Moisture-absorbing and sweat-releasing cool-feeling fabric and preparation method thereof
By combining hollow PVDF nanofibers, graphene and biofilm on the fabric, the heat transfer effect of polysaccharides and graphene in the biofilm is used to solve the problem of poor moisture absorption and sweating effect of commercially available fabrics, and quickly absorb sweat and reduce sweat The effect of skin temperature significantly improves the moisture absorption, quick drying and coolness of the fabric.
Patent Information
- Application Number
- CN202411013669.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The commercially available summer clothing and fabrics generally have poor moisture absorption and sweating effect, the cool feeling is not obvious, and it cannot effectively reduce the skin surface temperature.
Hollow PVDF nanofibers and graphene combined with biofilm were used to prepare core-shell nanofiber membranes by coaxial electrospinning, and multiple finishing treatments were performed on modal fabrics, and dopamine hydrochloride solution was added to enhance moisture absorption and cooling performance.
It quickly absorbs sweat and reduces the skin surface temperature, significantly improves the moisture absorption and quick drying performance and coolness of the fabric, and has good washing and weather resistance.
Smart Images

Figure CN118996854A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile finishing, and in particular relates to a moisture absorbing and perspiration wicking cool fabric and a preparation method thereof. Background Art
[0002] Moisture wicking fabrics are often called "moisture wicking and quick-drying fabrics" or "breathable fabrics". Moisture wicking fibers generally have a high specific surface area, with numerous pores or grooves on the surface, and their cross-sections are generally special shapes. Using the capillary effect, the fibers can quickly absorb moisture and sweat from the skin surface and diffuse and transfer them to the outer layer of the hair.
[0003] The main technical features of moisture-wicking fabrics are as follows. Special fiber design: Cool fabrics may use fibers with special cross-sectional shapes, such as special-shaped cross-sectional fibers. These fiber structures can increase the surface area, promote air circulation, and accelerate the evaporation of sweat, thereby taking away body surface heat. Some fibers contain microcapsules inside, which are wrapped with cooling ingredients. When the fabric contacts the skin, the microcapsules gradually break and release cool substances, giving people a cool feeling. Moisture absorption and heat dissipation: Some cool fabrics work through the moisture absorption and sweat-wicking ability of the fiber itself. They can quickly absorb sweat from the skin surface and quickly diffuse it to the surface of the fabric, expand the evaporation area, and use the latent heat exchange principle when water evaporates to take away a large amount of heat, thereby achieving the effect of lowering body temperature. Minerals or special additives: During the fiber production process, mineral powders or special chemicals with excellent thermal conductivity may be added. These ingredients can accelerate the conduction and dissipation of heat, so that the fabric can take away heat faster when it contacts the skin. Finishing technology: Through special finishing processes, such as the use of cooling finishing agents, a layer of coating or microcapsules that can absorb and quickly release heat is added to the surface of the fabric without changing the original fabric properties, achieving an instant cool touch while maintaining good washability. Physical or chemical modified fibers: The original fibers are modified by physical or chemical methods to have better thermal conductivity and moisture absorption, or new synthetic fibers that have cooling properties are directly used.
[0004] However, the summer clothing and fabrics currently available on the market generally have poor moisture absorption and perspiration removal effects, and the cooling effect is not obvious. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a moisture absorbing and perspiration wicking cooling fabric and a preparation method thereof, wherein the fabric can quickly absorb sweat, while lowering the skin surface temperature and wicking sweat.
[0006] In order to solve the above technical problems, the present invention provides a moisture absorbing and perspiration wicking cooling fabric and a preparation method thereof, comprising the following steps:
[0007] S1. Coaxially electrospinning the shell layer spinning solution and the core layer spinning solution to obtain a core-shell nanofiber membrane, immersing the core-shell nanofiber membrane in an aqueous solution containing a surfactant, washing, drying and crushing the membrane to obtain a hollow PVDF nanofiber; the shell layer spinning solution is a PVDF solution, and the core layer spinning solution is a polyvinyl pyrrolidone solution;
[0008] S2. Preparation of biofilm: Pseudomonas aeruginosa is inoculated into LB medium, and glass beads are added after shaking culture for 24-48 hours, and then incubated for 20-24 hours. After filtering, the glass beads are poured into water, and the biofilm suspension is obtained after high-speed vortexing to remove the glass beads; the polysaccharide content in the biofilm suspension is 10-15g / L.
[0009] S3. Fabric finishing: adding the hollow PVDF nanofibers and graphene to the biofilm suspension to obtain a finishing liquid; using the finishing liquid to finish the modal fabric, repeating the finishing process 3-5 times, and then immersing in a dopamine hydrochloride solution for treatment, taking out and washing and drying to obtain a moisture-absorbing, perspiration-wicking, cooling fabric.
[0010] Furthermore, in step S1, the shell spinning solution is prepared by adding polyvinylidene fluoride (PVDF) into a mixed solvent of N,N-dimethylacetamide and acetone, wherein the weight average molecular weight of PVDF is 400,000-600,000, and the concentration of PVDF is 10-15 w / v%.
[0011] Furthermore, in step S1, the shell spinning solution is prepared by adding PVDF to a mixed solvent of N,N-dimethylacetamide and acetone in a ratio of 1:1, stirring to completely dissolve and disperse the PVDF, and then standing to degas, thereby obtaining the shell spinning solution.
[0012] Furthermore, in step S1, the core layer spinning solution is prepared by dissolving polyvinyl pyrrolidone in anhydrous ethanol, the polyvinyl pyrrolidone is polyvinyl pyrrolidone PVPK90, and the concentration of polyvinyl pyrrolidone in the core layer spinning solution is 8-20w / v%.
[0013] Furthermore, in step S1, the method for preparing the core layer spinning solution is: dissolving polyvinyl pyrrolidone PVPK90 in anhydrous ethanol, stirring at 60° C. until completely dissolved, and standing to degas, thereby obtaining the core layer spinning solution.
[0014] Furthermore, in step S1, the coaxial electrospinning conditions are: voltage 20-25 kV, receiving distance 12-18 cm, shell layer spinning solution flow rate 0.5-0.7 ml / h, core layer spinning solution flow rate 0.4-0.5 ml / h.
[0015] Furthermore, in step S1, in the aqueous solution containing a surfactant, the surfactant is one of Tween 80, rhamnolipid and sodium dodecyl sulfate, and the concentration is 10-15 w / v%.
[0016] Furthermore, in step S1, the average length of the hollow PVDF nanofibers is 10-200 μm.
[0017] Furthermore, in step S2, the preparation process of the biofilm is as follows: Pseudomonas aeruginosa is inoculated into LB medium and cultured by shaking. After culturing for 24-48 hours, 5-10 w / v% sterile glass beads with a diameter of 4-6 mm are added, and then incubated for 20-24 hours. After filtering, the glass beads are poured into water, vortexed at high speed, and the glass beads are removed with a sieve to obtain a biofilm suspension.
[0018] Furthermore, in step S3, the finishing is specifically: applying the finishing liquid on the modal fabric, and drying at 120-140°C for shaping.
[0019] Furthermore, in step S3, in the finishing liquid, the concentration of the hollow PVDF nanofibers is 1.0-1.5 w / v%, and the concentration of graphene is 0.1-0.5 w / v%.
[0020] Furthermore, in step S3, the amount of the finishing liquid is 50-80 ml / m 2 ; The pH of the dopamine hydrochloride solution is 9.5-10.0, and the concentration is 0.4-0.9w / v%.
[0021] Furthermore, the immersion in the dopamine hydrochloride solution is performed for a treatment time of 20-50 minutes.
[0022] The present invention also provides a moisture absorbing and perspiration wicking cool fabric prepared by the above preparation method.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1) The present invention utilizes the adhesion of biofilm on solid surface to combine graphene and hollow PVDF nanofiber on the surface of modai fabric, and its main component polysaccharide contains rich hydroxyl groups, which can promote the synthesis and coverage of polydopamine. Biofilm mainly contains polysaccharide, which can be hydrophilic and hygroscopic, and can also use the rich three-dimensional network structure to achieve capillary action and transport water to the surface. In addition, the modified hollow PVDF nanofiber can also absorb water from the biofilm on the surface, and then absorb the water into the hollow fiber and evaporate it to the outside in combination with the heat transfer and heat pipe effect of graphene, and at the same time obtain an excellent cooling effect.
[0025] 2) The present invention adopts a biological membrane, which can have strong resistance to stress and decomposition, which is very important for maintaining the function of the moisture absorption and perspiration cooling fabric after finishing and the washing and weather resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a scanning electron microscope photograph of the fabric prepared in Example 1. DETAILED DESCRIPTION
[0027] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0028] Example 1
[0029] A moisture wicking cool fabric and a preparation method thereof, comprising the following steps:
[0030] 1. Preparation of hollow PVDF nanofibers: Add PVDF with a weight average molecular weight of 500,000 at 12w / v% to a mixed solvent of N,N-dimethylacetamide and acetone in a ratio of 1:1, stir until completely dissolved and dispersed, and let stand to degas, which is the shell spinning solution; dissolve polyvinyl pyrrolidone PVPK90 at 16w / v% in anhydrous ethanol, stir until completely dissolved, and let stand to degas, which is the core spinning solution. Coaxial electrospinning was performed using a voltage of 23kV, a receiving distance of 15cm, a shell spinning solution flow rate of 0.6ml / h, and a core spinning solution flow rate of 0.45ml / h to obtain a core-shell nanofiber membrane, which was then immersed in an aqueous solution containing 12w / v% rhamnolipid for washing, drying and crushing to obtain hollow PVDF nanofibers, so that the average length of the fiber is 150μm;
[0031] 2. Preparation of biofilm: Pseudomonas aeruginosa was inoculated into LB medium and cultured by shaking. After culturing for 36 hours, 8 w / v% sterile glass beads with a diameter of 5 mm were added, and then incubated for 22 hours. After filtering, the glass beads were poured into water, vortexed at high speed, and the glass beads were removed with a sieve to obtain a biofilm suspension, so that the polysaccharide content in the biofilm suspension was 14 g / L;
[0032] 3. Fabric finishing: hollow PVDF nanofibers and graphene were added to the biofilm suspension to make the content of hollow PVDF nanofibers 1.2w / v% and the content of graphene 0.4w / v%, and coated on the modal fabric at a dosage of 65ml / m 2 , dried at 130℃ for finalization, the finishing process was repeated 4 times, and then immersed in a solution containing 0.6w / v% dopamine hydrochloride at pH 9.8, treated for 30 minutes, and then washed and dried to obtain a moisture wicking and cool fabric ( Figure 1 ). Figure 1 It can be seen that the biofilm containing graphene is attached to the outside of the hollow nanofibers, forming a three-dimensional network structure with narrow gaps between the fibers, which may be conducive to the capillary action of water diffusion.
[0033] Example 2
[0034] A moisture wicking cool fabric and a preparation method thereof, comprising the following steps:
[0035] 1. Preparation of hollow PVDF nanofibers: Add PVDF with a weight average molecular weight of 600,000 at 15 w / v% to a mixed solvent of N,N-dimethylacetamide and acetone in a ratio of 1:1, stir until completely dissolved and dispersed, and let stand to degas, which is the shell spinning solution; dissolve polyvinyl pyrrolidone PVPK90 in anhydrous ethanol at 20 w / v%, stir until completely dissolved, and let stand to degas, which is the core spinning solution. Coaxial electrospinning was performed using a voltage of 25 kV, a receiving distance of 18 cm, a shell spinning solution flow rate of 0.7 ml / h, and a core spinning solution flow rate of 0.5 ml / h to obtain a core-shell nanofiber membrane, which was then immersed in an aqueous solution containing 15 w / v% Tween 80 for washing, drying and crushing to obtain hollow PVDF nanofibers, so that the average length of the fiber is 10 μm;
[0036] 2. Preparation of biofilm: Pseudomonas aeruginosa was inoculated into LB medium and cultured by shaking. After culturing for 48 hours, 10 w / v% sterile glass beads with a diameter of 4 mm were added, and then incubated for 24 hours. After filtering, the glass beads were poured into water, vortexed at high speed, and the glass beads were removed with a sieve to obtain a biofilm suspension, so that the polysaccharide content in the biofilm suspension was 15 g / L;
[0037] 3. Fabric finishing: hollow PVDF nanofibers and graphene were added to the biofilm suspension to make the content of hollow PVDF nanofibers 1.5w / v% and the content of graphene 0.5w / v%, and coated on the modal fabric at a dosage of 80ml / m 2 , dried at 140℃ for finalizing, the finishing process was repeated 5 times, and then immersed in a solution containing 0.9w / v% dopamine hydrochloride at pH 10. After treatment for 50 minutes, the fabric was washed and dried to obtain a moisture-absorbing and sweat-wicking cooling fabric.
[0038] Example 3
[0039] A moisture wicking cool fabric and a preparation method thereof, comprising the following steps:
[0040] 1. Preparation of hollow PVDF nanofibers: Add PVDF with a weight average molecular weight of 400,000 at 10 w / v% to a mixed solvent of N,N-dimethylacetamide and acetone in a ratio of 1:1, stir until completely dissolved and dispersed, and let stand to degas, which is the shell spinning solution; dissolve polyvinyl pyrrolidone PVPK90 at 8 w / v% in anhydrous ethanol, stir until completely dissolved, and let stand to degas, which is the core spinning solution. Coaxial electrospinning was performed using a voltage of 20 kV, a receiving distance of 12 cm, a shell spinning solution flow rate of 0.5 ml / h, and a core spinning solution flow rate of 0.4 ml / h to obtain a core-shell nanofiber membrane, which was then immersed in an aqueous solution containing 10 w / v% sodium dodecyl sulfate for washing, drying and crushing to obtain hollow PVDF nanofibers, so that the average length of the fiber is 200 μm;
[0041] 2. Preparation of biofilm: Pseudomonas aeruginosa was inoculated into LB medium and cultured by shaking. After culturing for 24 hours, 5 w / v% sterile glass beads with a diameter of 6 mm were added, and then incubated for 20 hours. After filtering, the glass beads were poured into water, vortexed at high speed, and the glass beads were removed with a sieve to obtain a biofilm suspension, so that the polysaccharide content in the biofilm suspension was 10 g / L;
[0042] 3. Fabric finishing: Add hollow PVDF nanofibers and graphene to the biofilm suspension, so that the content of hollow PVDF nanofibers is 1.0 w / v% and the content of graphene is 0.1 w / v%, and coat it on the modal fabric at a dosage of 50 ml / m 2 , dried at 120℃ for finalizing, the finishing process was repeated 3 times, and then immersed in a solution containing 0.4w / v% dopamine hydrochloride at pH 9.5. After treatment for 20 minutes, the fabric was washed and dried to obtain a moisture-absorbing and sweat-wicking cooling fabric.
[0043] Comparative Example 1 (without hollow PVDF nanofibers)
[0044] A fabric and a preparation method thereof, comprising the following steps:
[0045] 1. Preparation of biofilm: Pseudomonas aeruginosa was inoculated into LB medium and cultured by shaking. After culturing for 36 hours, 8 w / v% sterile glass beads with a diameter of 5 mm were added, and then incubated for 22 hours. After filtering, the glass beads were poured into water, vortexed at high speed, and the glass beads were removed with a sieve to obtain a biofilm suspension, so that the polysaccharide content in the biofilm suspension was 14 g / L;
[0046] 2. Fabric finishing: Add graphene to the biofilm suspension to make the graphene content 0.4w / v%, and apply it on the modal fabric at a dosage of 65ml / m 2, dried at 130℃ for finalizing, the finishing process was repeated 4 times, and then immersed in a solution containing 0.6w / v% dopamine hydrochloride at pH 9.8, treated for 30 minutes, and then washed and dried to obtain the fabric.
[0047] Comparative Example 2 (no biofilm)
[0048] A fabric and a preparation method thereof, comprising the following steps:
[0049] 1. Preparation of hollow PVDF nanofibers: Add PVDF with a weight average molecular weight of 500,000 at 12w / v% to a mixed solvent of N,N-dimethylacetamide and acetone in a ratio of 1:1, stir until completely dissolved and dispersed, and let stand to degas, which is the shell spinning solution; dissolve polyvinyl pyrrolidone PVPK90 at 16w / v% in anhydrous ethanol, stir until completely dissolved, and let stand to degas, which is the core spinning solution. Coaxial electrospinning was performed using a voltage of 23kV, a receiving distance of 15cm, a shell spinning solution flow rate of 0.6ml / h, and a core spinning solution flow rate of 0.45ml / h to obtain a core-shell nanofiber membrane, which was then immersed in an aqueous solution containing 12w / v% rhamnolipid for washing, drying and crushing to obtain hollow PVDF nanofibers, so that the average length of the fiber is 150μm;
[0050] 2. Fabric finishing: Add hollow PVDF nanofibers and graphene into water, so that the content of hollow PVDF nanofibers is 1.2w / v% and the content of graphene is 0.4w / v%, and apply it on modal fabric at a dosage of 65ml / m 2 , dried at 130℃ for finalizing, the finishing process was repeated 4 times, and then immersed in a solution containing 0.6w / v% dopamine hydrochloride at pH 9.8, treated for 30 minutes, and then washed and dried to obtain the fabric.
[0051] Comparative Example 3 (without graphene)
[0052] A fabric and a preparation method thereof, comprising the following steps:
[0053] 1. Preparation of hollow PVDF nanofibers: Add PVDF with a weight average molecular weight of 500,000 at 12w / v% to a mixed solvent of N,N-dimethylacetamide and acetone in a ratio of 1:1, stir until completely dissolved and dispersed, and let stand to degas, which is the shell spinning solution; dissolve polyvinyl pyrrolidone PVPK90 at 16w / v% in anhydrous ethanol, stir until completely dissolved, and let stand to degas, which is the core spinning solution. Coaxial electrospinning was performed using a voltage of 23kV, a receiving distance of 15cm, a shell spinning solution flow rate of 0.6ml / h, and a core spinning solution flow rate of 0.45ml / h to obtain a core-shell nanofiber membrane, which was then immersed in an aqueous solution containing 12w / v% rhamnolipid for washing, drying and crushing to obtain hollow PVDF nanofibers, so that the average length of the fiber is 150μm;
[0054] 2. Preparation of biofilm: Pseudomonas aeruginosa was inoculated into LB medium and cultured by shaking. After culturing for 36 hours, 8 w / v% sterile glass beads with a diameter of 5 mm were added, and then incubated for 22 hours. After filtering, the glass beads were poured into water, vortexed at high speed, and the glass beads were removed with a sieve to obtain a biofilm suspension, so that the polysaccharide content in the biofilm suspension was 14 g / L;
[0055] 3. Fabric finishing: Add hollow PVDF nanofibers to the biofilm suspension to make the content of hollow PVDF nanofibers 1.2w / v%, and coat them on the modal fabric at a dosage of 65ml / m 2 , dried at 130℃ for finalizing, the finishing process was repeated 4 times, and then immersed in a solution containing 0.6w / v% dopamine hydrochloride at pH 9.8, treated for 30 minutes, and then washed and dried to obtain the fabric.
[0056] Moisture absorption and quick drying test
[0057] According to the national standard GB / T21655.1-2008 "Evaluation of Moisture Absorption and Quick-drying Properties of Textiles Part 1: Single Item Combined Test Method", the test was carried out under the conditions of humidity 60%, temperature 20°C and standard air pressure. The moisture absorption performance of the fabrics of Examples 1-3 and Comparative Examples 1-3 and the modal fabric was evaluated by water absorption rate and water drop diffusion time; the quick-drying performance of each sample fabric was evaluated by evaporation rate. The results are shown in Table 1.
[0058] Table 1 Test results of moisture absorption and quick drying of fabrics
[0059] sample Water absorption / % Droplet diffusion time / s 40 minutes residual water rate / % Water evaporation rate / (g / h) Modal fabric 207 2.5 25 0.10 Example 1 358 0.5 4 2.66 Example 2 347 0.7 6 2.51 Example 3 353 0.7 5 2.34 Comparative Example 1 249 2.3 22 0.14 Comparative Example 2 210 2.2 17 0.17 Comparative Example 3 298 2.0 20 0.13
[0060] As can be seen from Table 1, the hygroscopicity index and quick-drying index of the fabric prepared in the embodiment have reached the requirements of the standard, and both have excellent hygroscopic and quick-drying performance. After 40 minutes of drying time, the total residual water rate of the fabric is lower than the 13% recognized by the standard, and the evaporation rate is greater than the 0.18g / h recognized by the standard. Although the water absorption rate and drip diffusion time of the base fabric modal fabric and the fabric prepared in the comparative example have reached 200% and 3s recognized by the standard in hygroscopicity, the quick-drying characteristics are poor. The reason why the fabric of the embodiment has good quick-drying property is determined by the finishing and surface structure of the fabric. The polydopamine and biofilm on the surface have strong hygroscopicity, and then rely on graphene to transfer heat and the hollow PVDF nanofibers to absorb heat and control the evaporation of water, which is conducive to the transfer of a small amount of water contained in the interior to the outer surface, thereby increasing the evaporation area of water and improving the evaporation rate. The fabric prepared in comparative example 1 has no hollow PVDF nanofibers, which affects the three-dimensional mesh structure of the fabric surface, reduces the water absorption of the fabric, and affects the heat pipe effect and the evaporation and discharge of water. Comparative Example 2 has no biofilm, which directly affects the three-dimensional network structure of the fabric surface, reduces the water absorption of the fabric, and is only close to the raw material base fabric. In addition, the hollow PVDF nanofibers and graphene are highly hydrophobic, which will also affect the synthesis of polydopamine on its surface, and also affect its affinity and water absorption to the skin. Comparative Example 3 has no graphene. Graphene is a lamellar structure and is an important component of the three-dimensional network structure on the surface of the fabric of the embodiment of the present invention. The lack of it will lead to defects in the three-dimensional network structure, reduce water absorption, and affect the thermal conductivity of the fabric surface, limiting the evaporation of water.
[0061] Cooling performance test
[0062] Refer to GB / T35263-2017 "Testing and Evaluation of Instantaneous Cooling Performance of Textiles upon Contact" to test the cooling performance of Example 1-3 and Comparative Example 1-3 fabrics and Modal fabrics. The test method for instant cooling is: the fabric sample is placed between the cold plate (20±0.5℃ below) and the hot plate (35±0.5℃ above) platform, and the polyethylene surface contacts the hot plate with a layer of water film (simulating human skin). The highest value is reached about 0.2s after the instant of contact, and the entire test is completed within 10s. The test hot plate area is 9cm 2 The temperature difference between the cold and hot plates in the test is 15°C. The instantaneous coolness of the fabric is tested on the fabric coolness tester. The heat flow transfer test is carried out to test the fabric contact temperature and coolness, that is, the instantaneous coolness value q max (W / cm 2 ), the test results are shown in Table 2.
[0063] Table 2 Test results of instant cool feeling of fabrics
[0064] sample <![CDATA[Instantaneous cool feeling value q max (W / cm 2 )]]> Modal fabric 0.14 Example 1 0.218 Example 2 0.214 Example 3 0.209 Comparative Example 1 0.168 Comparative Example 2 0.172 Comparative Example 3 0.154
[0065] It can be seen from Table 2 that the fabric prepared in the embodiment has a good cooling effect, while the fabric prepared in the comparative example is inferior. The cooling effect of the fabric in the embodiment comes from the latent heat taken away by water evaporation and the rapid heat transfer to the outside by heat conduction such as graphene. The fabric prepared in comparative example 1 does not have hollow PVDF nanofibers, which affects the heat pipe effect and the evaporation and discharge of water, so the cooling effect is not good. Comparative example 2 has no biofilm, which directly affects the three-dimensional network structure on the surface of the fabric and reduces the water absorption of the fabric. Water evaporation is required to take away the latent heat. The lack of water retention of the biofilm will cause a poor cooling effect. Comparative example 3 has no graphene. Graphene is a lamellar structure and is an important component of the three-dimensional network structure on the surface of the fabric in the embodiment of the present invention. The lack of it will lead to defects in the three-dimensional network structure, reduce water absorption, and affect the thermal conductivity of the fabric surface, limit the evaporation of water, and significantly reduce the cooling performance.
[0066] The present invention provides a moisture wicking cool fabric and a method for preparing the same. There are many methods and approaches to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be considered as the scope of protection of the present invention. All components not specified in this embodiment can be implemented using existing technologies.
Claims
1. A method for preparing a moisture wicking cool fabric, characterized in that: The preparation method comprises the following steps: S1. Coaxially electrospinning the shell layer spinning solution and the core layer spinning solution to obtain a core-shell nanofiber membrane, immersing the core-shell nanofiber membrane in an aqueous solution containing a surfactant, washing, drying and crushing the membrane to obtain a hollow PVDF nanofiber; the shell layer spinning solution is a polyvinylidene fluoride solution, and the core layer spinning solution is a polyvinyl pyrrolidone solution; S2. Preparation of biofilm: Pseudomonas aeruginosa was inoculated into LB medium, and glass beads were added after shaking culture for 24-48 hours, and then incubated for 20-24 hours. After filtering, the glass beads were poured into water, and the biofilm suspension was obtained after high-speed vortexing to remove the glass beads; S3. Fabric finishing: adding the hollow PVDF nanofibers and graphene to the biofilm suspension to obtain a finishing liquid; using the finishing liquid to finish the modal fabric, repeating the finishing process 3-5 times, and then immersing in a dopamine hydrochloride solution for treatment, taking out and washing and drying to obtain a moisture-absorbing, perspiration-wicking, cooling fabric.
2. The preparation method according to claim 1, characterized in that: In step S1, the shell spinning solution is prepared by adding polyvinylidene fluoride into a mixed solvent of N,N-dimethylacetamide and acetone, wherein the weight average molecular weight of the polyvinylidene fluoride is 400,000-600,000, and the concentration of the polyvinylidene fluoride is 10-15 w / v%.
3. The preparation method according to claim 1, characterized in that: In step S1, the core layer spinning solution is prepared by dissolving polyvinyl pyrrolidone in anhydrous ethanol, the polyvinyl pyrrolidone is polyvinyl pyrrolidone PVPK90, and the concentration of polyvinyl pyrrolidone in the core layer spinning solution is 8-20w / v%.
4. The preparation method according to claim 1, characterized in that: In step S1, the coaxial electrospinning conditions are: voltage 20-25 kV, receiving distance 12-18 cm, shell layer spinning solution flow rate 0.5-0.7 ml / h, core layer spinning solution flow rate 0.4-0.5 ml / h.
5. The preparation method according to claim 1, characterized in that: In step S1, in the aqueous solution containing a surfactant, the surfactant is one of Tween 80, rhamnolipid and sodium dodecyl sulfate, and the concentration is 10-15 w / v%.
6. The preparation method according to claim 1, characterized in that: In step S1, the average length of the hollow PVDF nanofibers is 10-200 μm.
7. The preparation method according to claim 1, characterized in that: In step S3, the finishing process specifically comprises: applying the finishing liquid on the modal fabric, and drying and shaping at 120-140°C.
8. The preparation method according to claim 1, characterized in that: In step S3, in the finishing liquid, the concentration of the hollow PVDF nanofibers is 1.0-1.5 w / v%, and the concentration of graphene is 0.1-0.5 w / v%.
9. The preparation method according to claim 8, characterized in that: In step S3, the amount of the finishing liquid is 50-80 ml / m 2 ; The dopamine hydrochloride solution has a pH of 9.5-10.0 and a concentration of 0.4-0.9 w / v%.
10. A moisture absorbing and perspiration wicking cool fabric prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of anti-fouling and sun-resistant composite functional fabric, fabric prepared through preparation method and clothes containing fabric
CN108103778A
Moisture-conducting heat-dissipating cool-feeling fabric and preparation method thereof
CN113605098A
Surface-modified PVDF (polyvinylidene fluoride) anti-fouling hydrophilic membrane as well as one-step preparation process and application thereof
CN114471185A