Control method for directly returning residual casting molten steel to empty ladle and utilizing ladle overflow slag
Through slag pouring and argon blowing station treatment, the w[C] and aluminum content in the molten steel is controlled, and the problem of overflowing slag in the ladle is solved, and the safe recycling and efficient utilization of the molten steel is achieved. Reduces steelmaking costs and temperature drops.
Patent Information
- Application Number
- CN202310573285.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-22
AI Technical Summary
There is a problem of ladle overflow during the use of existing casting residual steel ladles, resulting in long processing time, large temperature losses and safety hazards.
Through slag pouring treatment, the use of bottom argon blowing device, deoxygenation treatment of converter steel, argon stirring at argon blowing station and aluminum wire feeding, the w[C] and aluminum content in the molten steel is controlled to avoid lag slag Foaming and spilling slag to achieve safe recycling and utilization of molten steel.
The treatment time of casting residual steel is shortened, the temperature loss is reduced, the blasting and overflow of ladle cladding is avoided, the cost of steelmaking is reduced, and the utilization rate of metal materials and the level of resource recycling is improved.
Smart Images

Figure BDA0004239229810000031 
Figure BDA0004239229810000032 
Figure BDA0004239229810000033
Abstract
Description
Technical Field
[0001] The invention relates to a production and utilization technology of excess molten steel, in particular to a control method for directly returning excess molten steel to an empty ladle to utilize ladle overflow slag, and belongs to the technical field of steelmaking and continuous casting. Background Art
[0002] There are usually three ways to return the remaining molten steel to production:
[0003] The first casting waste treatment mode is to pour large bags of casting waste into a slag basin. After a period of cooling, it is transported to a slag treatment site by a tank truck. After being separated by a heavy hammer, the part with a high iron content is returned to the steel plant by magnetic separation and treated as scrap steel. It is smelted in a converter or electric furnace. The disadvantage of the first treatment mode is that the treatment time is long, and the casting waste becomes cold, resulting in temperature loss.
[0004] The second casting waste treatment mode is to return the casting waste to the iron ladle for utilization, pour the large ladle of casting waste into the iron ladle for the bottom molten iron, add molten iron after 3-5 ladle of casting waste, and return it to the converter or electric furnace for re-smelting. In the second casting waste return to iron ladle mode, the casting waste and the bottom molten iron have a long waiting time, a large temperature loss, and the metal material loss is increased after smelting in the converter or electric furnace.
[0005] The third mode of treating the casting waste is to pour the casting waste into the ladle that has already discharged the molten steel and process it through the refining process. In the third mode, the casting waste is returned to the ladle that has already discharged the molten steel. During the return process, there will be waiting, and the ladle slag will easily foam or overflow due to the return of carbon and oxygen in the process of directly returning the large ladle casting waste to the ladle, burning the argon gas pipe and causing personal injury accidents.
[0006] A Chinese patent application document with application publication number CN102766725A discloses a method for hot utilization of stainless steel continuous casting overfill, comprising the steps of transporting a ladle with overfill to an electric furnace charging line, stopping power supply to the electric furnace, and opening the electric furnace; II. Transportation and utilization: pouring all the slag and molten steel in the ladle into a dephosphorized iron ladle, and then adding the dephosphorized molten iron into the electric furnace to be used as a raw material for smelting stainless steel in an electric furnace, wherein the ratio of continuous casting overfill to dephosphorized molten iron is: 2-5 tons of continuous casting overfill; 80-120 tons of dephosphorized molten iron; III. Returning the electric furnace to power supply for smelting; this method pours the overfilled molten steel and slag into the molten iron ladle for utilization. Summary of the invention
[0007] The purpose of the present invention is to provide a method for controlling slag overflow from the ladle when the leftover steel liquid is directly returned to an empty ladle, mainly to solve the technical problem of slag overflow from the ladle during the argon blowing treatment process when the leftover steel liquid is directly returned to an empty ladle; the method of the present invention realizes the safe recycling of the leftover steel liquid, and reduces the cost of returning the leftover steel liquid to production; the method of the present invention shortens the processing time of the leftover steel liquid when it is returned to production, reduces the temperature loss of the leftover steel liquid, and avoids the problem of foaming and slag overflow from the ladle containing the leftover steel liquid during the converter tapping process.
[0008] The technical idea of the present invention is to carry out slag removal treatment on the overcast molten steel in the ladle of the finished heat; add the overcast molten steel in the ladle of the previous heat into the empty ladle of the current heat with a set bottom blowing flow rate; deoxidize and alloy the molten steel tapped from the converter; transport the molten steel in the ladle to an argon blowing station for argon blowing treatment, and carry out continuous casting of the molten steel treated by the argon blowing station.
[0009] The technical solution adopted by the present invention is a method for controlling the slag overflow from the ladle by directly returning the remaining molten steel to the empty ladle, comprising the following steps:
[0010] 1) Top and bottom combined blowing converter smelting is adopted; the converter smelting end point is controlled, sampling is performed to detect w[C] and molten steel temperature in the converter blowing end point, and when w[C] in the molten steel at the converter blowing end point is detected to be 0.03% to 0.08%, and when the molten steel temperature at the converter blowing end point is ≥1650°C, the converter blowing is terminated;
[0011] 2) The remaining molten steel in the ladle of the finished heat is slag-drained. When the amount of remaining molten steel is less than 10 tons, the remaining ladle is hoisted to the top of the slag basin by a crane and the ladle is tilted to drain the slag;
[0012] 3) Add the remaining molten steel into the empty ladle of this furnace. Before adding the remaining molten steel, open the bottom argon blowing device of the ladle. The bottom blowing argon gas flow rate is 5-25Nm 3 / h; add the molten steel after slag pouring into the empty ladle, and control the adding time of the molten steel to be ≤5min; control the time interval from the end of adding the molten steel into the empty ladle to the start of tapping of the converter to be <6min;
[0013] 4) Steel is tapped immediately after the converter blowing is completed. When the converter starts tapping steel, the argon gas flow rate at the bottom of the ladle is controlled to be 15-35Nm 3 / h; deoxidize and alloy the molten steel tapped from the converter, and control the aluminum content in the molten steel to be 0.02-0.04% of the aluminum content in the molten steel; when w[C] in the molten steel is ≤0.08%, at the end of tapping, add lime to the molten steel in the ladle to modify the ladle slag; the amount of lime added is 1.0-1.2 kg / ton of steel, and the weight percentage of the chemical composition of the lime is CaO ≥ 90%, SiO2 ≤ 3.5% and the burnout is not more than 5%;
[0014] 5) The molten steel in the ladle is transported to the argon blowing station to control the aluminum and carbon content in the molten steel. The molten steel in the ladle is transported to the argon blowing station, the temperature of the molten steel entering the argon blowing station is controlled to be ≥1615°C, and argon is introduced into the molten steel to stir the molten steel for 3-4 minutes; the introduction of argon into the molten steel is stopped, and the aluminum content in the molten steel is tested by sampling; argon is introduced into the molten steel again, and aluminum wire is fed into the molten steel. The amount of aluminum wire added is determined according to the aluminum content in the finished molten steel; after feeding the aluminum wire, the argon is turned off, the molten steel treatment at the argon blowing station is completed, and the w[Al] in the molten steel leaving the argon blowing station is controlled to be 0.045%-0.055%;
[0015] 6) Continuously casting the molten steel into slabs to obtain continuously cast slabs.
[0016] Further, in step 5), when the thickness of the ladle slag layer is ≤150 mm, the argon blowing time from the start of feeding the aluminum wire into the molten steel to the end of argon blowing is controlled to be ≥6 min; when the thickness of the ladle slag layer is >150 mm, the argon blowing time from the start of feeding the aluminum wire into the molten steel to the end of argon blowing is controlled to be ≥9 min.
[0017] Repeat the steps of the present invention and start returning the excess molten steel from the current cast to the ladle for utilization.
[0018] The method of the present invention is based on the following research of the applicant:
[0019] The applicant has found that in this mode of adding the remaining molten steel from the finished heat into the ladle from which the steel has been finished, the time that the full ladle of molten steel from the current heat waits for the remaining molten steel from the previous heat is uncontrollable, sometimes short and sometimes long; the long waiting time for the remaining molten steel from the previous heat is likely to cause a large drop in the temperature of the molten steel; in addition, when the remaining molten steel from the previous heat is returned to production, the carbon content in the molten steel is high; when the mass content of carbon in the molten steel is greater than 0.06%, severe foaming of the ladle slag and severe slag overflow from the ladle are likely to occur during carbon replenishment or argon blowing treatment, which can burn the argon gas pipe and easily cause personal injury accidents.
[0020] By adopting the method of the present invention, most of the residual oxidized steel slag in the residual molten steel of the finished furnace is poured out first; in the process of tapping the steel from the converter, the residual molten steel is subjected to deoxidation, alloying and ladle slag modification treatments, and then argon blowing treatment is carried out in an argon blowing station, so that foaming of the ladle slag and overflow of slag can be avoided, the process of refining treatment in the LF furnace can be reduced, and the steelmaking cost is reduced.
[0021] Compared with the prior art, the present invention has the following positive effects: 1. The cast waste steel is directly cast after hot cycle treatment, which shortens the cast waste treatment cycle, reduces the temperature drop, and greatly improves the utilization rate of cast waste metal materials. 2. The utilization of cast waste returned to the ladle allows the slag steel produced by steelmaking to be directly recycled, reducing processing costs and emissions, which is of great practical significance for improving the comprehensive recycling level of enterprise resource cycles. DETAILED DESCRIPTION
[0022] The present invention is further described below in conjunction with specific embodiments 1 to 6, as shown in Tables 1 to 7.
[0023] The embodiment of the present invention takes 150-ton top and bottom combined blowing converter smelting as an example.
[0024] The steel grade smelted in Examples 1-3 is SAE1006; the steel grade smelted in Examples 4-6 is MRT-4CA.
[0025] Table 1 Parameters of slag pouring and recasting of excess molten steel after pouring the remaining molten steel in the heat of the present invention
[0026]
[0027] Table 2 The composition and temperature of the molten steel at the end of converter smelting in the embodiment of the present invention
[0028]
[0029] Table 3 Amount of auxiliary materials and alloy added in the converter steel-tapping process of the embodiment of the present invention Unit: kg / ton steel.
[0030]
[0031]
[0032] Table 4 Argon blowing parameters at the bottom of ladle during converter steel tapping in the embodiment of the present invention
[0033] Heat <![CDATA[Argon bottom blowing in ladle / Nm 3 / h]]> Example 1 10 Example 2 14 Example 3 20 Example 4 6 Example 5 7 Example 6 9
[0034] Table 5 Parameters of molten steel entering the argon blowing station according to the embodiment of the present invention
[0035]
[0036] Table 6 Process parameters of the argon blowing station in the embodiment of the present invention
[0037]
[0038] Table 7 Composition and temperature of molten steel at the outlet of argon blowing station according to the embodiment of the present invention
[0039]
[0040]
[0041] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.
Claims
1. A method for controlling the slag overflow from the ladle by directly returning the remaining molten steel to the empty ladle, characterized in that: The method comprises the following steps: 1) Top and bottom combined blowing converter smelting is adopted; the converter smelting end point is controlled, sampling is performed to detect w[C] and molten steel temperature in the converter blowing end point, and when w[C] in the molten steel at the converter blowing end point is detected to be 0.03% to 0.08%, and when the molten steel temperature at the converter blowing end point is ≥1650°C, the converter blowing is terminated; 2) The remaining molten steel in the ladle of the finished heat is slag-drained. When the amount of remaining molten steel is less than 10 tons, the remaining ladle is hoisted to the top of the slag basin by a crane and the ladle is tilted to drain the slag; 3) Add the remaining molten steel into the empty ladle of this furnace. Before adding the remaining molten steel, open the bottom argon blowing device of the ladle. The bottom blowing argon gas flow rate is 5-25Nm 3 / h; add the molten steel after slag pouring into the empty ladle, and control the adding time of the molten steel to be ≤5min; control the time interval from the end of adding the molten steel into the empty ladle to the start of tapping of the converter to be <6min; 4) Steel is tapped immediately after the converter blowing is completed. When the converter starts tapping steel, the argon gas flow rate at the bottom of the ladle is controlled to be 15-35Nm 3 / h; deoxidize and alloy the molten steel tapped from the converter, and control the aluminum content in the molten steel to be 0.02-0.04% of the aluminum content in the molten steel; when w[C] in the molten steel is ≤0.08%, at the end of tapping, add lime to the molten steel in the ladle to modify the ladle slag; the amount of lime added is 1.0-1.2 kg / ton of steel, and the weight percentage of the chemical composition of the lime is CaO ≥ 90%, SiO2 ≤ 3.5% and the burnout is not more than 5%; 5) The molten steel in the ladle is transported to the argon blowing station to control the aluminum and carbon content in the molten steel. The molten steel in the ladle is transported to the argon blowing station, the temperature of the molten steel entering the argon blowing station is controlled to be ≥1615°C, and argon is introduced into the molten steel to stir the molten steel for 3-4 minutes; the introduction of argon into the molten steel is stopped, and the aluminum content in the molten steel is tested by sampling; argon is introduced into the molten steel again, and aluminum wire is fed into the molten steel. The amount of aluminum wire added is determined according to the aluminum content in the finished molten steel; after feeding the aluminum wire, the argon is turned off, the molten steel treatment at the argon blowing station is completed, and the w[Al] in the molten steel leaving the argon blowing station is controlled to be 0.045%-0.055%; 6) Continuously casting the molten steel into slabs to obtain continuously cast slabs.
2. The method for controlling the slag overflow from the ladle by directly returning the cast molten steel to the empty ladle as claimed in claim 1 is characterized in that: In step 5), when the thickness of the ladle slag layer is ≤150 mm, the argon blowing time from the start of feeding the aluminum wire into the molten steel to the end of argon blowing is controlled to be ≥6 min; when the thickness of the ladle slag layer is >150 mm, the argon blowing time from the start of feeding the aluminum wire into the molten steel to the end of argon blowing is controlled to be ≥9 min.