Visual stretchable pressure sensor based on mechanoluminescence microcolumn and preparation method thereof
Through visual stretchable pressure sensor based on force-radiation micropillar, the problem of low spatial resolution and long response time of flexible pressure sensors in pressure distribution detection is solved, and high sensitivity and visual pressure sensing is achieved, which improves the Application value.
Patent Information
- Application Number
- CN202411097358.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing flexible pressure sensors have problems such as low spatial resolution, difficulty in visualization, and long response time in pressure distribution detection, resulting in low equipment feedback and incomplete and inaccurate signal acquisition.
Using a visual stretchable pressure sensor based on a force-ellow-emission microcolumn, spin-coating is performed by preparing a silicon wafer mold with a micro-pit array, and mixing the force-emiting particles with polydimethylsiloxane monomer and crosslinking agent. and thermal curing to form a force-ellow-luminescent composite material, and prepare a force-ellow-luminescent microcolumn and film to achieve high sensitivity and visual pressure sensing.
It improves the spatial resolution and response speed of the pressure sensor, can directly convert the pressure signal into visible light signals without external power, realize real-time visualization of pressure distribution, and has high sensitivity and stretchability, deepening its application value.
Smart Images

Figure CN118999860A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of optical sensing technology, and in particular to a visualized stretchable pressure sensor based on a mechanoluminescent microcolumn and a preparation method thereof. Background Art
[0002] Electronic skin can sense the external physical world like human skin and convert the signals of the external physical world into electrical signals or optical signals. It is a bridge to connect the physical world to the digital world and has great application potential in health monitoring, augmented reality (AR) and human-computer interface. Usually, electronic skin is composed of a large number of flexible pressure sensors, which detect the pressure distribution on a complex three-dimensional surface to obtain the corresponding signal for subsequent analysis of the intelligent perception system. However, the current flexible pressure sensors have gradually shown their limitations in some applications, including low spatial resolution of pressure distribution detection, easy crosstalk, delayed response, etc., resulting in practical application problems such as low feedback of equipment, incomplete and inaccurate signal acquisition. This is because the pressure distribution detection is usually realized by a plurality of flexible pressure sensor arrays arranged vertically and horizontally. The output of each sensing unit reflects the pressure situation at the corresponding position. It is difficult to reduce the size of a single sensing unit, which makes the spatial resolution of pressure distribution detection low.
[0003] In addition, the current flexible pressure sensors directly output electrical signals, making it difficult to intuitively display the actual distribution of pressure; at the same time, the current flexible pressure sensors have problems such as low spatial pressure distribution resolution, difficulty in visualization, and long response time. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a visualized stretchable pressure sensor based on piezoluminescent microcolumns and a preparation method, which solves the problems of low spatial pressure distribution resolution, difficulty in visualization, and long response time in current flexible pressure sensors. The pressure sensor has the properties of high sensitivity, visualization, and stretchability, has good application prospects, and deepens its application value.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] A method for preparing a visualized stretchable pressure sensor based on a mechanoluminescent microcolumn comprises the following steps:
[0007] preparing a silicon wafer mold having a micropit array;
[0008] The mechanoluminescent particles and the polydimethylsiloxane monomer are mixed and stirred, and then a cross-linking agent is added and mixed and stirred uniformly to obtain a mixture;
[0009] Covering the mixture on the surface of the silicon wafer mold and evenly spin coating it with a spin coater;
[0010] placing the silicon wafer mold covered with the mixture into an oven for thermal curing to obtain a mesoluminescent composite material;
[0011] The mechanoluminescent composite material is peeled off from the silicon wafer mold by using tweezers to obtain connected mechanoluminescent microcolumns and mechanoluminescent films, thus preparing a pressure sensor.
[0012] Preferably, the preparation of a silicon wafer mold with a micro-pit array includes: preparing a mask plate with a circular hole array structure, the diameter of the circular holes of the mask plate is 30 to 200 μm, and the center spacing of the circular holes is 60 to 400 μm; then spin coating photoresist on the silicon wafer, and combining the silicon wafer evenly coated with photoresist with the mask plate for photolithography; then completing the preparation of the silicon wafer mold by deep silicon etching.
[0013] Preferably, the depth of the micro-pits on the silicon wafer is 30-100 μm.
[0014] Preferably, the mechanoluminescent particles are mixed with polydimethylsiloxane monomers, and then a cross-linking agent is added and mixed evenly to obtain a mixture, including: the mechanoluminescent particles are composed of ZnS:Cu / ZnS:Mn particles, and the mass ratio of the mechanoluminescent particles to the polydimethylsiloxane monomer is 0.5:1 to 3:1.
[0015] Preferably, the crosslinking agent is SYLGARD 184 SILICONE ELASTOMER CURINGAGENT, and the weight ratio of the polydimethylsiloxane monomer to the crosslinking agent is 8 to 12:1.
[0016] Preferably, the silicon wafer mold covered with the mixture is placed in an oven for thermal curing to obtain the mesoluminescent composite material, including: the temperature of the oven is 80-100° C., and the thermal curing time is 60-120 min.
[0017] The present invention also provides a visualized stretchable pressure sensor based on mesoluminescent microcolumns, and the pressure sensor is prepared by the preparation method provided above; the pressure sensor includes the mesoluminescent microcolumns and the mesoluminescent film from top to bottom, and the mesoluminescent microcolumns are connected to the mesoluminescent film.
[0018] Preferably, the mechanoluminescent microcolumns and the mechanoluminescent film are both composed of polydimethylsiloxane and ZnS:Cu / ZnS:Mn particles, and the mechanoluminescent microcolumns have a diameter of 30 μm, a center spacing of 60 to 400 μm, and a height of 30 to 200 μm.
[0019] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:
[0020] (1) Compared with the existing flexible pressure sensors for planar pressure distribution, the present invention has a mechanoluminescent micro-column array structure. The surface of the micro-columns has a small contact area with the pressure application surface, which can cause a sharp increase in the force applied to the ZnS:Cu / ZnS:Mn particles under a small pressure. When the threshold of all pressures of the ZnS:Cu / ZnS:Mn particles is reached, green or orange visible light will be emitted, which greatly improves the sensitivity of the sensor to external pressure.
[0021] (2) The visualized stretchable pressure sensor provided by the present invention utilizes the characteristic of spontaneous luminescence of mesoluminescent materials under stress, so that the sensor can directly convert the pressure signal into an optical signal visible to the naked eye without the need for an external power supply. Compared with other technologies, the pressure distribution display is more intuitive, and real-time visualization of the pressure distribution can be achieved. In addition, the sensor has a simple composition, consisting of polydimethylsiloxane and ZnS:Cu / ZnS:Mn particles. Polydimethylsiloxane is stretchable, which makes the entire device stretchable. Compared with existing technologies, the sensor can simultaneously possess the properties of high sensitivity, visualization, and stretchability, has good application prospects, and deepens its application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 It is a flow chart of a method for preparing a visualized stretchable pressure sensor based on mesoluminescent microcolumns of the present invention;
[0024] Figure 2 A schematic diagram of the structure of a visualized stretchable pressure sensor based on mechanoluminescent microcolumns according to the present invention;
[0025] Figure 3 This is a scanning electron microscope cross-sectional view of the microstructure of a visualized stretchable pressure sensor based on mesoluminescent micropillars of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] Embodiment 1
[0029] like Figure 1 As shown, the present invention provides a method for preparing a visualized stretchable pressure sensor based on a mechanoluminescent microcolumn, comprising the following steps:
[0030] Step 100: preparing a silicon wafer mold having a micro-pit array;
[0031] Step 200: Mixing the mesoluminescent particles and the polydimethylsiloxane monomer, and then adding a cross-linking agent and mixing them evenly to obtain a mixture;
[0032] Step 300: Covering the mixture on the surface of the silicon wafer mold and evenly spin coating it using a spin coater;
[0033] Step 400: placing the silicon wafer mold covered with the mixture into an oven for thermal curing to obtain a mesoluminescent composite material;
[0034] Step 500: peeling the mesoluminescent composite material from the silicon wafer mold by using tweezers to obtain connected mesoluminescent microcolumns and mesoluminescent films, that is, preparing a pressure sensor.
[0035] In the above steps, step 100 specifically includes: preparing a mask plate with a circular hole array structure, wherein the diameter of the circular holes of the mask plate is 30 to 200 μm, and the center spacing of the circular holes is 60 to 400 μm; then, spin-coating photoresist on a silicon wafer, and combining the silicon wafer uniformly coated with the photoresist with the mask plate for photolithography; then, completing the preparation of the silicon wafer mold by deep silicon etching. Specifically, the depth of the micro-pits on the silicon wafer is 30 to 100 μm.
[0036] In step 200, the mechanoluminescent particles are mixed with polydimethylsiloxane monomers, and then a cross-linking agent is added and mixed evenly to obtain a mixture, including: the mechanoluminescent particles are composed of ZnS:Cu / ZnS:Mn particles, and the mass ratio of the mechanoluminescent particles to the polydimethylsiloxane monomer is 0.5:1 to 3:1.
[0037] More specifically, the crosslinking agent is SYLGARD 184 SILICONE ELASTOMER CURINGAGENT, and the weight ratio of the polydimethylsiloxane monomer to the crosslinking agent is 8-12:1.
[0038] In step 400, the silicon wafer mold covered with the mixture is placed in an oven for thermal curing to obtain a mesoluminescent composite material, including: the temperature of the oven is 80-100° C., and the thermal curing time is 60-120 minutes.
[0039] The preparation method provided above is used to prepare Figure 2 The visualized stretchable pressure sensor shown in the figure includes the mechanoluminescent microcolumn and the mechanoluminescent film from top to bottom, wherein the mechanoluminescent microcolumn is connected to the mechanoluminescent film. In addition, the mechanoluminescent microcolumn and the mechanoluminescent film are both composed of polydimethylsiloxane and ZnS:Cu / ZnS:Mn particles, referring to Figure 3 The diameter of the mesoluminescent microcolumn is 30 μm, the center distance is 60 to 400 μm, and the height is 30 to 200 μm.
[0040] Specific application: Place the visualized stretchable pressure sensor on a hard base. When an object with a certain pattern exerts a certain force on the force-induced luminescent microcolumns, the force-induced luminescent microcolumns under contact will generate visible light, corresponding to the pattern of the object exerting the force. The stronger the applied pressure, the greater the intensity of visible light generated by the force-induced luminescent microcolumns. The pattern of the light emitted by the force-induced luminescent microcolumns can be collected by a camera, and the pressure of the object at different positions can be displayed. In addition, the visualized stretchable pressure sensor provided in this embodiment has a 1520kPa -1 It has a sensitivity of 100kPa, a pressure sensing accuracy of 80kPa, and a high plane pressure mapping resolution of over 400dpi.
[0041] Therefore, in this embodiment, a flexible pressure sensor is obtained by using a mechanoluminescent microcolumn array prepared by polydimethylsiloxane (PDMS) and ZnS:Cu / ZnS:Mn particles. In terms of sensitivity and resolution, the mechanoluminescent microcolumn array in the prepared pressure sensor structure is composed of microcolumns at a certain distance, and the microcolumns are composed of polydimethylsiloxane and ZnS:Cu / ZnS:Mn particles, which can form an array of luminescent microstructures. There is a small contact area between the surface of this microcolumn and the pressure application surface, which can cause a sharp increase in the force of the ZnS:Cu / ZnS:Mn particles under a small pressure. When the threshold of all the pressure of the ZnS:Cu / ZnS:Mn particles is reached, green or orange visible light will be emitted, so that the sensitivity and response time of the sensor are greatly improved. In terms of pressure signal visualization, since this structure introduces a mechanoluminescent microcolumn array with high spatial resolution to complete the conversion of pressure signals to optical signals, the sensor can visualize the pressure distribution.
[0042] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing a visual stretchable pressure sensor based on mechanoluminescent microcolumns, characterized in that: The following steps are involved: preparing a silicon wafer mold having a micropit array; The mechanoluminescent particles and the polydimethylsiloxane monomer are mixed and stirred, and then a cross-linking agent is added and mixed and stirred uniformly to obtain a mixture; Covering the mixture on the surface of the silicon wafer mold and evenly spin coating it with a spin coater; placing the silicon wafer mold covered with the mixture into an oven for thermal curing to obtain a mesoluminescent composite material; The mechanoluminescent composite material is peeled off from the silicon wafer mold by using tweezers to obtain connected mechanoluminescent microcolumns and mechanoluminescent films, thus preparing a pressure sensor.
2. The method for preparing a visualized stretchable pressure sensor based on mesoluminescent microcolumns according to claim 1, characterized in that: The method for preparing a silicon wafer mold with a micro-pit array includes: preparing a mask plate with a circular hole array structure, wherein the diameter of the circular holes of the mask plate is 30 to 200 μm, and the center spacing of the circular holes is 60 to 400 μm; then spin coating photoresist on a silicon wafer, and combining the silicon wafer uniformly coated with the photoresist with the mask plate for photolithography; and then completing the preparation of the silicon wafer mold by deep silicon etching.
3. The method for preparing a visualized stretchable pressure sensor based on mesoluminescent microcolumns according to claim 2, characterized in that: The depth of the micro-pits on the silicon wafer is 30-100 μm.
4. The method for preparing a visualized stretchable pressure sensor based on mesoluminescent microcolumns according to claim 1, characterized in that: The mechanoluminescent particles are mixed with polydimethylsiloxane monomers, and then a cross-linking agent is added and mixed to obtain a mixture, including: the mechanoluminescent particles are composed of ZnS:Cu / ZnS:Mn particles, and the mass ratio of the mechanoluminescent particles to the polydimethylsiloxane monomer is 0.5:1 to 3:
1.
5. The method for preparing a visualized stretchable pressure sensor based on mesoluminescent microcolumns according to claim 4, characterized in that: The crosslinking agent is SYLGARD 184 SILICONE ELASTOMER CURINGAGENT, and the weight ratio of the polydimethylsiloxane monomer to the crosslinking agent is 8-12:
1.
6. The method for preparing a visualized stretchable pressure sensor based on mesoluminescent microcolumns according to claim 1, characterized in that: The silicon wafer mold covered with the mixture is placed in an oven for thermal curing to obtain a mesoluminescent composite material, which comprises: the temperature of the oven is 80-100° C., and the thermal curing time is 60-120 minutes.
7. A visual stretchable pressure sensor based on mechanoluminescent microcolumns, characterized in that: The pressure sensor is prepared by the method for preparing a pressure sensor according to any one of claims 1 to 6; the pressure sensor comprises the mesoluminescent microcolumns and the mesoluminescent film in order from top to bottom, and the mesoluminescent microcolumns are connected to the mesoluminescent film.
8. The visual stretchable pressure sensor based on mesoluminescent microcolumns according to claim 7, characterized in that: The mechanoluminescent microcolumn and the mechanoluminescent film are both composed of polydimethylsiloxane and ZnS:Cu / ZnS:Mn particles. The mechanoluminescent microcolumn has a diameter of 30 μm, a center distance of 60 to 400 μm, and a height of 30 to 200 μm.
Citation Information
Patent Citations
Pressure sensing imaging array, device and manufacturing method thereof
CN105865668A
Gravity sensor
CN107655596A
Flexible pressure sensor for electronic skin and preparation method of flexible pressure sensor
CN109100075A
Capacitive type flexible pressure sensor, and preparation method and application thereof
CN110346078A
Flexible pressure visual sensor based on SBCs-GaN micro-LED and preparation method thereof
CN113701929A