Powder explosion suppressant and preparation method thereof
By heating and stirring the divalent and trivalent metal cationic solutions in deionized water, and adding NaOH and NaH2PO4 solutions, a powder explosion inhibitor with a synergistic explosion inhibition effect was prepared, which solved the explosion inhibition in the prior art The problem of poor agent effect has achieved efficient and environmentally friendly explosion prevention and control of metal dust and fire explosives.
Patent Information
- Application Number
- CN202411096845.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The existing technology lacks technical level in preventing metal dust explosions and ignition explosive production accidents, and lacks efficient, environmentally friendly and economical explosive inhibitors, which leads to major challenges in safe production.
Using a powder explosion inhibitor preparation method, by heating and stirring the divalent metal cation solution and the trivalent metal cation solution in deionized water, NaOH and NaH2PO4 solution are added, the pH value is controlled at 8-10, and the reaction is 8-12 hours. , and then washed with anhydrous ethanol, centrifuged, suction filtered and dried to obtain a powder explosion inhibitor with a synergistic explosion inhibitor.
The prepared powder explosion inhibitor has superior explosion inhibitory properties, is environmentally friendly, cost-effective, and is simple in preparation and is easy to produce in order of magnitude, which can effectively suppress the explosion hazards of metal dust and ignition explosives.
Smart Images

Figure CN118995134A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of explosion suppressants, and in particular relates to a powder explosion suppressant and a preparation method thereof. Background Art
[0002] Metal dusts such as aluminum, magnesium and their alloys are widely present in industries such as metallurgy, aerospace, and 3D printing. There is a general risk of combustion and explosion in each link of dust production, dust collection, and disposal. They are also easy to spontaneously combust, have low ignition energy, great explosion power, and various disaster-causing factors. In recent years, accidents involving explosives have occurred frequently. In addition to the above characteristics, the self-oxygen supply system of explosives makes them more dangerous. Once an accident occurs, it will cause serious casualties, economic losses, and adverse social negative impacts.
[0003] Dust explosion has become an important regulatory area for preventing and curbing major production safety accidents, and metal dust explosion has become the top priority for preventing all kinds of dust explosion accidents. The importance of safe production of explosives is also increasing day by day. At present, the development of explosion suppression technology is insufficient, and the overall technical level of prevention of metal dust explosion accidents and explosive production accidents is still significantly behind that of developed countries, which seriously restricts the healthy development of safe production.
[0004] Today's powder explosion suppressants are of a single form and inefficient, and there is a lack of efficient, environmentally friendly and economical explosion suppressants. At the same time, the existing new powder explosion suppressants also need to be improved urgently. Summary of the invention
[0005] In view of the above technical problems, the present invention proposes a powder explosion suppressant and a preparation method thereof. The explosion suppressant has the characteristics of good explosion suppression effect, environmental friendliness, economy, etc., and the preparation method thereof is simple to operate, has little pollution, and is easy to realize mass production.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a powder explosion suppressant comprises the following steps:
[0008] Adding a divalent metal cation solution and a trivalent metal cation solution into deionized water, heating and stirring, to obtain a solution A;
[0009] The NaOH solution and NaH 2 PO 4 The solution was added into deionized water, heated and stirred to obtain solution B;
[0010] In a nitrogen atmosphere, the solution B was added dropwise to the solution A, the pH value was maintained at 8-10 during the addition, and the reaction was continued for 8-12 hours after the addition was completed;
[0011] After the reaction is completed, the powder explosion suppressant is obtained by washing with anhydrous ethanol, centrifuging, filtering and drying.
[0012] Furthermore, the volume ratio of the divalent metal cation solution to the trivalent metal cation solution is (3-5):1.
[0013] Furthermore, the divalent metal cation is Mg 2+ 、Co 2+ , Fe 2+ or Ni 2+ ; The trivalent metal cation is Al 3+ or Fe 3+ .
[0014] Furthermore, the heating and stirring temperature is 70°C.
[0015] Furthermore, the NaOH solution and NaH 2 PO 4 The volume ratio of the solution is 4:1.
[0016] The present invention also provides a powder explosion suppressant prepared by the above preparation method.
[0017] The invention also provides an application of a powder explosion suppressant as an explosion suppressant material.
[0018] Furthermore, the powder explosion suppressant is used at a concentration of 300-600 g / m 3 .
[0019] Furthermore, the powder explosion suppressant is used at a concentration of 600 g / m 3 .
[0020] Compared with the prior art, the present invention has the following advantages and technical effects:
[0021] (1) The powder explosion suppressant prepared by the present invention has better effect than the traditional explosion suppressant, has physical and chemical synergistic explosion suppression effect, and has excellent explosion suppression performance;
[0022] (2) It is environmentally friendly and economically efficient.
[0023] (3) The preparation method is simple, the raw materials are cheap and readily available, and large-scale production can be easily achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0025] Figure 1 This is a SEM image of the powder explosion suppressant prepared in Example 1;
[0026] Figure 2This is the XRD pattern of the powder explosion suppressant prepared in Example 1;
[0027] Figure 3 This is the relationship between aluminum powder concentration and explosion pressure;
[0028] Figure 4 The figure is a relationship diagram between the concentration of the powder explosion suppressant prepared in Example 1 and the explosion pressure;
[0029] Figure 5 This is a relationship diagram between different injection times and explosion pressure of the new powder explosion suppressant prepared in Example 1;
[0030] Figure 6 The figure is the relationship between the concentration of different explosion suppressants and the explosion pressure;
[0031] Figure 7 For different concentrations of Mg(OH) 2 Relationship diagram with explosion pressure. DETAILED DESCRIPTION
[0032] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0033] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0034] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0035] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0036] The embodiment of the present invention discloses a method for preparing a powder explosion suppressant, comprising the following steps:
[0037] Adding a divalent metal cation solution and a trivalent metal cation solution into deionized water, heating and stirring, to obtain a solution A;
[0038] The NaOH solution and NaH 2 PO 4 The solution was added into deionized water, heated and stirred to obtain solution B;
[0039] In a nitrogen atmosphere, the solution B was added dropwise to the solution A, the pH value was maintained at 8-10 during the addition, and the reaction was continued for 8-12 hours after the addition was completed;
[0040] After the reaction is completed, the powder explosion suppressant is obtained by washing with anhydrous ethanol, centrifuging, filtering and drying.
[0041] In some preferred embodiments, the volume ratio of the divalent metal cation solution to the trivalent metal cation solution is (3-5):1, such as 3:1, 4:1 or 5:1.
[0042] In some preferred embodiments, the divalent metal cation is Mg 2+ 、Co 2+ , Fe 2+ or Ni 2+ Mg is preferred 2 + ; The trivalent metal cation is Al 3+ or Fe 3+ , preferably Al 3+ The salt providing the divalent metal cation may be Mg(NO 3 ) 2 MgCl 2 etc. magnesium salts; the salt providing trivalent metal cations may be Al(NO 3 ) 3 、AlCl 3 Aluminum salts etc.
[0043] In some preferred embodiments, the heating and stirring temperature is 70°C.
[0044] In some preferred embodiments, the NaOH solution and NaH 2 PO 4 The volume ratio of the solution is 4:1.
[0045] The powder explosion suppressant prepared by the above preparation method can be used as an explosion suppressant material, has a physical and chemical synergistic explosion suppression effect, and has excellent explosion suppression performance. The concentration of the powder explosion suppressant is 300-600g / m 3When the explosion suppression effect is better than that of the traditional explosion suppression agent, in some preferred embodiments, the concentration of the powder explosion suppression agent is 300-600g / m 3 In a more preferred embodiment, the concentration of the powder explosion suppressant is 600g / m 3 .
[0046] Among the many explosion prevention and control technologies, explosion suppression technology is considered to be the most promising means to reduce or even eliminate explosion hazards. It can detect and prevent combustion from turning into explosion in the early stage of combustion. The metal layers of the powder explosion suppressant of the present invention carry a large number of hydroxyl groups. When it is in the explosion field, the layers collapse and the ordered layered structure is destroyed. The hydroxyl groups of the layers absorb heat through evaporation and have excellent physical heat absorption and cooling effect. At the same time, the layers are made of M 2+ and M 3+ The metal ions in the explosion field can react with oxygen free radicals to generate metal oxides, interrupting the explosion chain reaction and further reducing the explosion hazard. Sodium bicarbonate and ammonium dihydrogen phosphate in traditional dry powder inhibitors have excellent chemical inhibition. Therefore, bicarbonate and dihydrogen phosphate are inserted between metal layers to form a stable layered structure. Combined with the heat absorption of hydroxyl evaporation of the layer, the heat absorption of metal layer collapse, the oxygen deprivation of the layer metal, and the neutralization of free radicals by interlayer anions to block the explosion chain reaction, multi-dimensional explosion inhibition with fast physical heat absorption and cooling and strong chemical inhibition can be achieved.
[0047] The powder explosion suppressant of the present invention enters the core area of the explosion reaction in the form of powder. With the collapse of the layer plate in the explosion field, the separation of components, the evaporation of the liquid phase, the multi-phase thermal decomposition, and the interaction with the flame free radicals, the physical endothermic explosion suppression of the layer plate collapse, the chemical free radical explosion suppression of the interlayer anions, and the explosion suppression of the metal layer plate ions are involved. The explosion suppression material has a multi-dimensional explosion suppression synergistic effect of both physical endothermic cooling and chemical free radical suppression.
[0048] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.
[0049] The "room temperature" in the present invention refers to 20-30°C unless otherwise specified.
[0050] The raw materials used in the present invention are all purchased from the market.
[0051] The technical solution of the present invention is further illustrated by the following embodiments.
[0052] Example 1
[0053] 1) Mg(NO 3 ) 2 6H 2 O is dissolved in water to prepare Mg(NO3 ) 2 solution, Al(NO 3 ) 3 9H 2 O is dissolved in water to prepare Al(NO 3 ) 3 The two were mixed in a volume ratio of 3:1 and dissolved in deionized water so that the solution contained Mg 2+ The concentration is 0.3M, Al 3+ The concentration is 0.1 M, and the mixture is stirred evenly at 70°C to obtain solution A;
[0054] 2) NaOH solution and NaH 2 PO 4 The solution was added to deionized water at a volume ratio of 4:1, so that the concentration of NaOH solution in the solution was 0.8 M. 2 PO 4 The concentration of the solution is 0.1 M, and the mixture is stirred at 70°C to obtain solution B;
[0055] 3) In a nitrogen atmosphere, solution B was added dropwise to solution A, and the pH value was maintained at 10 during the addition process. After the addition was completed, the reaction was continued for 12 hours. After the reaction was completed, the solution was washed with 200 mL of anhydrous ethanol, centrifuged, and filtered. The three steps (washing, centrifugation, and filtration) were repeated three times and then dried for 12 hours to obtain a powder explosion suppressant (LDHs, hydrotalcite).
[0056] Figure 1 This is a SEM image of the powder explosion suppressant prepared in Example 1. Figure 1 It can be seen that the powder explosion suppressant prepared by the method of Example 1 has a layered structure. 2 PO 4 - It can be judged that the present invention has successfully prepared a layered bimetallic supramolecular targeted explosion suppression new material.
[0057] Figure 2 The XRD pattern of the powder explosion suppressant prepared in Example 1 is shown in FIG. Figure 2 It can be seen from the figure that the material shows typical LDHs diffraction peaks, with (003), (006) and (009) plane diffraction peaks appearing at 11.69°, 23° and 35°, respectively. Correspondingly, d(003) is 7.56, which is consistent with the 0.76-0.78 (CO 3 2- The difference between the intercalation layer and the larger tetrahedral H 2 PO 4 - ions enter the LDH interlamellar space, forming Mg-Al-H 2PO 4 The (009) crystal plane diffraction peak intensity is significantly enhanced, indicating that H 2 PO 4 - The H 2 PO 4 - After entering the interlayer, only the interlayer spacing changes, and the layer structure is not affected. In summary, the present invention prepares H 2 PO 4 - The intercalated layered structure, i.e. Mg-Al-H 2 PO 4 .
[0058] Example 2
[0059] 1) Put Co(NO 3 ) 2 6H 2 O is dissolved in water to prepare Co(NO 3 ) 2 solution, Fe(NO 3 ) 3 9H 2 O is dissolved in water to prepare Fe(NO 3 ) 3 The two were mixed in a volume ratio of 3:1 and dissolved in deionized water so that the solution contained Co 2+ The concentration of Fe is 0.3M. 3+ The concentration is 0.1 M, and the mixture is stirred evenly at 70°C to obtain solution A;
[0060] 2) NaOH solution and NaH 2 PO 4 The solution was added to deionized water at a volume ratio of 4:1, so that the concentration of NaOH solution in the solution was 0.8 M. 2 PO 4 The concentration of the solution is 0.1 M, and the mixture is stirred at 70°C to obtain solution B;
[0061] 3) In a nitrogen atmosphere, solution B was added dropwise to solution A, and the pH value was maintained at 10 during the addition. After the addition was completed, the reaction was continued for 12 hours. After the reaction was completed, the solution was washed with 200 mL of anhydrous ethanol, centrifuged, and filtered. The three steps (washing, centrifugation, and filtration) were repeated three times and then dried for 12 hours to obtain a powder explosion suppressant.
[0062] Application Examples
[0063] 1. Explosion of pure aluminum powder
[0064] A 20L spherical explosion device was used to test the pressure generated by the explosion of aluminum powder of different concentrations. The specific experimental method is as follows: 200g / m 3 , 300g / m 3 , 400g / m 3 , 500g / m 3 , 600g / m 3 , 700g / m 3 , 800g / m 3 Aluminum powder is placed in a 20L ball for testing. The experiment is repeated three times and the average value is recorded as the explosion pressure of the aluminum powder.
[0065] Figure 3 The graph is the relationship between aluminum powder concentration and explosion pressure. It can be found that when the aluminum powder concentration is 700g / m 3 The maximum explosion pressure is 800g / m 3 There is obvious aluminum powder residue in the test container at 400g / m 3 A small peak pressure value is reached at 700g / m 3 The explosion pressure is high, the temperature is high, and there is residual aluminum powder, which makes the experiment dangerous. Therefore, the aluminum powder concentration of 400g / m 3 The explosion suppression effect of the explosion suppression agent prepared in Example 1 of the present invention was studied as the research object.
[0066] 2. Powder explosion suppressant suppresses aluminum powder explosion
[0067] A 20L spherical explosion device was used to test the effects of different concentrations of powder explosion suppressants as explosion suppressants on aluminum powder explosion. The specific test method is as follows: The aluminum powder concentration is set to 400g / m 3 The concentrations used are 0 (no explosion suppressant), 150, 300, 450, and 600 g / m 3 Powder explosion suppressant. Other methods are the same as above.
[0068] Figure 4 The graph is a relationship between the concentration of the powder explosion suppressant prepared in Example 1 and the explosion pressure. It can be seen that the powder explosion suppressant prepared in Example 1 has an inhibitory effect on the explosion of aluminum powder. 3 The explosion suppression effect is best when the maximum explosion pressure of aluminum powder explosion drops from 0.955MPa to 0.676MPa.
[0069] 3. Powder explosion suppressant suppresses the explosion of aluminum-containing explosives
[0070] The effect of the injection time of the new powder explosion suppressant on the explosion of aluminum-containing explosives was tested using a 20L spherical explosion device. The specific test method is as follows: the explosive concentration is set to 300g / m 3 , explosion suppressant concentration is 300g / m3 The explosion suppressant was sprayed 10ms, 20ms and 30ms after the explosion of the explosive respectively. The experiment was repeated three times and the average value was recorded as the relationship between different injection times of the new explosion suppressant and the explosion pressure.
[0071] Figure 5 This is a relationship diagram between different spraying times of the new powder explosion suppressant prepared in Example 1 and the explosion pressure. It can be seen that the new powder explosion suppressant prepared in Example 1 has an inhibitory effect on the explosion of aluminum powder. The explosion suppression effect is best when the explosion suppressant is sprayed 10ms after the explosion of the aluminum powder, and the explosive is basically completely suppressed.
[0072] 4. Comparison between powder explosion suppressant and traditional explosion suppressant in suppressing aluminum powder explosion
[0073] The effects of different types of explosion suppressants on aluminum powder explosion were tested using a 20L spherical explosion device to verify the effect of the powder explosion suppressant prepared in Example 1. The specific test method is as follows: The aluminum powder concentration is set to 400g / m 3 The concentration of explosion suppressant was set to 0 (no explosion suppressant), 150, 300, 450, 600 g / m 3 . Other methods are the same as 2.
[0074] There are two types of traditional explosion suppressants:
[0075] 1) NaHCO 3 , from Guangzhou Keqi Chemical Technology Co., Ltd.;
[0076] 2) NaH 2 PO 4 , from Guangzhou Keqi Chemical Technology Co., Ltd.
[0077] Figure 6 : is a relationship diagram between the concentration of different explosion suppressants and the explosion pressure. It can be seen from the figure that under the same working conditions, the explosion suppression effect of the explosion suppressant prepared in Example 1 is better than that of the traditional explosion suppressant, and as the concentration of the explosion suppressant increases, the effect becomes more obvious.
[0078] Comparative Example 1
[0079] Same as Example 1, except that Mg(NO 3 ) 2 The solution was replaced with Mg(OH) 2 Solution. Mg(OH) 2 There are metal cations that take away oxygen, and water is easily formed in the reaction to suppress explosion through endothermic absorption, but there is no layered structure.
[0080] The effects of different types of explosion suppressants on aluminum powder explosion were tested using a 20L spherical explosion device to verify the effect of the powder explosion suppressant prepared in Example 1. The specific test method is as follows: The aluminum powder concentration is set to 400g / m3 The concentration of explosion suppressant was set to 0 (no explosion suppressant), 150, 300, 450, 600 g / m 3 . Other methods are the same as 2.
[0081] Figure 7 For different concentrations of Mg(OH) 2 The relationship diagram with the explosion pressure shows that under the same working conditions, the explosion suppression effect of the explosion suppressant of Example 1 is obviously weaker than that of the new explosion suppressant. The explosion pressure of aluminum powder only drops from 0.954 to 0.71, which is lower than 0.676MPa of the new explosion suppressant.
[0082] The results show that the new powder explosion suppressant with a layered structure prepared by the present invention has a better explosion suppression effect than other chemical explosion suppressants with non-layered structures. This is because the layered structure will collapse in the explosion field, and this phenomenon will compete with the explosion suppression object for oxygen in the explosion field, thereby inhibiting the explosion reaction.
[0083] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a powder explosion suppressant, characterized in that: The following steps are involved: Adding a divalent metal cation solution and a trivalent metal cation solution into deionized water, heating and stirring, to obtain a solution A; Add NaOH solution and NaH2PO4 solution into deionized water, heat and stir to obtain solution B; In a nitrogen atmosphere, the solution B was added dropwise to the solution A, the pH value was maintained at 8-10 during the addition, and the reaction was continued for 8-12 hours after the addition was completed; After the reaction is completed, the powder explosion suppressant is obtained by washing with anhydrous ethanol, centrifuging, filtering and drying.
2. The method for preparing a powder explosion suppressant according to claim 1, characterized in that: The volume ratio of the divalent metal cation solution to the trivalent metal cation solution is (3-5):
1.
3. The method for preparing a powder explosion suppressant according to claim 2, characterized in that: The divalent metal cation is Mg 2+ 、Co 2+ , Fe 2+ or Ni 2+ ; The trivalent metal cation is Al 3+ or Fe 3+ .
4. The method for preparing a powder explosion suppressant according to claim 1, characterized in that: The heating and stirring temperature was 70°C.
5. The method for preparing a powder explosion suppressant according to claim 1, characterized in that: The volume ratio of the NaOH solution to the NaH2PO4 solution is 4:
1.
6. A powder explosion suppressant prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the powder explosion suppressant as claimed in claim 6 as an explosion suppression material.
8. The use according to claim 7, characterized in that: The powder explosion suppressant is used at a concentration of 300-600 g / m 3 .
9. The use according to claim 8, characterized in that: The concentration of the powder explosion suppressant is 600 g / m 3 .
Citation Information
Patent Citations
Novel inorganic explosion suppression material with low silica-alumina ratio and preparation method thereof
CN118239498A
Fire extinguishing and explosion suppressant substances
WO1993000963A2
Cited By
Composite dry water explosion suppressant for suppressing explosion of organic dust and preparation method of composite dry water explosion suppressant
CN119982039A