Anti-erasing thermosensitive printing paper and preparation method thereof
By adding transparent top coating and improving coating formula on medical thermal printing paper, combined with curtain coating process, the problem of text blurring and image disappearance after contact with alcohol is solved, achieving efficient images Save and clear scanning and reading improve image preservation and anti-alcohol penetration performance.
Patent Information
- Application Number
- CN202411036602.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing medical thermal printing paper prints unclear text after contacting alcohol, abnormal barcode scanning and reading, and low image storage rate, resulting in inconvenience during use.
Add a transparent top coating to the color development layer, adopting a stronger coating formula and curtain coating process, preventing alcohol penetration, improving image preservation and printing through the combination of base coating, top coating and top coating Color rendering sensitivity.
It has achieved good barcode information scanning and reading, image storage rate ≥85%, strong anti-alcohol penetration performance, improved clarity and retention rate of the chromogenic layer, and reduced production costs.
Smart Images

Figure CN118996913A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal printing paper manufacturing, and relates to thermal printing paper with anti-erasing function and a preparation method thereof. Background Art
[0002] Medical thermal printing paper with anti-erasing function is mainly used for printing labels in medical occasions. Because medical staff often touch alcohol and then touch the labels on patients' infusion bottles with their hands, the handwriting on the record label will be dissolved by alcohol and become blurred or disappear, resulting in incomplete information recorded on the label. Existing medical thermal printing paper has the following shortcomings: 1. Before printing, the text printed by the thermal paper is not clear after contacting alcohol, and the barcode scanning and reading are not normal; 2. After printing, the image will be dissolved after the thermal paper contacts alcohol, and the preservation rate is less than 60%. The above shortcomings will cause great inconvenience in the use of thermal printing paper. Summary of the invention
[0003] To solve these deficiencies, the present invention provides a thermal printing paper with anti-erasing function and its manufacturing process and method by adjusting the product structure, coating formula and production process. The thermal printing paper is particularly suitable for use in the medical field.
[0004] The present invention makes improvements in the following three aspects to obtain thermal printing paper that is resistant to erasure: 1. A transparent top coating layer is added on the color developing layer to protect the color developing layer and prevent alcohol from penetrating into the color developing layer and damaging it; 2. A coating formula with stronger color development is adopted; 3. A curtain coating process is adopted to ensure a more precise coating amount, uniform coverage, and protection without dead angles.
[0005] The anti-erasing thermal printing paper comprises a substrate layer at the bottom, a primer layer above the substrate layer, a surface coating layer above the primer layer and a top coating layer above the surface coating layer, wherein the coating amounts of the primer layer, the surface coating layer and the top coating layer are 4-5g / ㎡, 3-4g / ㎡ and 1-3g / ㎡ per square meter respectively.
[0006] The substrate layer is made of base paper, and the base paper is 40-70g / ㎡ pure wood pulp base paper.
[0007] The base coating is made of kaolin, PVA, styrene-butadiene latex, hollow ball pigment and other raw materials, and its main functions are:
[0008] A. Filling and increasing the coverage rate: improving the flatness of the original paper surface and the opacity of the paper during the coating process;
[0009] B. Prevent penetration: prevent the effective ingredients of the primer coating from penetrating into the substrate layer (base paper);
[0010] C. Reduce heat loss: During the printing process, the heat energy is concentrated on the color development layer instead of being conducted to the substrate layer, so that a small amount of thermal sensitive coating can be applied to obtain higher printing color development sensitivity and speed, thereby reducing production costs.
[0011] The top coating is a mixture of PVA, developer grinding fluid, colorless dye grinding fluid, sensitizer and styrene-butadiene latex and other raw materials. Its main function is: when the thermal paper is printed, the print head heats up (also called a thermal head), instantly heating the paper surface it contacts, so that the colorless dye molecules in the thermochromic layer of the heated part of the paper surface react with the developer, that is, they become colored dyes, thereby displaying the color of the font or pattern.
[0012] The top coating is made of kaolin, silicon dioxide, PVA, zinc stearate, organic solvent resistance, lubricant and crosslinking agent, and its main functions are:
[0013] 1) Isolation protection: It is mainly a mixture of silica + anti-organic solvent. A layer of organic material is coated on the surface of silica to form a silica structure, namely, fumed silica. Due to its small particle size, it has hydrophobic properties to inhibit flow after forming a network structure. In addition, the role of PVA and cross-linking agents cross-links and bonds the molecular chains together to improve the bonding effect. It has good sealing and anti-permeability, establishes a penetration barrier, prevents alcohol, water, oil, etc. from penetrating into the color developing layer to destroy the printed pattern, and plays a protective role such as anti-erasure.
[0014] 2) Improve smoothness: mainly add lubricants and zinc stearate, and combine with pressure shaping during production to improve the surface smoothness, brightness and light stability of thermal paper.
[0015] 3) Prevent adhesion: The main component of the top coating is kaolin, which is mixed and cross-linked with other raw materials to form a very smooth, flat, non-sticky thin layer, which can prevent the top coating from adhering to the print head. At the same time, kaolin has a heat conduction function and does not hinder the transfer of heat during printing to affect the color development effect.
[0016] The present invention also provides a method for preparing the above-mentioned anti-erasure thermal printing paper, and the preparation method is as follows:
[0017] Step 1): Material preparation
[0018] Basecoat coating formulation
[0019] According to the ratio and order of adding in the base coating ratio table (see Table 1), the raw materials are added into the stirring kettle in sequence, and stirred at the specified speed and time after adding, and a base coating with a solid content of 30-35% is obtained after mixing. The mass ratio of water, calcined kaolin, PVA glue, styrene-butadiene latex and pigment is 205-220:51-55:2-4:11-15:30-34:
[0020]
[0021] Table 1 Primer coating ratio
[0022] Topcoat coating formulation;
[0023] According to the ratio and order of adding in the top coating ratio table (see Table 2), the raw materials are added into the stirring kettle in turn, stirred at the specified speed and time after adding, and a top coating with a solid content of 25-32% is obtained after mixing. The mass ratio of water, PVA glue, developer grinding liquid, colorless dye grinding liquid, sensitizer grinding liquid and styrene-butadiene latex is 190-210:17-20:38-42:20-24:9-11:8-11.
[0024]
[0025] Table 2 Topcoat coating ratio
[0026] Top coat coating formulation
[0027] According to the ratio and addition order in the top coating ratio table (see Table 3), the raw materials are added to the stirring and dispersing tank in sequence, and stirred at the specified speed and time after addition, and a top coating with a solid content of 18-22% is obtained after mixing. The mass ratio of kaolin dispersion, silicon dioxide dispersion, PVA glue, zinc stearate, anti-organic solvent mixed solution, lubricant, crosslinking agent, defoamer and water is 23-26: 13-15: 17-19: 10-13: 4-6: 15-17: 8-10: 0.3-0.5: 390-410.
[0028]
[0029]
[0030] Table 3 Top coating paint ratio table
[0031] Step 2): Prepare anti-erasing thermal printing paper
[0032] The multifunctional thermal paper curtain coating machine with a machine speed of 500 meters per minute is used for coating production. The multifunctional thermal paper coating equipment is mainly composed of a winding and unwinding system, a curtain coating system, a drying system, a transmission system, an electrical control system, etc. The drying system consists of 18 sets of hot air ovens. Through curtain coating, the base coating, top coating and top coating of medical triple-proof thermal paper can be completed at a high speed of 500 meters per minute, and the paper surface shaping and / calendering can be completed at one time.
[0033] 2.1) Base material layer: The base paper has a width of 1560mm-1760mm and is made of pure wood pulp paper of 40-70g / ㎡.
[0034] 2.2) Applying the primer coating for the first time and then drying to form a primer coating;
[0035] 2.3) Applying a second coat of topcoat paint, followed by drying, to form a topcoat;
[0036] 2.4) coating the top coating material for the third time, and then drying to form a top coating layer;
[0037] 2.5) Shaping and calendering: The coated paper is shaped by solid cast iron rollers and rubber-coated soft rollers under the action of a hydraulic system pressurized at 150KN / m to improve the smoothness and brightness of the paper. The anti-marking thermal printing paper can be obtained by rolling and packaging.
[0038] The coating amounts of the primer, topcoat and upper coating are 4-5g / ㎡, 3-4g / ㎡ and 1-3g / ㎡ respectively.
[0039] The drying temperature is controlled between 80℃-120℃.
[0040] The moisture content of the finished paper after coating and drying is controlled at 6.0%-7.5%.
[0041] The beneficial effects of the present invention are:
[0042] 1. The barcode information is well scanned and read. The non-direct curtain coating method is adopted, which causes less damage to the base coating and the top coating. The coating is thin and uniform (low cost), the display is clearer, and the barcode is well scanned and read.
[0043] 2. Higher image preservation rate. The formula of the base coat and top coat is adjusted to improve the water resistance and oil resistance of thermal paper, making the image preservation rate ≥85%.
[0044] 3. The top coating provides an anti-penetration barrier layer against alcohol penetration, thereby effectively preventing alcohol from penetrating into the thermal color-developing layer and avoiding the color degradation of the thermal color-developing layer, which causes blurring or disappearance of handwriting or patterns, thereby improving the retention rate of thermal paper and its anti-alcohol penetration performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a simple structural schematic diagram of the anti-erasure thermal printing paper of the present invention;
[0046] Figure 2 The present invention is a flow chart for preparing the anti-erasure thermal printing paper. DETAILED DESCRIPTION
[0047] Example 1
[0048] Step 1): Material preparation
[0049] The specifications of the base paper are 1560mm in width and 55g / ㎡ pure wood pulp paper.
[0050] Basecoat coating formulation
[0051] According to the ratio and addition order in the primer coating ratio table (see Table 1), the raw materials are added to the stirring kettle in sequence, and after adding, they are stirred at the specified speed and time to obtain a primer coating with a solid content of 31% after mixing.
[0052]
[0053] Table 1 Primer coating ratio
[0054] Topcoat coating formulation;
[0055] According to the ratio and order of adding in the top coating ratio table (see Table 2), the raw materials are added to the stirring kettle in sequence, and after adding, they are stirred at the specified speed and time to obtain a top coating with a solid content of 32% after mixing.
[0056]
[0057]
[0058] Table 2 Topcoat coating ratio
[0059] Top coat coating formulation
[0060] According to the ratio and addition order in the top coating paint ratio table (see Table 3), the raw materials are added to the stirring and dispersing tank in sequence, and after adding, they are stirred at the specified speed and time to obtain a top coating paint with a solid content of 19% after mixing.
[0061]
[0062]
[0063] Table 3 Top coating paint ratio table
[0064] Step 2): Prepare anti-erasing thermal printing paper
[0065] The multifunctional thermal paper curtain coating machine with a machine speed of 500 meters per minute is used for coating production. The multifunctional thermal paper coating equipment is mainly composed of a winding and unwinding system, a curtain coating system, a drying system, a transmission system, an electrical control system, etc. The drying system consists of 18 sets of hot air ovens. Through curtain coating, the base coating, top coating and top coating of medical triple-proof thermal paper can be completed at a high speed of 500 meters per minute, and the paper surface shaping and / calendering can be completed at one time.
[0066] 2.1) Prepare the base material layer: The base paper has a width of 1560mm-1760mm and is made of pure wood pulp paper of 40-70g / ㎡.
[0067] 2.2) Applying the primer coating for the first time and then drying to form a primer coating;
[0068] 2.3) Applying a second coat of topcoat paint, followed by drying, to form a topcoat;
[0069] 2.4) coating the top coating material for the third time, and then drying to form a top coating layer;
[0070] 2.5) Shaping and calendering: The coated paper is shaped by solid cast iron rollers and rubber-coated soft rollers under the action of a hydraulic system pressurized at 150KN / m to improve the smoothness and brightness of the paper. The anti-marking thermal printing paper can be obtained by rolling and packaging.
[0071] The coating amounts of the primer, topcoat and upper coating are 4-5g / ㎡, 3-4g / ㎡ and 1-3g / ㎡ respectively.
[0072] The drying temperature is controlled between 80℃-120℃.
[0073] The moisture content of the finished paper after coating and drying is controlled at 6.0%-7.5%.
[0074] Example 2 was carried out according to the same production process and formula. The base paper used in Example 2 was pure wood pulp paper with a width of 1560 mm and a weight of 58 g / m2.
[0075] Performance Testing
[0076] The various technical indicators of the printing paper of Example 1 and Example 2 after coating were tested, and the test results are shown in Table 4 below:
[0077]
[0078]
[0079] Table 4.
Claims
1. A thermal printing paper that prevents erasure, characterized in that: The anti-erasing thermal printing paper comprises a substrate layer at the bottom, a primer layer above the substrate layer, a surface coating layer above the primer layer and a top coating layer above the surface coating layer, wherein the coating amounts of the primer layer, the surface coating layer and the top coating layer are 4-5 g / ㎡, 3-4 g / ㎡ and 1-3 g / ㎡ per square meter respectively.
2. The thermal printing paper according to claim 1, characterized in that: The primer layer is prepared from water, calcined kaolin, PVA glue, styrene-butadiene latex and pigment in the following mass ratio of 205-220:51-55:2-4:11-15:30-34.
3. The thermal printing paper according to claim 1, characterized in that: The top coating is prepared from water, PVA glue, developer grinding liquid, colorless dye grinding liquid, sensitizer grinding liquid and styrene-butadiene latex in the following mass ratio of 190-210:17-20:38-42:20-24:9-11:8-11.
4. The thermal printing paper according to claim 1, characterized in that: The top coating is prepared from kaolin dispersion, silicon dioxide dispersion, PVA glue, zinc stearate, anti-organic solvent mixed solution, lubricant, crosslinking agent, defoaming agent and water in the following mass ratio of 23-26:13-15:17-19:10-13:4-6:15-17:8-10:0.3-0.5:390-410.
5. The method for preparing thermal printing paper according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Step 1): Prepare a primer coating, a top coating coating and a top coating coating according to parts by mass; Step 2): Prepare anti-erasing thermal printing paper: 2.1) Prepare the base material layer: the base paper is 1560mm-1760mm wide and 40-70g / ㎡ pure wood pulp paper; 2.2) Use the primer coating material for the first coating, and then dry it to form a primer coating; 2.3) Apply the topcoat paint for the second time and then dry it to form a topcoat; 2.4) Apply the top coating paint for the third time and then dry it to form a top coating; 2.5) After shaping and calendering, the anti-erasure thermal printing paper can be obtained by rolling and packaging; The coating amounts of the base coating, top coating and top coating are 4-5g / ㎡, 3-4g / ㎡ and 1-3g / ㎡ respectively; The drying temperature is controlled between 80℃-120℃; The moisture content of the finished paper after coating and drying is controlled at 6.0%-7.5%.
6. The method for preparing thermal printing paper according to claim 5, characterized in that: The three coating processes are carried out using a multifunctional thermal paper curtain coating machine with a machine speed of 500 meters per minute.
Citation Information
Patent Citations
Heat sensitive paper applicable to tags without bottom paper and manufacturing method of heat sensitive paper
CN110055816A
Heat sensitive paper
CN1472390A
Cited By
Partitioned coating experiment system and method for research and development of heat-sensitive materials