In-situ polymerization coated ferric sodium phosphate pyrophosphate composite material as well as preparation method and application thereof

The electrochemical in-situ polymerization technology coats organic monomers on the surface of sodium ferric phosphate material, which solves the problems of low electron conductivity and poor cycle stability, and improves the electrochemical and rate performance of the material.

CN119008877AActive Publication Date: 2024-11-22HUBEI THREE GORGES LAB

Patent Information

Application Number
CN202410945428.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-22
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing sodium ferric phosphate positive electrode materials have low electronic conductivity, easy to generate heterogeneous phases, poor voltage attenuation and cycle stability, which limits their commercial applications.

Method used

The organic monomer is uniformly coated on the surface of the material through electrochemical in-situ polymerization to form a protective layer, improve the electron conductivity and buffer volume changes, and ensure structural integrity.

Benefits of technology

High rate performance and cycle stability are achieved, the electronic conductivity and electrochemical properties of the material are improved, and the cycle life of the material is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008877A_ABST
    Figure CN119008877A_ABST
Patent Text Reader

Abstract

The invention relates to the field of sodium ion battery electrode materials, and discloses an in-situ polymerization coated ferric sodium phosphate pyrophosphate composite material as well as a preparation method and application thereof. The molecular formula of the sodium ferric phosphate pyrophosphate positive electrode material is NaxFey (PO4) zP2O7, and the preparation process comprises the following steps: preparing a precursor by combining a segmented grinding and drying process, pre-sintering and sintering under the protection of inert gas to obtain the sodium ferric phosphate pyrophosphate positive electrode material, and successfully and uniformly coating the surface of the material with an organic monomer through in-situ polymerization coating. According to the invention, the organic monomer is subjected to electrochemical in-situ polymerization to the surface of the prepared pyrophosphate ferric phosphate sodium material, so that the problems of serious side reaction caused by poor surface structure stability of the material, particle breakage caused by internal stress of secondary particles in the charging and discharging process and the like are successfully solved. The prepared material can be applied to the field of sodium ion batteries, and the electrochemical performance of the pyrophosphate ferric phosphate sodium material can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sodium ion battery electrode technology materials, and in particular relates to an in-situ polymerization-coated sodium iron pyrophosphate composite material and a preparation method and application thereof. Background Art

[0002] Among many energy storage technologies, electrochemical secondary batteries have become the first choice for energy storage systems due to their high conversion efficiency and easy maintenance. In the past 20 years, lithium-ion batteries have been widely used as the most mature energy storage devices. However, the uneven distribution of lithium resources on the earth and the limited storage capacity will seriously restrict the development of lithium-ion batteries in the future. Compared with lithium resources, sodium resources are abundant on the earth and are cheap. Sodium-ion batteries will surely usher in a blowout development and achieve large-scale application.

[0003] In sodium-ion batteries, the iron-based mixed polyanion fast ion conductor sodium iron pyrophosphate (Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 The material has three Fe-occupied sites in its crystal structure, and the typical three-dimensional framework structure ensures that sodium ions can migrate quickly, with high structural stability. The single-electron specific capacity of the material involved in the redox reaction is 43 mAh g -1 , making the theoretical capacity of sodium iron pyrophosphate material reach 129 mAh g -1 . (P 2 O 7 ) 4− The strong induction effect of Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 The high energy density of the material makes it a promising cathode material for sodium-ion batteries. 4 Fe 3 (PO 4 ) 2 P 2 O 7 The material not only has low electronic conductivity, but also easily generates NaFePO during the preparation process. 4 and Na 2 FeP 2 O 7 The impurities limit its capacity, while the obvious voltage decay and poor cycle stability restrict its commercial application. Summary of the invention

[0004] The problem to be solved by the present invention is to address the defects and deficiencies of the existing sodium iron pyrophosphate positive electrode materials, and to provide an in-situ polymerization-coated sodium iron pyrophosphate composite material and a preparation method and application. The sodium iron pyrophosphate material is successfully prepared by combining a segmented grinding method, a drying process and a high-temperature solid phase method, and then the organic monomer is successfully and evenly coated on the surface of the material through electrochemical in-situ polymerization to form a protective layer. The electronic conductivity of the composite material is improved, thereby achieving rapid ion transmission, and the coating layer formed after the polymerization of the organic monomer is used to further buffer the electrode in the Na + The volume change caused by the embedding and de-embedding process ensures the structural integrity of the material during the charging and discharging process, so that the material particles have both excellent high-rate performance and cycle stability.

[0005] The present invention aims to provide a method for preparing a sodium iron pyrophosphate material which has simple synthesis process, is environmentally friendly, low cost, good repeatability and has practical application potential.

[0006] In order to solve the technical problems proposed by the present invention, the present invention provides an in-situ polymerization-coated sodium iron pyrophosphate composite material, the composition of which is Na x Fe y (PO 4 ) z P 2 O 7 (3≤ x ≤4.5、2≤ y ≤3, 1≤ z ≤2), the in-situ polymerized coating material is an organic monomer material; the organic monomer includes at least one or a mixture of aniline monomer and its derivatives and pyrrole monomer and its derivatives, and the formed composite material is a conductive polymer (polypyrrole, polyaniline).

[0007] The XRD powder diffraction peaks of the in-situ polymerization-coated sodium iron pyrophosphate mainly have peak positions θ° including approximately 9.7±0.2°, 15.9±0.2°, 16.7±0.2°, 19.4±0.2°, 23.9±0.2°, 25.4±0.2°, 25.8±0.2°, 25.9±0.2°, 27.2±0.2°, 28.8±0.2°, 29.4±0.2°, 29.4±0.2°, and 30.2±0.2°.

[0008] The present invention also provides a method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material, characterized in that the preparation steps are as follows: Step 1: Assemble a button cell by using an electrode sheet containing an active material of sodium iron pyrophosphate as a positive electrode sheet, sodium metal as a negative electrode, glass fiber as a separator, and a mixed electrolyte formed by mixing a sodium electrolyte and an organic monomer; In some specific embodiments, the electrode sheet containing the active material of sodium ferric pyrophosphate is dried in a vacuum drying oven for a certain period of time and then placed in a glove box. The sodium ferric pyrophosphate electrode sheet is used as the positive electrode, sodium metal is used as the negative electrode, and glass fiber is used as the separator. The negative electrode shell, sodium metal, a certain amount of mixed electrolyte (sodium electrolyte and organic monomer are mixed in volume ratio), separator, a certain amount of mixed electrolyte, positive electrode, gasket, spring, positive electrode shell are assembled in this order, and finally the button battery is packaged using a button sealing machine; Step 2: After the button cell is cycled for a certain number of times by applying current, the organic monomers in the mixed electrolyte are polymerized in situ on the surface of the positive electrode of the sodium iron pyrophosphate to form a protective conductive polymer coating layer, thereby obtaining an in-situ polymerized coated sodium iron pyrophosphate composite material.

[0009] The sodium electrolyte in step 1 contains 0.5-2 M NaPF 6 The organic monomer comprises at least one of aniline monomer, pyrrole monomer and thiophene monomer, or a mixture of at least one of the above.

[0010] Specifically, the sodium electrolyte is NaPF 6 The sodium electrolyte is added to a mixture of ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC) in an equal volume ratio.

[0011] The volume ratio of the organic monomer to the sodium electrolyte is 1:9~999.

[0012] In the step 2, the current is 0.1-4 C, and the number of charge and discharge cycles is 2-10.

[0013] The steps for preparing the electrode sheet containing the active material of sodium ferric pyrophosphate are as follows: (1) Phosphorus salt, iron source and water are mixed and ground to form slurry A; sodium salt, pyrophosphate or pyrophosphate compound, dispersant and carbon source are stirred and mixed with water in proportion to form solution B; In some embodiments, the grinding method is one of ball milling or sand milling, the grinding time of slurry A is 0.5 to 6 h, and the stirring time of solution B is 10 to 60 min.

[0014] (2) adding solution B to slurry A and grinding again to finally obtain precursor solution C. After drying the precursor solution C, a powdered precursor is obtained; In some embodiments, the grinding time of slurry C is 0.5-6 h, and the drying method is one of spray drying, atmospheric pressure drying, freeze drying, infrared drying, and microwave drying.

[0015] (3) placing the obtained powdered precursor in an atmosphere furnace, pre-sintering at a low temperature for a period of time under an inert protective atmosphere or a reducing atmosphere, and then calcining at a high temperature for a period of time to obtain a product, sodium iron pyrophosphate positive electrode material; (4) Sodium iron pyrophosphate, a conductive agent and polyvinylidene fluoride are mixed with N-methyl-2-pyrrolidone to form a uniform active slurry, and then the active slurry is coated on the aluminum foil current collector using an automatic coater. After drying in a drying oven for a certain period of time, the electrode sheet is rolled by an electric roller machine, and then the obtained electrode sheet is cut into circular electrode sheets.

[0016] The phosphate salt includes at least one of ferric phosphate, ferric phosphate dihydrate and ferric phosphate tetrahydrate, or a mixture of more than one thereof; The iron source comprises at least one of iron oxalate (II) dihydrate, iron powder, iron oxide, ferric oxide, ferric pyrophosphate, ferric sulfate, ferrous sulfate, ferric citrate, ammonium ferric citrate, ferric acetylacetonate, iron (II) acetate, sodium ferric oxalate hydrate, ferric ethanol, ferric sucrose and ammonium iron sulfate hexahydrate (II) or a mixture of more than one; The sodium salt includes at least one of sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, sodium carbonate, sodium bicarbonate, sodium pyrophosphate, trisodium monohydrogen pyrophosphate, disodium dihydrogen pyrophosphate, sodium methoxide and sodium ascorbate, or a mixture of more than one thereof; The pyrophosphate or pyrophosphate compound includes at least one of pyrophosphate, sodium pyrophosphate, ferric pyrophosphate, tributylammonium pyrophosphate, trisodium monohydrogen pyrophosphate, disodium dihydrogen pyrophosphate, isopentenyl pyrophosphate triammonium salt, trisodium monohydrogen pyrophosphate monohydrate and sodium pyrophosphate decahydrate, or a mixture of more than one thereof; The dispersant comprises at least one of polyethylene glycol and Triton X-100 or a mixture of more than one thereof; The carbon source comprises at least one of sucrose, glucose, fructose, oxalic acid, ascorbic acid, starch, lactic acid, citric acid monohydrate and malic acid, or a mixture of more than one of the above.

[0017] In the step (3), the heating rate during the low-temperature pre-sintering process is 1-10°C / min, the pre-sintering temperature is 200-400°C, and the pre-sintering time is 1-5 h; the heating rate during the calcining process is 1-10°C / min, the calcining temperature is 450-600°C, and the calcining time is 5-18 h; the inert protective atmosphere or reducing atmosphere includes any one of high-purity argon, high-purity nitrogen, high-purity hydrogen and argon, high-purity helium, and high-purity carbon dioxide, or a mixture of more than one of them.

[0018] In the step (4), the mass ratio of sodium ferric pyrophosphate, conductive agent and polyvinylidene fluoride is 7+ x :2- x :1(0≤ x <2), the conductive agent includes one of acetylene black, conductive carbon black, conductive graphite and Ketjen black; the normal pressure drying temperature is 80~150℃, and the time is 1~4 h.

[0019] Another technical solution of the present invention is to use the prepared in-situ polymerization-coated sodium iron pyrophosphate composite material as an application in a sodium ion battery. The structural formula of the in-situ polymerization-coated sodium iron pyrophosphate composite material is Na:Fe:P:P 2 O 7 The ratio is x : y : z :1(3≤ x ≤4.5、2≤ y ≤3, 1≤ z ≤2).

[0020] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The present invention uses an electrochemical in-situ polymerization method to successfully and evenly coat the organic monomer on the surface of sodium iron pyrophosphate particles. The excellent conductivity of the conductive polymer is used to effectively improve the electronic conductivity between particles, which can effectively reduce the overpotential, increase the peak current, and shorten the Na + transmission path, thereby improving the electrochemical performance of the material.

[0021] (2) When a specific current is applied, the organic monomer molecules are anchored to the -OH and -COOH functional groups of the sodium iron pyrophosphate electrode (from carbon) through electrostatic forces between atoms. The oxidative current then oxidizes the organic monomer molecules to form monomer radicals. These radicals trigger subsequent oxidation reactions, and the organic monomers form conductive polymers, ensuring better access of electrons and ions to the redox active sites. Since the organic monomers are used as electrolyte additives and they are electrochemically polymerized inside the battery to form a protective conductive coating, no additional ex situ processes are required. The conductive polymer coating on the particle surface can significantly reduce the corrosion of the electrolyte to the electrode material, the occurrence of side reactions, and improve the surface stability of the material, which is beneficial to the long cycle life of the material under high current.

[0022] (3) The "electrochemical in situ polymerization method" used in the present invention has simple process, low cost, high preparation efficiency, and is suitable for most application scenarios. Compared with wet chemical technology, gas phase chemistry and dry process, it has obvious advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is Na in Example 1 of the present invention 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1% PANI X-ray diffraction pattern.

[0024] Figure 2 is Na in Example 1 of the present invention 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1% SEM image of PANI.

[0025] Figure 3 is Na in Example 1 of the present invention 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1% PANI’s first charge and discharge curve.

[0026] Figure 4 is Na in Example 1 of the present invention 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1% PANI constant current cycling performance diagram.

[0027] Figure 5 is Na in Example 1 of the present invention 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1% PANI rate performance diagram.

[0028] Figure 6 is Na in Example 2 of the present invention 3 Fe 2 (PO 4 ) 2 O 7 @Scanning electron microscope image of 2%PPy.

[0029] Figure 7 is Na in Example 2 of the present invention 3 Fe 2 (PO 4 ) 2 O 7 @2%PPy rate performance diagram.

[0030] Figure 8 is Na in Comparative Example 2 of the present invention 4 Fe 3 (PO 4 ) 2 P 2 O 7 X-ray diffraction pattern of .

[0031] Fig. 9 is Na in Comparative Example 2 of the present invention 4 Fe 3 (PO 4 ) 2 P 2 O 7 Rate performance diagram. DETAILED DESCRIPTION

[0032] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0033] In order to better understand the present invention, the content of the present invention is further described below in conjunction with embodiments and related drawings, but the content of the present invention is not limited to the following embodiments.

[0034] Example 1 This embodiment provides a method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material, which is specifically as follows: Step 1: Mix 12.0656 g of FePO4 in a ratio of 4:3:2:1. 4 , 7.196 g of FeC 2 O 4 2H 2 O was mixed with 100 mL of deionized water and sand-milled for 1.5 h to form slurry A. 10.636 g of Na 4 P 2 O 7 , 10 g of polyethylene glycol and 3.0026 g of C 6 H 12 O 6 Stir and mix with 200 mL of deionized water for 60 min to form solution B; Step 2: Add solution B to slurry A and perform sand milling again for 1 h to finally obtain precursor solution C. Spray dry the precursor solution to obtain a powdered precursor; Step 3: placing the obtained precursor powder in an atmosphere furnace, under the protection of high-purity argon, heating to 300°C at a heating rate of 3°C / min, keeping warm for 3 h, then heating to 550°C at a heating rate of 4°C / min, keeping warm for 12 h, and cooling to room temperature to finally obtain the product sodium iron pyrophosphate positive electrode material; Step 4: Mix the sodium iron pyrophosphate material, conductive agent and polyvinylidene fluoride (PVDF) with N-methyl-2-pyrrolidone (NMP) in a mass ratio of 7:2:1 to form a uniform active slurry, and then use an automatic applicator to apply the active slurry on the aluminum foil current collector. After drying at 100°C in a drying oven for 2 h, the electrode sheet is rolled by an electric roller machine, and then the obtained electrode sheet is cut into circular electrode sheets, weighed and the corresponding values ​​are recorded; Step 5: Dry the sodium iron pyrophosphate electrode sheet in a vacuum oven at 150°C for 12 h and place it in a glove box. Use the sodium iron pyrophosphate electrode sheet as the positive electrode, sodium metal as the negative electrode, and glass fiber as the separator. Follow the negative electrode shell, sodium metal, and 150 μL of mixed electrolyte (sodium electrolyte is NaPF 6(1M) volume ratio is 1:1:1 (v / v / v) ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC). The organic monomer is aniline monomer. And the volume ratio of the organic monomer to the sodium electrolyte is 1:99), the separator, 150 μL of mixed electrolyte, the positive electrode, the gasket, the shrapnel, and the positive electrode shell are assembled in order, and finally the button battery is packaged using a button sealing machine; Step 6: Place the button cell into the Xinwei tester and apply 0.5 C = 64.5 mAh g -1 After 5 cycles, the aniline organic monomer material in the mixed electrolyte will be in situ polymerized on the surface of the sodium iron pyrophosphate positive electrode to form a protective conductive polymer PANI coating layer, and finally Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1%PANI composite material.

[0035] Figure 1 The Na used in this example 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1% PANI material XRD spectrum; it can be seen from the figure that the diffraction peaks of the material are narrow and sharp, and the positions and relative intensities of the diffraction peaks are similar to those of Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 After comparison with the standard card, it was found that the diffraction peak position and relative intensity in the XRD spectrum of the sample were consistent with Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 The phase composition of the material, the diffraction peak positions are 9.794°, 15.949°, 16.74°, 19.496°, 23.951°, 25.417°, 25.823°, 25.981°, 27.279°, 28.838°, 29.409°, 29.494°, 30.286°. This shows that the polyaniline conductive layer formed by the electrochemical in-situ polymerization of aniline monomer does not affect the phase structure and elemental composition of the material itself.

[0036] Figure 2 The Na used in this example 4 Fe3 (PO 4 ) 2 P 2 O 7 @1% PANI material SEM image; it can be seen from the figure that the SEM image of the sample shows that the material has good crystallinity and the particle size diameter is between 0.5~5 μm.

[0037] Figure 3 The Na used in this example 4 Fe 3 (PO 4 ) 2 P 2 O 7 The first charge and discharge curve of @1% PANI material at 0.5 C; the specific capacity of the sample at the first discharge is 101.23 mAh g -1 The first cycle coulombic efficiency is 81.82%, and its charge and discharge platform meets the requirements of Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 Compared with Na without conductive polymer composite 4 Fe 3 (PO 4 ) 2 P 2 O 7 Materials, capacity and Coulombic efficiency are greatly improved.

[0038] Figure 4 The Na used in this example 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1% PANI material constant current cycling performance diagram at a current density of 1 C; the specific capacity of the sample at the first discharge is 100.91 mAh g -1 After 50 charge and discharge cycles, the discharge capacity is 87.62 mAh g -1 The capacity retention rate is 86.82%. This is because the conductive polymer coating on the particle surface can greatly reduce the corrosion of the electrolyte to the electrode material, the occurrence of side reactions, and improve the surface stability of the material.

[0039] Figure 5 The Na used in this example 4 Fe 3 (PO 4 ) 2 P 2O 7 @1% PANI material rate performance diagram. As can be seen from the figure, the first discharge specific capacity of the material at 0.5 C, 1 C, 2 C, 5 C, and 10 C is 96.35 mAh g -1 、87.83mAh g -1 、83.75 mAh g -1 、79.09 mAh g -1 , 71.99 mAh g -1 , and has a high initial discharge specific capacity at different rates.

[0040] In summary, the sodium iron pyrophosphate composite material Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 @1%PANI exhibits higher discharge specific capacity, better cycle life and more stable high-rate performance, indicating that after being compounded with the conductive polymer PANI, it has higher energy density and better electrochemical and cycle performance.

[0041] Example 2 This embodiment provides a method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material, which is specifically as follows: Step 1: Mix 18.8737 g of FePO4 in a ratio of 3:2:1:1. 4 2H 2 O, 18.3084 g of C 4 H 6 O 4 Fe was mixed with 200 mL of deionized water and sand-milled for 1 h to form slurry A. 18.7347 g of H 4 P 2 O 7 , 8 g of Triton X-100 and 34.23 g of C 12 H 22 O 11 Stir and mix with 400 mL of deionized water for 30 min to form solution B; Step 2: Add solution B to slurry A and perform sand milling again for 2 hours to finally obtain precursor solution C. After freeze drying the precursor solution, a powdered precursor is obtained; Step 3: placing the obtained precursor powder in an atmosphere furnace, under the protection of high-purity hydrogen and argon, heating the temperature to 350°C at a heating rate of 2°C / min, keeping the temperature for 5 hours, then heating the temperature to 500°C at a heating rate of 5°C / min, keeping the temperature for 15 hours, and cooling to room temperature to finally obtain the product sodium iron pyrophosphate positive electrode material; Step 4: Mix the sodium iron pyrophosphate material, conductive agent and polyvinylidene fluoride (PVDF) with N-methyl-2-pyrrolidone (NMP) in a mass ratio of 8:1:1 to form a uniform active slurry, and then use an automatic applicator to apply the active slurry on the aluminum foil current collector. After drying at 120°C in a drying oven for 1.5 h, the electrode sheet is rolled by an electric roller machine, and then the obtained electrode sheet is cut into circular electrode sheets, weighed and the corresponding values ​​are recorded; Step 5: Dry the sodium iron pyrophosphate electrode sheet in a vacuum oven at 180°C for 8 h and place it in a glove box. Use the sodium iron pyrophosphate electrode sheet as the positive electrode, sodium metal as the negative electrode, and glass fiber as the separator. Place the negative electrode shell, sodium metal, and 200 μL of mixed electrolyte (sodium electrolyte is NaPF 6 The volume ratio of (1M) is 1:1:1 (v / v / v) ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC). The organic monomer is a pyrrole monomer. And the volume ratio of the organic monomer to the sodium electrolyte is 1:49), the separator, 200 μL of the mixed electrolyte, the positive electrode, the gasket, the shrapnel, and the positive electrode shell are assembled in order, and finally the button battery is packaged using a button sealing machine; Step 6: Place the button battery into the Xinwei tester and apply 2 C=258mAh g -1 After 8 cycles, the pyrrole organic monomer material in the mixed electrolyte will be in situ polymerized on the surface of the sodium iron pyrophosphate positive electrode to form a protective conductive polymer PPy coating layer, and finally Na 3 Fe 2 (PO 4 ) 2 O 7 @2%PPy composite material.

[0042] Figure 6 The Na used in this example 3 Fe 2 (PO 4 ) 2 O 7 @2% PPy material SEM image; as can be seen from the figure, the SEM image of the sample shows that the material has good crystallinity and the particle size diameter is between 0.1~5 μm.

[0043] Figure 7The Na used in this example 3 Fe 2 (PO 4 ) 2 O 7 @2%PPy material rate performance diagram. It can be seen from the figure that the first discharge specific capacity of the material at 0.2 C, 0.5 C, 1 C, 2 C, and 5 C is 101.77 mAh g -1 , 95.99mAh g -1 , 91.07 mAh g -1 、87.47 mAh g -1 、83.99 mAh g -1 , and has a high initial discharge specific capacity at different rates.

[0044] In summary, the sodium iron pyrophosphate composite material Na 3 Fe 2 (PO 4 ) 2 O 7 @2%PPy exhibits more stable high-rate performance, indicating that the material composited with conductive polymer PPy exhibits better electrochemical performance at high current density.

[0045] Example 3 This embodiment provides a method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material. The preparation method is the same as that of Example 2. The difference from the embodiment is that the volume ratio of the pyrrole organic monomer to the sodium electrolyte in the mixed electrolyte in step 5 of this embodiment is 1:99. The specific current applied in step 6 is 4 C=516 mAhg -1 , and finally obtain the composite Na 3 Fe 2 (PO 4 ) 2 O 7 @1%PPy positive electrode material.

[0046] Example 4 This embodiment provides a method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material. The preparation method is the same as that of Example 1. The difference from the embodiment is that the volume ratio of the aniline organic monomer to the sodium electrolyte in the mixed electrolyte in step 5 of this embodiment is 1:9. The specific current applied in step 6 is 3 C=387 mAhg -1 , and finally obtain the composite Na 3 Fe 2 (PO 4 ) 2 O 7@10%PANI positive electrode material.

[0047] Comparative Example 1 Compared with Example 1, the only difference is that the electrolyte used in step 5 is 1 M NaPF 6 The volume ratio of (1M) is 1:1:1 (v / v / v) ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC), and it is not a mixed electrolyte to which organic monomers are added. Other operations and parameters are the same as those in Example 1.

[0048] The pure sodium iron pyrophosphate material prepared in this comparative example 1 was tested by a button half-cell and its electrochemical performance was found to be: 0.1 reversible capacity reached 90 mAh g -1 , 1C reversible capacity is 65 mAh g -1 After 50 cycles, the reversible capacity decayed to 21 mAh g -1 , the capacity retention rate is as low as 32.3%. For the 1 C reversible capacity of the button half-cell of this comparative example, the lower reversible capacity than that of Example 1 is due to the fact that the electrolyte used in step 5 does not add aniline organic monomer, the obtained sodium iron pyrophosphate is not compounded with the conductive polymer, and its conductivity and structural stability are poor. Compared with the battery prepared in Example 1, its capacity retention rate is lower.

[0049] Comparative Example 2 Compared with Example 1, the only difference is that the current applied in step 6 is 5 C = 645 mAh g -1 , other operations and parameters are the same as in Example 1.

[0050] like Fig. 9 As shown, after the positive electrode material prepared in Comparative Example 2 was assembled into a button cell, its rate performance was tested: the first discharge specific capacity of the material at 0.5 C, 1 C, 2 C, 5 C, and 10 C was 86.35 mAh g -1 、72.83 mAh g -1 、61.75 mAh g -1 , 45.09 mAh g -1 , 21.99 mAh g -1 Compared with Na in Example 1 4 Fe 3 (PO 4 ) 2 P 2 O 7@1% PANI composite material, the material in Comparative Example 2 has a smaller discharge capacity at different current densities and worse structural stability. This indicates that when the current density of the organic monomer is too high, the coating layer of the conductive polymer formed by the electrochemical in-situ polymerization will be broken, and the particles cannot be effectively coated, resulting in a significant decrease in the electrochemical performance of the material.

[0051] In summary, the method of the present invention can obtain a composite positive electrode material of sodium iron pyrophosphate@conductive polymer with excellent electrochemical performance and stable structure.

[0052] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.

Claims

1. An in-situ polymerization-coated sodium iron pyrophosphate composite material, characterized in that: The composition of the positive electrode material is Na x Fe y (PO4) z P2O7(3≤ x ≤4.5、2≤ y ≤3, 1≤ z ≤2), the in-situ polymerized coating material is an organic monomer material; the organic monomer comprises at least one of aniline monomer and pyrrole monomer or a mixture of more than one of them.

2. The in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 1, characterized in that: The XRD powder diffraction peaks of the in-situ polymerization-coated sodium iron pyrophosphate mainly have peak positions θ° including approximately 9.7±0.2°, 15.9±0.2°, 16.7±0.2°, 19.4±0.2°, 23.9±0.2°, 25.4±0.2°, 25.8±0.2°, 25.9±0.2°, 27.2±0.2°, 28.8±0.2°, 29.4±0.2°, 29.4±0.2°, and 30.2±0.2°.

3. The method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 1 or 2, characterized in that: The preparation steps are as follows: Step 1: Assemble a button cell by using an electrode sheet containing an active material of sodium iron pyrophosphate as a positive electrode sheet, sodium metal as a negative electrode, glass fiber as a separator, and a mixed electrolyte formed by mixing a sodium electrolyte and an organic monomer; Step 2: After the button cell is cycled for a certain number of times by applying current, the organic monomers in the mixed electrolyte are polymerized in situ on the surface of the positive electrode of the sodium iron pyrophosphate to form a protective conductive polymer coating layer, thereby obtaining an in-situ polymerized coated sodium iron pyrophosphate composite material.

4. The method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 3, characterized in that: The steps for preparing the electrode sheet containing the active material of sodium ferric pyrophosphate are as follows: (1) Phosphorus salt, iron source and water are mixed and ground to form slurry A; sodium salt, pyrophosphate or pyrophosphate compound, dispersant and carbon source are stirred and mixed with water in proportion to form solution B; (2) adding solution B to slurry A and grinding again to finally obtain precursor solution C. After drying the precursor solution C, a powdered precursor is obtained; (3) placing the obtained powdered precursor in an atmosphere furnace, pre-sintering at a low temperature for a period of time under an inert protective atmosphere or a reducing atmosphere, and then calcining at a high temperature for a period of time to obtain a product, sodium iron pyrophosphate positive electrode material; (4) Sodium iron pyrophosphate, a conductive agent and polyvinylidene fluoride are mixed with N-methyl-2-pyrrolidone to form a uniform active slurry, and then the active slurry is coated on the aluminum foil current collector using an automatic coater. After drying in a drying oven for a certain period of time, the electrode sheet is rolled by an electric roller machine, and then the obtained electrode sheet is cut into circular electrode sheets.

5. The method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 4, characterized in that: The phosphate salt includes at least one of ferric phosphate, ferric phosphate dihydrate and ferric phosphate tetrahydrate, or a mixture of more than one thereof; The iron source comprises at least one of iron oxalate (II) dihydrate, iron powder, iron oxide, ferric oxide, ferric pyrophosphate, ferric sulfate, ferrous sulfate, ferric citrate, ammonium ferric citrate, ferric acetylacetonate, iron (II) acetate, sodium ferric oxalate hydrate, ferric ethanol, ferric sucrose and ammonium iron sulfate hexahydrate (II) or a mixture of more than one; The sodium salt includes at least one of sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, sodium carbonate, sodium bicarbonate, sodium pyrophosphate, trisodium monohydrogen pyrophosphate, disodium dihydrogen pyrophosphate, sodium methoxide and sodium ascorbate, or a mixture of more than one thereof; The pyrophosphate or pyrophosphate compound includes at least one of pyrophosphate, sodium pyrophosphate, ferric pyrophosphate, tributylammonium pyrophosphate, trisodium monohydrogen pyrophosphate, disodium dihydrogen pyrophosphate, isopentenyl pyrophosphate triammonium salt, trisodium monohydrogen pyrophosphate monohydrate and sodium pyrophosphate decahydrate, or a mixture of more than one thereof; The dispersant comprises at least one of polyethylene glycol and Triton X-100 or a mixture of more than one thereof; The carbon source comprises at least one of sucrose, glucose, fructose, oxalic acid, ascorbic acid, starch, lactic acid, citric acid monohydrate and malic acid, or a mixture of more than one of the above.

6. The method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 4, characterized in that: In the step (3), the heating rate during the low-temperature pre-sintering process is 1-10°C / min, the pre-sintering temperature is 200-400°C, and the pre-sintering time is 1-5 h; the heating rate during the calcining process is 1-10°C / min, the calcining temperature is 450-600°C, and the calcining time is 5-18 h; the inert protective atmosphere or reducing atmosphere includes any one of high-purity argon, high-purity nitrogen, high-purity hydrogen and argon, high-purity helium, and high-purity carbon dioxide, or a mixture of more than one of them.

7. The method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 4, characterized in that: In the step (4), the mass ratio of sodium ferric pyrophosphate, conductive agent and polyvinylidene fluoride is 7+ x :2- x :1(0≤ x <2), the conductive agent includes one of acetylene black, conductive carbon black, conductive graphite and Ketjen black; the normal pressure drying temperature is 80~150℃, and the time is 1~4 h.

8. The method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 4, characterized in that: In the step 1, the sodium electrolyte is a mixture of ethylene carbonate / diethyl carbonate / ethyl methyl carbonate in equal volume ratios containing 0.5-2M NaPF6; the organic monomer includes at least one or a mixture of more than one of aniline monomer, pyrrole monomer and thiophene monomer, and the volume ratio of the organic monomer to the sodium electrolyte is 1:9~999.

9. The method for preparing an in-situ polymerization-coated sodium iron pyrophosphate composite material according to claim 4, characterized in that: In the step 2, the current is 0.1-4 C, and the number of charge and discharge cycles is 2-10.

10. An in-situ polymerization-coated sodium iron pyrophosphate composite material prepared as claimed in any one of claims 3 to 9 for use in a sodium ion battery, wherein the in-situ polymerization-coated sodium iron pyrophosphate composite material has a structural formula of Na:Fe:P:P2O7 and a ratio of x : y : z :1(3≤ x ≤4.5、2≤ y ≤3, 1≤ z ≤2).

Citation Information

Patent Citations

  • Iron-based phosphate sodium ion battery positive electrode material and preparation method thereof

    CN114883540A

  • Carbon-coated ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof

    CN116230923A

  • Preparation method and application of composite phosphoric acid and pyrophosphoric acid polyanionic positive electrode material

    CN117361482A

  • Composite-coated lithium iron phosphate and preparation method therefor, and lithium ion battery

    US20180097228A1

Cited By

  • Method for preparing ferric sodium pyrophosphate material based on regulation and control of valence state of iron source

    CN119409174A

  • Sodium ferromanganese pyrophosphate positive electrode material as well as preparation method and application thereof

    CN119786572A

  • Sodium ferric pyrophosphate positive electrode material and preparation method thereof

    CN119920899A

  • Modified ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof

    CN119943909A

  • Pyrophosphate and ferric phosphate sodium composite positive electrode material, preparation method thereof, positive plate and sodium ion battery

    CN120413652A