main wavelength of 365nm and an intensity of 20mW / cm 2Irradiate for 25 seconds to make the colloid cross-link and solidify again.
[0073] Comparative Example 1
[0074] (1) 55 parts of butyl acrylate, 21 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 3 parts of acrylic acid, 3 parts of 2-hydroxyethyl methacrylate, 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 15 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 180 r / min.
[0075] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 245nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 8cm. The irradiation time is controlled to be 5min. When the system viscosity reaches 2500cps (25°C), the prepolymer preparation is completed.
[0076] (3) After the prepolymer is prepared, add 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, stir evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500μm), control the thickness of the dry glue to 25μm, and then laminate it with a polycarbonate diffusion film (thickness is 100μm), and use a high-pressure mercury lamp at a main wavelength of 365nm and an intensity of 20mW / cm 2 Irradiate for 20 s to make the colloid cross-link and solidify again.
[0077] Comparative Example 2
[0078] (1) 55 parts of butyl acrylate, 20 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 4 parts of acrylic acid, 3 parts of 2-hydroxyethyl methacrylate, 1 part of ethoxylated trimethylolpropane triacrylate, and 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 15 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 180 r / min.
[0079] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 245nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 8cm. The irradiation time is controlled to be 5min. When the system viscosity reaches 2500cps (25°C), the prepolymer preparation is completed.
[0080] (3) After the prepolymer is prepared, add 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, stir evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500μm), control the thickness of the dry glue to 25μm, and then laminate it with a polycarbonate diffusion film (thickness is 100μm), and use a high-pressure mercury lamp at a main wavelength of 365nm and an intensity of 20mW / cm 2 Irradiate for 20 s to make the colloid cross-link and solidify again.
[0081] Comparative Example 3
[0082] (1) 55 parts of butyl acrylate, 20 parts of isooctyl acrylate, 15 parts of methyl methacrylate, 3 parts of acrylic acid, 3 parts of 2-hydroxyethyl methacrylate, 1 part of ethoxylated trimethylolpropane triacrylate, 1 part of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone were respectively placed in a flask with nitrogen protection, and the mixture was rapidly stirred for 30 minutes under nitrogen protection to fully mix the raw materials, wherein the stirring speed was 180 r / min.
[0083] (2) After the raw materials are evenly mixed, the transparent reaction container is irradiated with a UVLED device to cause the monomer raw materials in the container to undergo polymerization under the condition of ultraviolet light with a wavelength of 245nm. During this period, the stirring speed is controlled to be 180r / min, and the distance between the light source and the reaction container is controlled to be 8cm. The irradiation time is controlled to be 2min. When the system viscosity reaches 1500cps (25°C), the prepolymer preparation is completed.
[0084] (3) After the prepolymer is prepared, stir it evenly and put it into a light-proof container for later use. When using, evenly apply the prepolymer on a polycarbonate diffusion plate (plate thickness is 1500μm), control the thickness of the dry glue to 25μm, and then laminate it with a polycarbonate diffusion film (thickness is 100μm), and use a high-pressure mercury lamp at a main wavelength of 365nm and an intensity of 20mW / cm 2 Irradiate for 20 s to make the colloid cross-link and solidify again.
[0085] The optical pressure-sensitive adhesives obtained in the examples and comparative examples were tested for performance, and the results are shown in Table 1 below.
[0086] Table 1 Performance test results
[0087]
[0088] It can be seen from the above embodiments that the present invention provides an optical pressure-sensitive adhesive for a polycarbonate diffuser plate and a preparation method thereof. Through the example results, it is found that the preparation process of the optical pressure-sensitive adhesive of the present invention is simple and easy to implement, meets the policy requirements of green environmental protection, and the optical pressure-sensitive adhesive exhibits excellent light transmittance, weather resistance, etc. when applied to polycarbonate diffuser materials.
[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An optical pressure-sensitive adhesive for a polycarbonate diffuser plate, characterized in that: Prepared from the following raw materials in parts by weight:
2. The optical pressure-sensitive adhesive for a polycarbonate diffuser plate according to claim 1, characterized in that: The hydroxyl functional monomer comprises hydroxyethyl acrylate and / or hydroxyethyl methacrylate.
3. The optical pressure-sensitive adhesive for a polycarbonate diffuser plate according to claim 1 or 2, characterized in that: The internal crosslinking monomer comprises 1,6-hexanediol diacrylate and / or ethoxylated trimethylolpropane triacrylate.
4. The optical pressure-sensitive adhesive for a polycarbonate diffuser plate according to claim 1 or 2, characterized in that: The photoinitiator comprises one or more of 1-hydroxycyclohexyl benzophenone, 2-hydroxy-2-methyl-1-phenylacetone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
5. The optical pressure-sensitive adhesive for a polycarbonate diffuser plate according to claim 4, characterized in that: The active amine monomer comprises one or more of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone and 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone.
6. The method for preparing the optical pressure-sensitive adhesive for a polycarbonate diffuser plate according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) mixing butyl acrylate, isooctyl acrylate, methyl methacrylate, acrylic acid, hydroxyl functional monomer, internal crosslinking monomer, part of photoinitiator and active amine monomer under the protection of nitrogen to obtain a mixture; 2) subjecting the mixture to a polymerization reaction under ultraviolet light to obtain a prepolymer; 3) The prepolymer and the remaining photoinitiator are mixed and cross-linked and cured under light to obtain an optical pressure-sensitive adhesive for a polycarbonate diffuser plate.
7. The preparation method according to claim 6, characterized in that: The part of the photoinitiator accounts for 40-50% of the total amount of the photoinitiator.
8. The preparation method according to claim 6 or 7, characterized in that: The conditions of the ultraviolet irradiation are: the irradiation wavelength is 245-380nm, the irradiation distance is 1-10cm, and the irradiation time is 3-8min.
9. The preparation method according to claim 8, characterized in that: In step 3), the main wavelength of the illumination is 365 nm, and the intensity of the illumination is 20-30 mW / cm 2 The illumination time is 20 to 30 seconds.
Citation Information
Patent Citations
Method for synthesis of ultraviolet curing pressure-sensitive adhesive by photopolymerization
CN103333648A
Production method of ultraviolet light curing pressure-sensitive adhesive film
CN105131849A
UV glue and preparation method thereof
CN106833497A
Light curing pressure-sensitive adhesive and preparation method thereof, and pressure-sensitive adhesive tape
CN108300332A
Method for synthesizing photocurable acrylate PCB protective coating by photopolymerization
CN112063209A