Double-carbon-layer-coated silicon monoxide negative electrode material and preparation method thereof
By designing a double carbon layer clad structure on the negative electrode material of lithium-ion battery and using small-slice graphene and polydopamine-derived carbon to form an armor structure, the volume expansion and lithium ion conduction of the negative electrode material of lithium-ion battery during the deliquification process is solved. Problem, significantly improving cycle stability and electrochemical properties.
Patent Information
- Application Number
- CN202310549948.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-ion battery anode material has a volume expansion during the deliquification process, and graphene is difficult to effectively coat and conduct lithium ions, which limits the application potential of the material.
A double carbon layer coated silicon oxide negative electrode material is designed, using small-sheet graphene and polydopamine-derived carbon to form an armor structure, and is connected through amide bonds. The bonding between graphene and polydopamine-derived carbon layer is anchored The graphene is prevented from falling off and coated on the silicon oxide surface by dopamine self-polymerization and liquid phase self-assembly technology to form a bicarbonate layer.
A better lithium ion conduction path and volume expansion buffer is achieved, cycling stability and electrochemical performance are improved, and the energy density and lifetime of the material are enhanced.
Smart Images

Figure CN119008942A_ABST
Abstract
Description
Technical Field
[0001] A double carbon layer coated silicon oxide negative electrode material and a preparation method thereof belong to the field of silicon oxide negative electrode materials for lithium ion batteries, and specifically relate to a graphene and polydopamine derived carbon double carbon layer coated silicon oxide negative electrode material with an armor structure and a preparation method thereof. Background Art
[0002] Lithium-ion batteries (LIBs) stand out in the field of energy storage due to their many advantages such as no memory effect, low self-discharge rate, wide operating temperature range, safety, reliability and environmental friendliness. As an important component of lithium-ion batteries, negative electrode materials are one of the key factors in the development of lithium-ion batteries. The negative electrode material that has been commercialized and widely used is graphite negative electrode material, but the theoretical specific capacity of graphite material is only 372mAh / g, and its energy density has limited room for improvement. With the rapid development of various scientific and technological fields in recent years, people's demand for battery energy density has continued to increase. Therefore, the development of lithium-ion batteries with high energy density, long life and high safety has become a focus in this field.
[0003] Silicon-based materials have been widely studied due to their high theoretical specific capacity and suitable lithium insertion potential. Compared with the huge volume change of silicon, the volume expansion of silicon oxide (SiO) is about 150%, and its specific capacity (1700mAh / g) has become one of the research hotspots of negative electrode materials. However, SiO will cause capacity decay in the cycle process due to volume effect and low conductivity during lithium insertion and extraction, which limits the practical application of this material. Designing a coating layer on the surface of SiO can improve the interface characteristics and cycle stability of electrode materials. The composite of SiO and graphene can increase the transmission speed of lithium ions and electrons, and the flexibility of graphene can buffer the volume expansion. Therefore, the composite of graphene and SiO has become a research hotspot of silicon-carbon composite materials. However, graphene often has the problem of difficult coating and easy detachment, and it is difficult to conduct lithium ions perpendicular to the c-axis direction of graphene. Therefore, it is of application value to design a composite negative electrode material that can provide sufficient lithium ion transmission channels and maintain cycle stability.
[0004] In the literature (1) ACS Appl. Energy Mater. 2020, 3, 3562-3568, Chen et al. synthesized a nanostructured carbon nanotube with reduced graphene oxide nanosheets as substrate and SiO x Multi-component rGO@SiO with nitrogen-doped nanoporous carbon as the outer shell and as the middle layer x@C composite material, which improves the cycle performance but has a low specific capacity; in document (2) Natl Sci Rev, 2021, Vol. 8, nwab012, Chen et al. prepared a graphene hydrogel carbon cage with an internal void structure by a hydrothermal method to buffer the volume expansion of silicon; in document (3) Energy Fuels 2021, 35, 19784-19790, Zhang et al. used high-energy ball milling to introduce graphene and carbon nanotube dual carbon components to form a flexible network to buffer the volume expansion of SiO, but the material prepared by this method has poor coating effect; in patent (4) CN114122397A, Yi Xu et al. connected SiO and carbon layer by carbon nanotubes to prepare a double carbon layer-coated mesoporous SiO composite material to inhibit the volume expansion of SiO. The above work has certain effects in improving the cycle performance of silicon-based materials, but the preparation process is cumbersome and complicated, and there is still a certain gap from practical application. In addition, when introducing graphene components, it should be noted that it is difficult to conduct lithium ions perpendicular to the c-axis direction of graphene. Therefore, designing a coating structure that can buffer volume expansion and facilitate lithium ion conduction, and finding a simple process method for its preparation, is still a very challenging and innovative task. Summary of the invention
[0005] The purpose of the present invention is to design and synthesize a double carbon layer coated silicon oxide negative electrode material, characterized in that the material has an armor-like characteristic structure, the silicon oxide particle size used is 3-6 μm, the average sheet size of graphene is 0.5-1.5 μm, and the armor structure is a characteristic structure formed by multiple pieces of small-sheet graphene coated on the outside of silicon oxide particles; the double carbon layer is small-sheet graphene and polydopamine-derived carbon from the outside to the inside, and the graphene and the polydopamine-derived carbon coating layer are connected by an amide bond to anchor the graphene so that it is not easy to fall off; the mass percentage of each component is: polydopamine-derived carbon accounts for 8%-13%, graphene accounts for 8%-20%, and the rest is silicon oxide.
[0006] The present invention also provides a method for preparing a double carbon layer coated silicon oxide negative electrode material, characterized in that polydopamine is coated on the surface of silicon oxide by the self-polymerization reaction of dopamine, graphene oxide is coated on the surface by liquid phase self-assembly, and the double carbon layer coated silicon oxide negative electrode material is obtained after calcination in a reducing atmosphere. The process flow is as follows: Figure 1 As shown, the specific process steps are as follows:
[0007] (1) Preparation of polydopamine-coated silicon dioxide (SiO@PDA) material: SiO powder was dispersed into a Tris-HCl buffer solution (pH=8.3-8.7) at a solid-liquid ratio of 1:100, and dopamine hydrochloride was added at a mass ratio of silicon dioxide to dopamine hydrochloride of 1.5:1-2.5:1. Ultrasonication was performed for 25-35 min, and the mixture was evenly mixed. The mixture was magnetically stirred for 12-20 h to allow dopamine to fully polymerize on the surface of SiO to form a polydopamine coating layer. The mixture was filtered and washed several times. The filter cake was transferred to a vacuum oven and dried at 55-65°C for 6-10 h to obtain SiO@PDA.
[0008] (2) Preparation of double carbon layer coated silicon dioxide (SiO@NC@rGO) material: The SiO@PDA prepared in step (1) is slowly added to the graphene oxide dispersion, the mass ratio of SiO@PDA to graphene oxide being 10:1 to 5:1, and the two are evenly mixed by ultrasonication for 35 to 45 min, and then heated in a water bath at 85 to 95°C with stirring for 30 to 50 min to cross-link the carboxyl and amino groups, and the mixture is centrifuged to obtain a precipitate, which is freeze-dried to obtain SiO@PDA@GO. The obtained solid powder is ground and transferred to a clean porcelain boat, which is placed in the middle area of a tube furnace, and a hydrogen-argon mixed gas containing 5% hydrogen is introduced, and the mixture is calcined at 800 to 900°C for 2 to 3 h to fully reduce the graphene oxide and carbonize the polydopamine. After cooling to room temperature, SiO@NC@rGO, i.e., graphene and polydopamine derived carbon double carbon layer coated silicon dioxide material, is obtained.
[0009] The morphology of the samples was characterized using a Supra55 field emission scanning electron microscope (SEM) from Zeiss, Germany. Figure 2 This is the SEM image of SiO@NC@rGO. It can be seen that the overall coating effect is good and relatively uniform, and very few exposed SiO particles can be seen, indicating that the use of the dopamine carbon layer as a "bridge" can connect silicon oxide and graphene to achieve a relatively ideal coating effect. Figure 3 This is the SEM image of SiO@rGO in Comparative Example 1. It can be seen that part of the SiO surface is coated with graphene, but there are still many exposed SiO particles and scattered graphene sheets, indicating that the coating effect of the SiO@rGO composite material prepared by this method is not very good. The electrostatic effect can provide a certain force, but it cannot achieve a very ideal coating. Figure 4 The infrared spectrum of SiO@NC@rGO is shown at 790 cm -1 The Si-O vibration peak of silicon dioxide appears at 3470 cm -1 The broad peak at 1385 cm is the vibration peak of OH. -1 The peak that appears at is the stretching vibration of CN in the amide bond, indicating that the amino group and the carboxyl group have a bonding effect. Figure 5 The HRTEM image of SiO@NC@rGO shows that SiO particles are wrapped by multiple sheets of graphene. Two obvious coating layers are observed outside the SiO particles, in which the graphene layer has clear lattice fringes and a crystal plane spacing of 0.34nm, corresponding to the (002) crystal plane of carbon. Polydopamine will be converted into amorphous carbon at 800℃, without lattice fringes, corresponding to the part between SiO and graphene in the figure. Amorphous carbon and graphene are evenly coated on the surface of SiO particles, which not only effectively prevents direct contact between SiO and electrolyte, but also helps to alleviate the volume expansion of SiO during lithium storage and improve cycle stability.
[0010] Silicon oxide materials coated by different methods prepared by the method of the present invention and the comparative example method are used as negative electrode active materials, respectively mixed with Super-P conductive agent and CMC / SBR binder (solid content 4%) at a mass ratio of 7:1.5:1.5, coated on the surface of copper foil current collector, vacuum dried at 80°C for 8h and pressed into sheets, and an electrode sheet with a diameter of 1cm is obtained by a punching machine. A metal lithium sheet is used as the counter electrode and a polyethylene film is used as the diaphragm. Button batteries are assembled in a UniLab glove box (H2O<1ppm, O2<1ppm) of the German M.Braun company. The electrochemical performance test is carried out using a Wuhan Blue Electric CT2001A battery charge and discharge instrument, with a voltage range of 0.01-2V (vs.Li + / Li), the test temperature is 28℃, the test results are as follows Figure 6 , Figure 7 , Figure 8 As shown, the electrochemical test data of the embodiments of the present invention and the comparative examples are summarized in Table 1. The double carbon layer-coated silicon oxide material prepared by the method of the embodiments of the present invention has better cycle stability than that of the comparative example.
[0011] Table 1 Cyclic performance of silicon dioxide materials prepared in the embodiments of the present invention and the comparative examples
[0012] name 50-week capacity retention rate Example 1 92% Example 2 95% Example 3 83% Example 4 88% Comparative Example 1 56% Comparative Example 2 44% Comparative Example 3 71%
[0013] The characteristics and advantages of the present invention are: the armor structure formed by the small-diameter graphene can provide more paths for the diffusion of lithium ions; the double carbon coating layer can effectively inhibit the volume expansion of SiO2, and the bonding between the carbon layers can anchor the graphene, making it difficult to fall off. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a schematic diagram of the process flow for preparing a double carbon layer coated silicon oxide negative electrode material according to the present invention.
[0015] Figure 2 This is a scanning electron microscope photograph of the double carbon layer coated silicon oxide material prepared in Example 1.
[0016] Figure 3 This is a scanning electron microscope photograph of the graphene-coated silicon oxide material prepared in Comparative Example 1.
[0017] Figure 4 This is the infrared spectrum of the double carbon layer coated silicon oxide material prepared in Example 1.
[0018] Figure 5 This is a high-resolution transmission electron microscope photograph of the double carbon layer-coated silicon oxide material prepared in Example 1.
[0019] Figure 6 This is the electrochemical cycle performance curve of the double carbon layer coated silicon oxide material prepared in Example 1 of the present invention. The horizontal axis is the cycle number, the unit is: week; the vertical axis is the charge specific capacity, the unit is: milliampere hour / gram (mAh / g).
[0020] Figure 7 This is the rate performance curve of the double carbon layer coated silicon oxide material prepared in Example 1 of the present invention. The horizontal axis is the cycle number, the unit is: cycle; the vertical axis is the charge specific capacity, the unit is: milliampere hour / gram (mAh / g).
[0021] Figure 8 The electrochemical cycle performance curve of the comparative example is shown in FIG. 1 , wherein the horizontal axis is the cycle number, in units of weeks; and the vertical axis is the charge specific capacity, in units of milliampere hours per gram (mAh / g).
[0022] Curve a in the figure is the electrochemical cycle performance curve of the graphene-coated silicon dioxide material prepared in Comparative Example 1;
[0023] Curve b in the figure is the electrochemical cycle performance curve of the double carbon layer coated silicon oxide material with different coating sequences prepared in Comparative Example 3;
[0024] Curve c in the figure is the electrochemical cycling performance curve of the polydopamine-derived carbon-coated silicon dioxide material prepared in Comparative Example 2. DETAILED DESCRIPTION
[0025] In order to further illustrate the technical solution of the present invention, the implementation scheme of the present invention is described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the technical solution of the present invention, rather than limiting the claims of the present invention.
[0026] Example 1
[0027] (1) Preparation of polydopamine-coated silicon dioxide (SiO@PDA) material: Weigh 1.0 g of silicon dioxide powder and disperse it in 100 mL of Tris-HCl buffer solution (pH = 8.5), add 0.5 g of dopamine hydrochloride, ultrasonicate for 30 min, mix evenly, and stir magnetically for 12 h to allow dopamine to fully polymerize on the SiO surface. Filter and wash several times, transfer the filter cake to a vacuum oven, and dry it at 60 °C for 8 h to obtain SiO@PDA.
[0028] (2) Preparation of double carbon layer coated silicon dioxide (SiO@PDA@GO): 1.0 g SiO@PDA was slowly added into 40 mL (5 mg / mL) graphene oxide dispersion. SiO@PDA :m GO =5:1, ultrasonic for 40 minutes to make it evenly mixed, then heated in a water bath at 90°C for 40 minutes, centrifuged the mixture, took the precipitate, and freeze-dried it to obtain SiO@PDA@GO. The obtained solid powder was ground and transferred to a clean porcelain boat, placed in the middle area of a tube furnace, and a H2 / Ar mixed gas containing 5% H2 was introduced. It was calcined at 800°C for 2 hours to fully reduce the graphene oxide and carbonize the polydopamine. After cooling to room temperature, SiO@NC@rGO was obtained.
[0029] The scanning electron microscopy results of the double carbon layer coated silicon oxide material prepared in this example are as follows: Figure 2 As shown, the overall coating effect is good and relatively uniform. Figure 4 The infrared spectrum at 790 cm -1 The Si-O vibration peak of SiO appears at 3470 cm -1 The broad peak at 1385 cm is the vibration peak of OH. -1 The peak that appears at is the stretching vibration of CN in the amide bond, indicating that the amino group and the carboxyl group have a bonding effect. Figure 5 The HRTEM image shows two obvious coating layers outside the silicon oxide particles, in which the graphene layer has clear lattice fringes and a crystal plane spacing of 0.34nm, corresponding to the (002) crystal plane of carbon, while polydopamine will be converted into amorphous carbon at 800℃, without lattice fringes, corresponding to the part between silicon oxide and graphene in the figure. This shows that the dopamine carbon layer can be used as a "bridge" to connect SiO and graphene, achieving a relatively ideal coating effect.
[0030] The button cell assembled with the double carbon layer coated silicon oxide material prepared in this example was subjected to electrochemical performance test at a constant temperature of 28°C. The cycle performance is shown in FIG. Figure 6 As shown, the rate performance is Figure 7As shown, the material has a first charge specific capacity of 1439.4 mAh / g and a capacity retention rate of 92% after 50 cycles at 0.2C.
[0031] Example 2
[0032] (1) Preparation of polydopamine-coated silicon dioxide (SiO@PDA) material: Weigh 1.0 g of silicon dioxide powder and disperse it in 100 mL of Tris-HCl buffer solution (pH = 8.3), add 0.5 g of dopamine hydrochloride, ultrasonicate for 35 min, mix evenly, and stir magnetically for 16 h to allow dopamine to fully polymerize on the SiO surface. Filter and wash several times, transfer the filter cake to a vacuum oven, and dry at 65 °C for 6 h to obtain SiO@PDA.
[0033] (2) Preparation of double carbon layer coated silicon dioxide (SiO@NC@rGO) material: 1.0 g SiO@PDA was slowly added into 40 mL (5 mg / mL) graphene oxide dispersion. SiO@PDA :m GO =5:1, ultrasonic for 35 minutes to make it evenly mixed, then heated in a water bath at 85°C for 45 minutes, centrifuged the mixture, took the precipitate, and freeze-dried it to obtain SiO@PDA@GO. The obtained solid powder was ground and transferred to a clean porcelain boat, placed in the middle area of a tube furnace, and a H2 / Ar mixed gas containing 5% H2 was introduced. It was calcined at 900°C for 2.5 hours to fully reduce the graphene oxide and carbonize the polydopamine. After cooling to room temperature, SiO@NC@rGO was obtained.
[0034] The button cell assembled with the double carbon layer coated silicon oxide material prepared in this embodiment was subjected to electrochemical performance test at a constant temperature of 28°C. The initial charge specific capacity of the material was 1060.9 mAh / g, and the capacity retention rate after 50 cycles at 0.2C was 95%.
[0035] Example 3
[0036] (1) Preparation of polydopamine-coated silicon dioxide (SiO@PDA) material: Weigh 1.0 g of silicon dioxide powder and disperse it in 100 mL of Tris-HCl buffer solution (pH = 8.7), add 0.5 g of dopamine hydrochloride, ultrasonicate for 25 min, mix evenly, and stir magnetically for 20 h to allow dopamine to fully polymerize on the SiO surface. Filter and wash several times, transfer the filter cake to a vacuum oven, and dry it at 55 °C for 10 h to obtain SiO@PDA.
[0037] (2) Preparation of double carbon layer coated silicon dioxide (SiO@NC@rGO): 1.0 g SiO@PDA was slowly added into 20 mL (5 mg / mL) graphene oxide dispersion. SiO@PDA :mGO =10:1, ultrasonic for 45 minutes to make it evenly mixed, then heated in a water bath at 95°C for 30 minutes, centrifuged the mixture, took the precipitate, and freeze-dried it to obtain SiO@PDA@GO. The obtained solid powder was ground and transferred to a clean porcelain boat, placed in the middle area of a tube furnace, and a H2 / Ar mixed gas containing 5% H2 was introduced. It was calcined at 800°C for 3 hours to fully reduce the graphene oxide and carbonize the polydopamine. After cooling to room temperature, SiO@NC@rGO was obtained.
[0038] The electrochemical performance of the button-type battery assembled with double carbon layer coated silicon dioxide prepared in this embodiment was tested at a constant temperature of 28° C. The initial charge specific capacity of the material was 1039.8 mAh / g, and the capacity retention rate after 50 cycles at 0.2C was 83%.
[0039] Example 4
[0040] (1) Preparation of polydopamine-coated silicon dioxide (SiO@PDA) material: Weigh 1.0 g of silicon dioxide powder and disperse it in 100 mL of Tris-HCl buffer solution (pH = 8.5), add 0.5 g of dopamine hydrochloride, ultrasonicate for 30 min, mix evenly, and stir magnetically for 12 h to allow dopamine to fully polymerize on the SiO surface. Filter and wash several times, transfer the filter cake to a vacuum oven, and dry it at 60 °C for 8 h to obtain SiO@PDA.
[0041] (2) Preparation of double carbon layer coated silicon dioxide (SiO@PDA@GO): 1.0 g SiO@PDA was slowly added into 25 mL (5 mg / mL) graphene oxide dispersion. SiO@PDA :m GO =8:1, ultrasonic for 40 minutes to make it evenly mixed, then heated in a water bath at 90°C for 50 minutes, centrifuged the mixture, took the precipitate, and freeze-dried it to obtain SiO@PDA@GO. The obtained solid powder was ground and transferred to a clean porcelain boat, placed in the middle area of a tube furnace, and a H2 / Ar mixed gas containing 5% H2 was introduced. It was calcined at 850°C for 2 hours to fully reduce the graphene oxide and carbonize the polydopamine. After cooling to room temperature, SiO@NC@rGO was obtained.
[0042] The electrochemical performance of the button-type battery assembled with double carbon layer coated silicon oxide prepared in this embodiment was tested at a constant temperature of 28°C. The initial charge specific capacity of the material was 1165.5 mAh / g, and the capacity retention rate after 50 cycles at 0.2C was 88%.
[0043] Comparative Example 1
[0044] In order to verify the effect of only a single-layer graphene coating, this comparative example synthesized a silicon oxide material coated with only graphene as a comparison.
[0045] (1) Preparation of graphene-coated silicon dioxide material (SiO@rGO)
[0046] 1.0 g SiO powder was dispersed in 300 mL deionized water, and 5 mL polydiallyl dimethyl ammonium chloride (PDDA) was added. The SiO surface was ultrasonicated for 30 min to make it positively charged. The SiO surface was washed three times with deionized water to remove the excess PDDA. The remaining solid was dispersed in deionized water and slowly added dropwise to 40 mL graphene oxide dispersion (5 mg / mL) under stirring. SiO@PDA :m GO =5:1, stirred at 500rpm / min for 5h, centrifuged, freeze-dried, and SiO@GO was obtained. The solid powder was ground and transferred to a clean porcelain boat, placed in the middle area of the tube furnace, and a H2 / Ar mixed gas containing 5% H2 was introduced. It was calcined at 800℃ for 2h to fully reduce the graphene oxide. After cooling to room temperature, SiO@rGO was obtained. The thermal decomposition temperature of PDDA is 280℃, so during the high-temperature thermal reduction process, PDDA decomposed and disappeared, and only graphene was included in the product material.
[0047] The scanning electron microscopy results of the graphene-coated silicon oxide material prepared in this example are as follows: Figure 3 As shown, it can be seen that part of the silicon oxide is coated by graphene, and there are still many exposed SiO particles and scattered graphene sheets, indicating that the coating effect of the SiO@rGO composite material prepared by this method is not very good.
[0048] The electrochemical performance of the button cell assembled with the graphene-coated silicon dioxide material prepared in this comparative example was tested at a constant temperature of 28°C. The results are as follows: Figure 8 As shown in the middle curve a, the first charge specific capacity of the material is 1731.3 mAh / g, and the capacity retention rate after 50 cycles at 0.2C is 56%.
[0049] Comparative Example 2
[0050] In order to verify the effect of only a single layer of polydopamine-derived carbon coating, a silicon oxide material coated with only polydopamine-derived carbon was synthesized as a comparison.
[0051] (1) Preparation of polydopamine-derived carbon-coated silicon dioxide (SiO@NC) material: 0.6057 g Tris and 187.8 μL hydrochloric acid were mixed and dissolved in an appropriate amount of deionized water. After the mixture was dissolved and mixed evenly, it was transferred to a 100 mL volumetric flask and shaken to obtain a Tris-HCl buffer solution. 1.0 g SiO powder was dispersed in 100 mL Tris-HCl buffer solution (pH = 8.5), 0.5 g dopamine hydrochloride was added, ultrasonicated for 30 minutes, mixed evenly, and magnetically stirred for 12 hours to allow dopamine to fully polymerize on the SiO surface. The mixture was filtered and washed several times. The filter cake was transferred to a vacuum oven and dried at 60 ° C for 8 hours to obtain SiO@PDA. The solid powder was ground and transferred to a clean porcelain boat, placed in the middle area of a tube furnace, argon was introduced, and the mixture was calcined at 800 ° C for 2 hours to carbonize the polydopamine. After cooling to room temperature, SiO@NC was obtained.
[0052] The polydopamine-derived carbon-coated silicon dioxide material prepared in this comparative example was assembled into a button-type battery and the electrochemical performance was tested at a constant temperature of 28°C. The results are as follows: Figure 8 As shown in the middle curve c, the first charge specific capacity of the material is 1465.8 mAh / g, and the capacity retention rate after 50 cycles at 0.2C is 44%.
[0053] Comparative Example 3
[0054] In order to verify the effect of different coating orders, silicon oxide material coated with graphene first and then with polydopamine-derived carbon was synthesized as a comparison.
[0055] (1) Preparation of graphene oxide-coated silicon dioxide material (SiO@GO)
[0056] 1.0 g SiO powder was dispersed in 300 mL deionized water, and 5 mL polydiallyl dimethyl ammonium chloride (PDDA) was added. The SiO surface was ultrasonicated for 30 min to make it positively charged. The SiO surface was washed three times with deionized water to remove the excess PDDA. The remaining solid was dispersed in deionized water and slowly added dropwise to 40 mL graphene oxide dispersion (5 mg / mL) under stirring. SiO@PDA :m GO =5:1, stirred at 500 rpm / min for 5 h, centrifuged, and freeze-dried to obtain SiO@GO.
[0057] (2) Preparation of double carbon layer coated silicon oxide (SiO@rGO@NC): 1.0g SiO@GO powder was dispersed in 100mL Tris-HCl buffer solution (pH=8.5), 0.5g dopamine hydrochloride was added, ultrasonicated for 30min, mixed evenly, magnetically stirred for 12h, dopamine was fully polymerized on the surface of SiO@GO, filtered, washed several times, and the filter cake was transferred to a vacuum oven and dried at 60℃ for 8h. The solid powder was ground and transferred to a clean porcelain boat, placed in the middle area of a tube furnace, and a H2 / Ar mixed gas containing 5% H2 was introduced. The mixture was calcined at 800℃ for 2h to reduce graphene oxide and carbonize polydopamine. After cooling to room temperature, SiO@rGO@NC was obtained.
[0058] The electrochemical performance of the button cells assembled with double carbon layer coated silicon dioxide materials with different coating sequences prepared in this comparative example was tested at a constant temperature of 28°C. The results are as follows: Figure 8 As shown in the middle curve b, the first charge specific capacity of the material is 1244.7 mAh / g, and the capacity retention rate after 50 cycles at 0.2C is 71%.
Claims
1. A double carbon layer coated silicon oxide negative electrode material, characterized in that: The material has an armor-like characteristic structure. The silicon oxide particles used have a diameter of 3 to 6 microns, and the average sheet diameter of graphene is 0.5 to 1.5 microns. The armor structure is a characteristic structure formed by multiple pieces of small-sheet graphene coated on the outside of the silicon oxide particles. The double carbon layer comprises small-sheet graphene and polydopamine-derived carbon from the outside to the inside. The graphene and polydopamine-derived carbon coating layers are connected by an amide bond to anchor the graphene and prevent it from falling off. The mass percentages of the various components are: polydopamine-derived carbon accounts for 8% to 13%, graphene accounts for 8% to 20%, and the rest is silicon oxide.
2. The method for preparing the double carbon layer coated silicon oxide negative electrode material according to claim 1, characterized in that: The self-polymerization reaction of dopamine is used to coat polydopamine on the surface of silicon oxide, and graphene oxide is coated on its surface by liquid phase self-assembly. After calcination under a reducing atmosphere, a double carbon layer-coated silicon oxide negative electrode material is obtained. The specific process steps are as follows: (1) Preparation of polydopamine-coated silicon dioxide (SiO@PDA) material: silicon dioxide powder was dispersed in a Tris-HCl buffer solution (pH = 8.3-8.7) at a solid-liquid ratio of 1:100, and dopamine hydrochloride was added at a mass ratio of silicon dioxide to dopamine hydrochloride of 1.5:1-2.5:
1. Ultrasonication was performed for 25-35 minutes, and the mixture was evenly mixed. The mixture was magnetically stirred for 12-20 hours to allow dopamine to fully polymerize on the SiO surface to form a polydopamine coating layer. The mixture was filtered and washed several times. The filter cake was transferred to a vacuum oven and dried at 55-65°C for 6-10 hours to obtain SiO@PDA. (2) Preparation of double carbon layer coated silicon dioxide (SiO@NC@rGO) material: SiO@PDA prepared in step (1) is slowly added to the graphene oxide dispersion, the mass ratio of SiO@PDA to graphene oxide is 10:1 to 5:1, and the two are mixed evenly by ultrasonication for 35 to 45 minutes, and then heated in a water bath at 85 to 95°C with stirring for 30 to 50 minutes to cross-link the carboxyl and amino groups. The mixture is centrifuged, the precipitate is taken, and freeze-dried to obtain SiO@PDA@GO. The obtained solid powder is ground and transferred to a clean porcelain boat, placed in the middle area of a tube furnace, and a hydrogen-argon mixed gas containing 5% hydrogen is introduced. The mixture is calcined at 800 to 900°C for 2 to 3 hours to fully reduce the graphene oxide and carbonize the polydopamine. After cooling to room temperature, SiO@NC@rGO, i.e., graphene and polydopamine-derived carbon double carbon layer coated silicon dioxide material, is obtained.
Citation Information
Cited By
Negative electrode material and preparation method thereof, negative electrode slurry, negative electrode pole piece and lithium ion battery
CN119674048A
Negative electrode material, preparation method, negative electrode slurry, negative electrode sheet, and lithium-ion battery
CN119674048B
Graphene-coated lithium iron phosphate positive electrode material and preparation method thereof
CN119841298A