Composite membrane and preparation method thereof, current collector, pole piece and battery
By introducing AlSiMO film layer as a transition layer in the composite film, combining polymer film layer and using a variety of metal oxides, the defects and interface corrosion of traditional metal films in ultra-thin film processing and long-term use are solved, and stronger The bonding force and corrosion resistance extend the service life of the film layer.
Patent Information
- Application Number
- CN202411107588.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-11
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional metal films are prone to defects when processed into ultra-thin films, and interface corrosion and shedding are prone to occur between the substrate and the metal layer during long-term use, resulting in functional failure.
Using a composite film structure, including a substrate, an AlSiMO film layer and a metal film layer. The AlSiMO film layer serves as a transition layer to form chemical bonds with the polymer film layer to improve the binding force of the film layer, and improve resistance through the mixing of different metal oxides. Corrosive.
Improve the overall performance of the composite film, enhance the binding force with the substrate, reduce the binding force of the metal film layer directly adheres to the polymer film layer, extend the service life of the film layer, and improve the electrolyte Corrosion resistance avoids film layer falling off.
Smart Images

Figure CN119008967A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coating preparation, and in particular to a composite film and a preparation method thereof, a current collector, a pole piece and a battery. Background Art
[0002] With the development of industry, the use of traditional metal films continues to increase. For example, aluminum foil is currently widely used in food and drug packaging, electromagnetic shielding, lithium batteries and other fields. However, the cost of traditional aluminum foil is relatively high, and when processed into ultra-thin films, it is easy to produce defects such as pinholes. In the prior art, a metal film layer is deposited on a substrate to improve the defects of the metal film. For example, a metal film layer is deposited on the surface of a polymer film through a PVD (physical vapor deposition) process, so that the polymer film not only has the characteristics of traditional aluminum foil, but also has lower cost and higher safety.
[0003] Due to the different expansion coefficients of some substrates and metal film materials, the metal film cannot be effectively attached to the substrate. For example, the expansion coefficients of polymer materials and metal film materials are quite different. In order to ensure the effective adhesion of the deposited metal film, a transition layer needs to be introduced between the substrate and the film. As the use environment becomes harsher and the service life increases, the substrate, the transition layer and the metal film layer will separate, causing the film layer to fall off. Summary of the invention
[0004] The main purpose of the present invention is to provide a composite membrane, aiming to improve the performance of the composite membrane through a composite metal membrane layer.
[0005] To achieve the above object, the present invention provides a composite film, comprising a substrate and an AlSiMO film layer disposed on the surface of the substrate, wherein M comprises one or more of Cr, Zr, and Ti;
[0006] The molar content of Al is 30%-70%;
[0007] The molar content of Si is 4%-15%;
[0008] The molar content of M is 1%-10%;
[0009] The molar content of O is 25%-45%, and the substrate includes a metal material or a non-metal material.
[0010] Optionally, the substrate is a polymer film layer.
[0011] Providing a polymer film layer in the composite film can avoid using metal materials for the entire composite film, thereby reducing costs.
[0012] Optionally, the composite film further comprises a metal film layer, and the metal film layer is arranged on a side of the AlSiMO film layer away from the polymer film layer.
[0013] The composite film also includes a metal film layer, which is mainly used to give the composite film metallic properties. Moreover, the metal film layer is arranged on the side of the AlSiMO film layer away from the polymer film layer to avoid the metal film layer being directly arranged on the surface of the polymer film layer, thereby reducing the bonding force of the metal film layer on the composite film.
[0014] Optionally, the thickness of the AlSiMO film layer is 5nm-100nm;
[0015] And / or, the thickness of the polymer film layer is 3um-100um;
[0016] And / or, the thickness of the metal film layer is 0.5um-3um.
[0017] As needed, the thickness of the AlSiMO film layer is 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm, without specific limitation.
[0018] According to needs, the thickness of the polymer film layer is 3um, 10um, 20um, 30um, 40um, 50um, 60um, 70um, 80um, 90um, or 100um, without specific limitation.
[0019] As needed, the thickness of the metal film layer is 0.5um, 1um, 1.5um, 2um, 2.5um, or 3um, without specific limitation.
[0020] Optionally, the material of the polymer film layer includes a composite of one or more of polyethylene terephthalate, polymethyl methacrylate, polycarbonate or polyethylene naphthalate.
[0021] The AlSiMO film layer is combined with the polymer film layer as a transition layer. The AlSiMO film layer and the polymer film layer are combined by forming chemical bonds between the oxygen groups in the metal oxide and the oxygen-containing functional groups on the surface of the polymer film layer. The more oxygen-oxygen chemical bonds there are, the stronger the bonding force is. Therefore, the more oxygen-containing functional groups there are on the surface of the polymer film layer, the greater the possibility of forming oxygen-oxygen chemical bonds. Therefore, the material of the polymer film layer includes polyethylene terephthalate, polymethyl methacrylate, polycarbonate or polyethylene naphthalate, that is, the material of the polymer film layer can be polyethylene terephthalate, polymethyl methacrylate, polycarbonate or polyethylene naphthalate, or two or more materials can be selected from the above materials, or two or more materials can be composited to obtain the polymer film layer. These polymer materials contain oxygen functional groups, which are beneficial to improving the interface bonding force between the AlSiMO film layer and the polymer film layer.
[0022] Optionally, the material of the metal film layer includes metal aluminum, nickel or copper.
[0023] The material of the metal film layer can be aluminum, copper or nickel, without specific limitation. For example, when the composite film is used as the current collector for the positive electrode, the positive electrode can be made of metal aluminum, and when the composite film is used as the current collector for the negative electrode, the negative electrode can be made of metal copper or nickel.
[0024] The present application also provides a method for preparing a composite film, comprising the following steps:
[0025] Put the polymer film into a vacuum furnace and evacuate it;
[0026] The magnetron sputtering target is turned on, an AlSiM alloy target is selected, a mixed gas of Ar gas and O2 is introduced, and an AlSiMO film layer is deposited on the surface of the polymer film.
[0027] In the process of preparing AlSiMO film layer, it is necessary to maintain a vacuum environment to prevent active substances in the air from participating in the reaction during the film formation process and affecting the quality of the film layer. Therefore, the polymer film needs to be placed in a vacuum furnace and evacuated so that the film layer can be prepared in a vacuum environment.
[0028] In order to combine the AlSiMO film layer on the surface of the polymer film, the magnetron sputtering target is opened, the AlSiM alloy target material is selected, and a mixed gas of Ar gas and O2 is introduced to deposit the AlSiMO film layer on the surface of the polymer film.
[0029] Optionally, after the step of placing the polymer film in a vacuum furnace for evacuation, the method further comprises the following steps:
[0030] The ion source is turned on to clean and activate the surface of the polymer membrane.
[0031] There may be stains on the surface of the polymer membrane. In order to clean the surface of the polymer membrane and expose the oxygen functional groups on the surface of the polymer membrane, the ion source is turned on to generate an ion beam to bombard the surface of the polymer membrane, thereby cleaning and activating the surface of the polymer membrane.
[0032] Optionally, in parts by weight, the proportions of the AlSiM alloy target are Al 60wt%-90wt%, Si 8wt%-25wt%, and M 2wt%-15wt%.
[0033] The target material in a suitable proportion can be selected as needed. For example, Al can be 60wt%, 70wt%, 80wt%, or 90wt%; Si can be 8wt%, 10wt%, 15wt%, 20wt%, or 25wt%; M can be 2wt%, 5wt%, 10wt%, or 15wt%, and M includes one or more of Cr, Zr, and Ti.
[0034] Optionally, after depositing an AlSiMO film layer on the surface of the polymer film, the method further includes depositing a metal film layer on the surface of the AlSiMO film layer.
[0035] The metal film layer can be deposited on the AlSiMO film layer by physical vapor deposition, or can be plated on the AlSiMO film layer by electroplating, so that the composite film has metal properties.
[0036] Optionally, in the step of placing the polymer film in a vacuum furnace for evacuation, the background vacuum degree of the vacuum furnace is greater than or equal to 1.0×10 -2 Pa;
[0037] And / or, the ratio of Ar gas to O2 is (2:1)-(1:2);
[0038] And / or, the amount of O2 introduced is 100ml / min-500ml / min;
[0039] And / or, the magnetron sputtering target includes a high-power pulsed magnetron sputtering target, a DC magnetron sputtering target, a medium-frequency magnetron sputtering target or a radio frequency magnetron sputtering target;
[0040] And / or, the target power of the magnetron sputtering target is 10KW-100KW.
[0041] In order to ensure a good reaction environment, when the polymer film is placed in a vacuum furnace for evacuation, the background vacuum of the vacuum furnace is ≥1.0×10 -2 Pa, under a higher vacuum degree, ensure that there is no air in the vacuum furnace to prevent active substances in the air from affecting the quality of the film layer.
[0042] The metal target needs to react with oxygen to generate metal oxides that are deposited on the surface of the polymer film. The ratio of Ar gas to O2 is (2:1)-(1:2), for example, it can be 2:1, 1:1, 1:2, and there is no specific limitation.
[0043] The amount of O2 introduced is 100ml / min, 200ml / min, 300ml / min, 400ml / min, 500ml / min, without specific limitation.
[0044] Magnetron sputtering targets include high-power pulsed magnetron sputtering targets, DC magnetron sputtering targets, medium-frequency magnetron sputtering targets or radio frequency magnetron sputtering targets. Magnetron sputtering targets include high-power pulsed magnetron sputtering targets, DC magnetron sputtering targets, medium-frequency magnetron sputtering targets or radio frequency magnetron sputtering targets, which can be selected according to needs.
[0045] When the magnetron sputtering target is turned on and film formation is carried out, the target power of the magnetron sputtering target is 10KW, 20KW, 30KW, 40KW, 50KW, 60KW, 70KW, 80KW, 90KW, or 100KW, without specific limitation.
[0046] Optionally, the ions of the ion source are inert gas type ions;
[0047] And / or, the power of the ion source is 1KW-10KW.
[0048] When cleaning and activating the surface of the polymer film, the ions in the ion source are inert gas ions, such as helium ions and argon ions, to prevent other active ions from reacting with the polymer on the surface of the polymer film and affecting the quality of the film layer.
[0049] When the ion source is turned on to clean and activate the surface of the polymer membrane, the power of the ion source is 1KW, 2KW, 3KW, 4KW, 5KW, 6KW, 7KW, 8KW, 9KW, or 10KW, without specific limitation.
[0050] The present application also provides a current collector, which includes the composite film, the composite film includes a polymer film, the AlSiMO film layers are provided on two opposite sides of the polymer film, and each AlSiMO film layer is provided with a metal film layer on a side away from the polymer film.
[0051] The composite membrane is used as the current collector, which makes the current collector corrosion-resistant and has good mechanical properties. When immersed in the electrolyte for a long time, it is not easy to have interface corrosion and film shedding, thus avoiding the functional failure of the current collector.
[0052] The present application also provides a pole piece, which includes a current collector and an active material layer stacked in sequence, wherein the current collector is the composite film.
[0053] The current collector is used as the pole piece, so that the pole piece has good performance and improves the safety of the battery.
[0054] The present application also provides a battery, comprising: a cathode electrode piece, an anode electrode piece, a separator and an electrolyte, wherein the cathode electrode piece and / or the anode electrode piece is the electrode piece described.
[0055] Using the above-mentioned pole piece in the battery can improve the safety and service life of the battery.
[0056] The composite film of the present application comprises a substrate and an AlSiMO film layer arranged on the surface of the substrate, wherein M comprises one or more of Cr, Zr, and Ti; the molar content of Al is 30%-70%; the molar content of Si is 4%-15%; the molar content of M is 1%-10%; the molar content of O is 25%-45%, and the substrate comprises a metal material or a non-metal material. The AlSiMO film layer is a composite metal film layer, and the performance of the overall film layer is improved by the combination of different elements. Each metal element exists in the film layer in the form of oxides. The film layer mixed with multiple metal oxides not only has the excellent characteristics of aluminum oxide, but also has the mechanical properties of silicon oxide. The introduction of chromium oxide, zirconium oxide or titanium oxide further improves the corrosion resistance of the film layer, and the AlSiMO film layer can also form a strong bonding force with the substrate to improve the overall performance of the composite film. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0058] Figure 1 Schematic diagram of the process for preparing the composite membrane of the present invention;
[0059] Figure 2 Schematic diagram of the structure of a composite membrane according to an embodiment of the present invention.
[0060] Description of Figure Numbers:
[0061] Label name Label name 100 current collector 20 AlSiMO film 10 Polymer film 30 Metal film layer
[0062] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0063] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0064] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0065] In the present invention, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0066] In addition, in the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the meaning of "and / or" appearing in the full text is to include three parallel solutions. Taking "A and / or B as an example", it includes solution A, or solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0067] In lithium batteries, some metal foils are used, such as aluminum foil, copper foil or nickel foil. In some application scenarios, the metal foil needs to be processed into ultra-thin films. For example, the metal foil is used for the current collector. In order to increase the weight energy density, the metal foil is hoped to be thinner. At this time, when the metal foil is processed into an ultra-thin film, defects such as pinholes are easily generated, and burrs will appear on the metal foil, which makes the metal foil as the current collector of the lithium battery have the risk of internal short circuit. For example, burrs appear on the aluminum foil, and the burrs pierce the diaphragm, causing the positive and negative electrodes to be conductive, resulting in the risk of short circuit.
[0068] Therefore, the existing method is to plate a metal layer on the substrate to solve the above problem. However, due to the extended service life and the harsh use environment, the substrate and the metal layer will separate, affecting the performance, especially in the field of lithium batteries. Due to long-term immersion in electrolyte, the interface between the substrate and the metal layer is prone to corrosion, and the film layer will fall off, resulting in functional failure.
[0069] To this end, the present application provides a composite membrane, aiming to improve the performance of the composite membrane through a composite metal film layer.
[0070] The composite film includes an AlSiMO film layer, wherein M includes one or more of Cr, Zr, and Ti; the molar content of Al is 30%-70%; the molar content of Si is 4%-15%; the molar content of M is 1%-10%; and the molar content of O is 25%-45%.
[0071] The composite film of the present application includes an AlSiMO film layer, wherein M includes one or more of Cr, Zr, and Ti; the molar content of Al is 30%-70%; the molar content of Si is 4%-15%; the molar content of M is 1%-10%; and the molar content of O is 25%-45%. The AlSiMO film layer is a composite metal film layer, and the performance of the overall film layer is improved by the combination of different elements. Each metal element exists in the film layer in the form of oxides. The film layer mixed with multiple metal oxides not only has the excellent characteristics of aluminum oxide, but also has the mechanical properties of silicon oxide. The introduction of chromium oxide, zirconium oxide, or titanium oxide further improves the corrosion resistance of the film layer, and the AlSiMO film layer can also form a strong bonding force with the substrate to improve the overall performance of the composite film.
[0072] It is understood that the composite film includes a substrate and an AlSiMO film layer, wherein the AlSiMO film layer is bonded to the substrate, wherein the material of the substrate is not specifically limited, for example, it can be a metal material or a non-metal material. The thickness of the AlSiMO film layer is not specifically limited and can be set as needed.
[0073] Furthermore, the composite film also includes a polymer film layer, and the AlSiMO film layer is arranged on the surface of the polymer film layer.
[0074] The polymer film layer refers to a film layer composed of a polymer material, and the thickness and shape of the polymer film layer are not limited. The specific polymer material is not limited and can be selected according to the specific application field and application requirements.
[0075] The surface of the polymer film layer refers to, for example, when the polymer film layer is placed in the air, the surface of the polymer film layer that is in contact with the air is the surface of the polymer film layer.
[0076] Providing a polymer film layer in the composite film can avoid using metal materials for the entire composite film, thereby reducing costs. In addition, the polymer film layer has the properties of polymer materials, further improving the safety of the composite film. For example, some polymers are flexible, making the composite film as a whole not easy to tear or break.
[0077] In order to improve the bonding force of the AlSiMO film layer on the surface of the polymer film layer, the material of the polymer film layer can be selected as a polymer material having oxygen-containing functional groups. It can be understood that the oxygen functional groups on the surface of the polymer film layer form oxygen-oxygen chemical bonds with the oxygen groups in the metal oxide, thereby forming a stronger bonding force. The polymer material containing oxygen functional groups and the AlSiMO film layer are connected by chemical bonds, and their bonding force is stronger.
[0078] Furthermore, the composite film also includes a metal film layer, and the metal film layer is arranged on a side of the AlSiMO film layer away from the polymer film layer.
[0079] The metal film layer refers to a film layer composed of a metal material, wherein the material of the metal film layer is not specifically limited, the thickness of the metal film layer is not limited, and the shape of the metal film layer is not limited, and can be selected according to specific application fields and needs.
[0080] The composite film also includes a metal film layer, which is mainly used to give the composite film metallic properties. Moreover, the metal film layer is arranged on the side of the AlSiMO film layer away from the polymer film layer to avoid the metal film layer being directly arranged on the surface of the polymer film layer, thereby reducing the bonding force of the metal film layer on the composite film.
[0081] The metal film layer is arranged on the side of the AlSiMO film layer away from the polymer film layer, which means that the polymer film layer and the metal film layer are arranged on opposite sides of the AlSiMO film layer, respectively, and the AlSiMO film layer is located between the polymer film layer and the metal film layer. The AlSiMO film layer serves as a transition layer to firmly bond the metal film layer to the polymer film layer.
[0082] The method of providing the metal film layer on the AlSiMO film layer is not specifically limited. For example, the metal film layer may be deposited on the AlSiMO film layer by physical vapor deposition, or may be plated on the AlSiMO film layer by electroplating.
[0083] Further, the thickness of the AlSiMO film layer is 5nm-100nm, and / or the thickness of the polymer film layer is 3um-100um, and / or the thickness of the metal film layer is 0.5um-3um.
[0084] It can be understood that, as needed, the thickness of the AlSiMO film layer is 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm, without specific limitation.
[0085] According to needs, the thickness of the polymer film layer is 3um, 10um, 20um, 30um, 40um, 50um, 60um, 70um, 80um, 90um, or 100um, without specific limitation.
[0086] As needed, the thickness of the metal film layer is 0.5um, 1um, 1.5um, 2um, 2.5um, or 3um, without specific limitation.
[0087] Furthermore, the material of the polymer film layer includes a composite of one or more of polyethylene terephthalate, polymethyl methacrylate, polycarbonate or polyethylene naphthalate.
[0088] It can be understood that the AlSiMO film layer is combined with the polymer film layer as a transition layer, and the AlSiMO film layer and the polymer film layer are combined by forming chemical bonds between the oxygen groups in the metal oxide and the oxygen-containing functional groups on the surface of the polymer film layer. The more oxygen-oxygen chemical bonds there are, the stronger the bonding force is. Therefore, the more oxygen-containing functional groups there are on the surface of the polymer film layer, the greater the possibility of forming oxygen-oxygen chemical bonds. Therefore, the material of the polymer film layer includes polyethylene terephthalate, polymethyl methacrylate, polycarbonate or polyethylene naphthalate, that is, the material of the polymer film layer can be polyethylene terephthalate, polymethyl methacrylate, polycarbonate or polyethylene naphthalate, or two materials can be selected from the above materials, or two or more materials can be composited to obtain a polymer film layer. These polymer materials contain oxygen functional groups, which are beneficial to improving the interface bonding force between the AlSiMO film layer and the polymer film layer.
[0089] Furthermore, the material of the metal film layer includes metal aluminum, nickel or copper.
[0090] The material of the metal film layer can be aluminum, copper or nickel, without specific limitation. For example, when the composite film is used as the current collector for the positive electrode, the positive electrode can be made of metal aluminum, and when the composite film is used as the current collector for the negative electrode, the negative electrode can be made of metal copper or nickel.
[0091] Furthermore, if Figure 1 As shown, the present application also provides a method for preparing a composite film, comprising the following steps: placing a polymer film in a vacuum furnace and evacuating the vacuum; opening a magnetron sputtering target, selecting an AlSiM alloy target, introducing a mixture of Ar gas and O2, and depositing an AlSiMO film layer on the surface of the polymer film.
[0092] A vacuum furnace is a furnace that uses a vacuum system (which is carefully assembled from components such as a vacuum pump, a vacuum measuring device, and a vacuum valve) to discharge some of the material in the furnace cavity, making the pressure in the furnace cavity less than a standard atmospheric pressure. The space in the furnace cavity is thus in a vacuum state. This is a vacuum furnace.
[0093] Magnetron sputtering target is one of the important equipment for vacuum coating.
[0094] Target material, coating target material is a sputtering source that forms various functional thin films on substrates through magnetron sputtering, multi-arc ion plating or other types of coating systems under appropriate process conditions. Simply put, the target material is the target material bombarded by high-speed energetic particles.
[0095] That is, in the process of preparing the AlSiMO film layer, it is necessary to maintain a vacuum environment to prevent active substances in the air from participating in the reaction during the film formation process and affecting the quality of the film layer. Therefore, the polymer film needs to be placed in a vacuum furnace and evacuated so that the film layer can be prepared in a vacuum environment.
[0096] In order to combine the AlSiMO film layer on the surface of the polymer film, the magnetron sputtering target is opened, the AlSiM alloy target material is selected, and a mixed gas of Ar gas and O2 is introduced to deposit the AlSiMO film layer on the surface of the polymer film.
[0097] Furthermore, after the step of placing the polymer film in a vacuum furnace for evacuation, the method further comprises the following steps: turning on the ion source to clean and activate the surface of the polymer film.
[0098] Ion source, an ion source is a device that ionizes neutral atoms or molecules and extracts ion beams from them.
[0099] There may be stains on the surface of the polymer membrane. In order to clean the surface of the polymer membrane and expose the oxygen functional groups on the surface of the polymer membrane, the ion source is turned on to generate an ion beam to bombard the surface of the polymer membrane, thereby cleaning and activating the surface of the polymer membrane.
[0100] Of course, other cleaning methods may also be used to clean the surface of the polymer film, such as chemical reagents, which are not specifically limited.
[0101] Furthermore, in terms of weight, the proportions of the AlSiM alloy target are 60wt% to 90wt% of Al, 8wt% to 25wt% of Si, and 2wt% to 15wt% of M.
[0102] That is, the target material with a suitable proportion can be selected as needed. For example, Al can be 60wt%, 70wt%, 80wt%, or 90wt%; Si can be 8wt%, 10wt%, 15wt%, 20wt%, or 25wt%; M can be 2wt%, 5wt%, 10wt%, or 15wt%, and M includes one or more of Cr, Zr, and Ti.
[0103] For example, by adding a certain proportion of silicon and chromium to the aluminum target, the co-deposition of the AlSiCrO transition layer is achieved. The AlSiCrO transition layer not only has the excellent characteristics of aluminum oxide, such as good bonding strength, surface roughness, and corrosion resistance, but also has the mechanical properties of silicon oxide. The introduction of chromium oxide further improves the corrosion resistance and film-based bonding strength of the transition layer.
[0104] Furthermore, after depositing the AlSiMO film layer on the surface of the polymer film, the method further includes depositing a metal film layer on the surface of the AlSiMO film layer.
[0105] That is, a metal film layer can be deposited on the AlSiMO film layer by physical vapor deposition, or a metal film layer can be plated on the AlSiMO film layer by electroplating, so that the composite film has metal properties.
[0106] Furthermore, in the step of placing the polymer film in a vacuum furnace and evacuating the vacuum, the background vacuum degree of the vacuum furnace is ≥1.0×10 -2 Pa; and / or, the ratio of Ar gas and O2 is (2:1)-(1:2); and / or, the amount of O2 introduced is 100ml / min-500ml / min; and / or, the magnetron sputtering target includes a high-power pulsed magnetron sputtering target, a DC magnetron sputtering target, a medium-frequency magnetron sputtering target or a radio frequency magnetron sputtering target; and / or, the target power of the magnetron sputtering target is 10KW-100KW.
[0107] For example, in one embodiment, the background vacuum is drawn to 5×10 -4 Pa, using high-power pulsed magnetron sputtering target, the high-power pulse waveform is square wave, the pulse width is 27μs-29μs, the frequency is 1KHz, and the average power density is 8W / cm 2 , peak power density is 177W / cm 2 When the coil coating method is adopted, the film speed is set to 50m / min-600m / min to obtain the AlSiMO film layer. Of course, the parameters of the equipment can also be changed according to the needs.
[0108] That is, in order to ensure a good reaction environment, when the polymer film is placed in a vacuum furnace and evacuated, the background vacuum of the vacuum furnace is ≥1.0×10 -2Pa, under a higher vacuum degree, ensure that there is no air in the vacuum furnace to prevent active substances in the air from affecting the quality of the film layer.
[0109] The metal target needs to react with oxygen to generate metal oxides that are deposited on the surface of the polymer film. The ratio of Ar gas to O2 is (2:1)-(1:2), for example, it can be 2:1, 1:1, 1:2, and there is no specific limitation.
[0110] The amount of O2 introduced is 100ml / min, 200ml / min, 300ml / min, 400ml / min, 500ml / min, without specific limitation.
[0111] Magnetron sputtering targets include high-power pulsed magnetron sputtering targets, DC magnetron sputtering targets, medium-frequency magnetron sputtering targets or radio frequency magnetron sputtering targets. The types of magnetron sputtering targets include high-power pulsed magnetron sputtering targets, DC magnetron sputtering targets, medium-frequency magnetron sputtering targets or radio frequency magnetron sputtering targets, which can be selected according to needs. The working principle of magnetron sputtering is that electrons collide with argon atoms in the process of flying to the substrate under the action of the electric field E, ionizing them to produce Ar positive ions and new electrons; new electrons fly to the substrate, and Ar ions are accelerated to fly to the cathode target under the action of the electric field, and bombard the target surface with high energy, causing the target material to sputter. Among the sputtered particles, neutral target atoms or molecules are deposited on the substrate to form a thin film.
[0112] Among them, high-power pulsed magnetron sputtering technology has obvious advantages. It is a new type of magnetron sputtering technology that combines magnetron sputtering with pulse discharge. It can achieve non-melting of target materials and high ionization of sputtered particles under the condition of extremely high transient external power density. Compared with conventional magnetron sputtering technology, high-power pulsed magnetron sputtering technology has two significant characteristics: (1) high peak power density and low average power density. The peak power density of the target surface in high-power pulsed magnetron sputtering technology can reach 107W / m 2 Above, and its average power density is only 105W / m 2 The power density of the sputtered particles is about 2000MW, which is lower than that of ordinary magnetron sputtering. (2) The ionization rate of sputtered particles is very high. In high-power pulsed magnetron sputtering technology, the ionization rate of most sputtered particles is greater than 60%, and some are even higher. For example, the ionization rate of sputtered Ti particles can reach 90%. At the same time, this process can effectively suppress the occurrence of "target poisoning" phenomenon, and the film deposition is dense and uniform, and the thickness is controllable.
[0113] In the present application, a high-power pulsed magnetron sputtering technology is used to prepare an AlSiMO film layer, thereby increasing the ionization rate of the metal material, allowing the metal to react more fully with oxygen, and making the deposited AlSiMO film layer transition layer more dense and uniform, with better bonding strength. Since the AlSiMO film layer is dense and uniform, the AlSiMO film layer is immersed in an electrolyte, and the electrolyte is difficult to pass through the AlSiMO film layer, and the chemical bond between the AlSiMO film layer and the polymer film layer will not be destroyed, thereby avoiding the phenomenon of metal layer shedding due to interface corrosion and stress.
[0114] As the application scope of polymer composite films becomes wider and wider, for example, polyethylene terephthalate composite films, the requirements for metal film layers become higher. In particular, as the current collector of lithium batteries, it is necessary to have strong film-base bonding and electrolyte corrosion resistance. The quality of the transition layer plays a key role in this, and the traditional oxide transition layer can no longer meet the existing needs. In long-term use, the metal layer is prone to fall off due to interface corrosion and stress, resulting in functional failure.
[0115] A new transition layer, AlSiMO film layer, is introduced through high-power pulsed magnetron sputtering technology. This transition layer can improve the performance of the metal film layer and further increase the service life of the product.
[0116] In particular, the present application has significant advantages when other coating methods are used for coating. For example, when using a resistive thermal evaporation vacuum coating machine, in the process of depositing the transition layer, due to the fast resistance evaporation rate, the evaporated material is deposited on the substrate without being completely oxidized, resulting in excessive metal doping in the transition layer, which seriously affects the deposition quality of the oxide layer and reduces the bonding strength of the metal film layer. That is, the metal material is evaporated by the resistive heating method, and the evaporation rate of the metal material is fast. It is directly deposited on the substrate in the form of metal, rather than in the form of metal oxide. When a polymer film is used as a substrate, the metal is directly deposited on the polymer film without oxidation. There is no oxygen-oxygen chemical bond between the polymer film and the metal film, and the bonding strength is greatly weakened. Moreover, the activity of the metal is greater than that of the metal oxide, making the film layer obtained by the resistive thermal evaporation vacuum coating method not corrosion-resistant.
[0117] When the magnetron sputtering target is turned on and film formation is carried out, the target power of the magnetron sputtering target is 10KW, 20KW, 30KW, 40KW, 50KW, 60KW, 70KW, 80KW, 90KW, or 100KW, without specific limitation.
[0118] Further, the ions of the ion source are inert gas type ions. And / or, the power of the ion source is 1KW-10KW.
[0119] When cleaning and activating the surface of the polymer film, the ions in the ion source are inert gas ions, such as helium ions and argon ions, to prevent other active ions from reacting with the polymer on the surface of the polymer film and affecting the quality of the film layer.
[0120] When the ion source is turned on to clean and activate the surface of the polymer membrane, the power of the ion source is 1KW, 2KW, 3KW, 4KW, 5KW, 6KW, 7KW, 8KW, 9KW, or 10KW, without specific limitation.
[0121] Furthermore, the present application also provides a current collector, which includes a composite film, the composite film includes a polymer film, AlSiMO film layers are provided on two opposite sides of the polymer film, and each AlSiMO film layer is provided with a metal film layer on the side away from the polymer film.
[0122] The current collector refers to the structure or part that collects current. In lithium-ion batteries, it mainly refers to metal foil, such as copper foil and aluminum foil. The current collector is used as a substrate to attach the positive or negative active material, and plays the role of collecting the current generated by the active material and outputting a large current to the outside. Generally, aluminum foil is used as the positive current collector, and copper foil is used as the negative current collector.
[0123] The composite membrane is used as the current collector, which makes the current collector corrosion-resistant and has good mechanical properties. When immersed in the electrolyte for a long time, it is not easy to have interface corrosion and film shedding, thus avoiding the functional failure of the current collector.
[0124] Since the composite membrane adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0125] That is, if Figure 2 As shown, AlSiMO film layers 20 are provided on both sides of the polymer film 10, and metal film layers 30 are provided on the AlSiMO film layers 20 on both sides, so that the prepared current collector 100 has good conductivity.
[0126] The present application also provides a pole piece, which includes a current collector and an active material layer stacked in sequence, wherein the current collector is a composite film. Since the current collector adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here one by one.
[0127] For example, the electrode piece may be a cathode electrode piece or an anode electrode piece, and when the electrode piece is a cathode electrode piece, the flexible composite current collector and the cathode material are stacked. When the electrode piece is an anode electrode piece, the flexible composite current collector and the anode material are stacked.
[0128] The current collector is used as the pole piece, so that the pole piece has good performance and improves the safety of the battery.
[0129] The present application also provides a battery, the battery includes: a cathode electrode, an anode electrode, a separator and an electrolyte, wherein the cathode electrode and / or the anode electrode are the electrodes mentioned above. The solvent of the electrolyte includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate, and the solute includes one or more of LiPF6, LiBF4, LiBOB, LiAsF6, Li(CF3SO2)2N, LiCF3SO3, LiClO4. The separator is selected from a film with electrochemical stability and chemical stability, including one or more materials of polyethylene, polypropylene, non-woven fabrics, and polyfiber materials. Since the electrode adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here.
[0130] Using the above-mentioned pole piece in the battery can improve the safety and service life of the battery.
[0131] Example
[0132] Example 1
[0133] The AlSiCrO transition layer was deposited on the film surface by high power pulsed magnetron sputtering.
[0134] 1) Place the polyethylene terephthalate (PET) film into a vacuum furnace and evacuate it to a vacuum level of 6.0 × 10 -3 Pa.
[0135] 2) Turn on the ion source, which is an inert gas, and perform plasma treatment on the surface of the membrane material to activate the surface of the membrane material. The power of the ion source is 6KW.
[0136] 3) Turn on the high-power pulse medium-frequency magnetron target, select AlSiCr alloy target, target ratio Al80wt%, Si12wt%, Cr 8wt%. Introduce Ar gas and O2, the ratio of Ar gas to O2 is 1:1, the amount of O2 introduced is 300ml / min, and the target power is set to 80KW. Deposit a 30nm AlSiCrO transition layer on the surface of the film material.
[0137] 4) A layer of aluminum film is evaporated on the surface of the AlSiCrO transition layer film material, and the thickness of the aluminum film is 800 nm.
[0138] Example 2
[0139] On the basis of Example 1, with other conditions unchanged, the target material ratio was adjusted to 60wt% Al, 25wt% Si, and 15wt% Cr.
[0140] Example 3
[0141] On the basis of Example 1, with other conditions unchanged, the target material ratio was adjusted to 90wt% Al, 8wt% Si, and 2wt% Cr.
[0142] Example 4
[0143] On the basis of Example 1, with other conditions unchanged, the thickness of the deposited AlSiCrO transition layer was adjusted to 5 nm.
[0144] Example 5
[0145] On the basis of Example 1, with other conditions unchanged, the thickness of the deposited AlSiCrO transition layer was adjusted to 100 nm.
[0146] Example 6
[0147] On the basis of Example 1, with other conditions unchanged, an AlSiZr alloy target is selected.
[0148] Example 7
[0149] On the basis of Example 1, with other conditions unchanged, an AlSiTi alloy target is selected.
[0150] Example 8
[0151] On the basis of Example 1, with other conditions unchanged, an AlSiCrZrTi alloy target is selected.
[0152] Comparative Example 1
[0153] The AlO transition layer was deposited on the surface of the film by high power pulsed magnetron sputtering.
[0154] On the basis of Example 1, 100 wt % Al was deposited while other conditions remained unchanged.
[0155] Comparative Example 2
[0156] A SiO transition layer was deposited on the surface of the film material by high-power pulsed magnetron sputtering. Based on Example 1, 100 wt% Si was deposited while other conditions remained unchanged.
[0157] Comparative Example 3
[0158] A CrO transition layer was deposited on the surface of the film material by high-power pulsed magnetron sputtering. Based on Example 1, Cr 100wt% was deposited while other conditions remained unchanged.
[0159] Comparative Example 4
[0160] A ZrO transition layer was deposited on the surface of the film material by high-power pulsed magnetron sputtering. Based on Example 1, 100 wt% Zr was deposited while other conditions remained unchanged.
[0161] Comparative Example 5
[0162] A TiO transition layer was deposited on the surface of the film material by high-power pulsed magnetron sputtering. Based on Example 1, 100 wt% Ti was deposited while other conditions remained unchanged.
[0163] Table 1 Parameters for preparing transition layer
[0164]
[0165] Table 2 Parameters for preparing transition layer
[0166]
[0167]
[0168] Performance Test:
[0169] 1. Test the bonding strength between metal film and substrate
[0170] EAA Test Method
[0171] Test steps: Take 1-2 groups of samples with a width of about 60mm and a length of 150mm-200mm along the longitudinal direction of the film layer, with no less than 3 layers in each group. Align the aluminum-plated surface of the sample with the corona surface of the EAA, and place it flat on the rubber pad. Then cover the non-corona surface of the EAA film with 12μm PET, and place the film together with the rubber pad on the heat sealing test machine for sealing. On the heat-sealed sample, take the heat-sealed part as the center line, take a sample with a width of (15±1)mm and an unfolded length greater than 150mm, and clamp it on the fixture of the tensile testing machine, with the longitudinal axis coinciding with the center of the upper and lower fixtures. The clamping distance is about 50mm, and the speed is 10mm / min.
[0172] 2. Elongation at break test
[0173] Test steps: The specimen width is (15±0.1) mm, the length is at least 150 mm, the distance between the clamps is 100 mm, the specimen gauge length is 50 mm, and the tensile speed is (500±50) mm / min. Test 5 longitudinal and 5 transverse specimens on the tensile testing machine.
[0174] 3. Electrolyte corrosion resistance test
[0175] Test steps: Take a 10cm×10cm sample, soak it in the pre-prepared electrolyte solution, seal it and transfer it to an 85℃ oven. Soak it for 24 hours, 48 hours, 72 hours, and 96 hours respectively, and take it out after completion to observe the changes in the film layer.
[0176] The products prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were subjected to performance tests, and the test results are shown in the following table.
[0177] Table 3 Product performance test
[0178]
[0179]
[0180] Among the various test methods, the metal film and substrate bonding test reflects the strength of the bonding between the metal film and the substrate. The larger the test data, the better the bonding strength. The elongation at break test reflects the fracture deformation of the composite material. The larger the test data, the better the mechanical properties and the less likely it is to break. The electrolyte corrosion resistance test reflects the phenomenon of separation and detachment of the metal film and the substrate when immersed in electrolyte. The larger the test data, the better the corrosion resistance.
[0181] Combining the data in Tables 1 to 3, it can be seen that the transition layers in Examples 1 to 5 are AlSiCrO transition layers, and the transition layers in Comparative Examples 1 to 3 are AlO transition layers, SiO transition layers, and CrO transition layers, respectively. From the test results, it can be obtained that in the test data of Comparative Example 1, its electrolyte corrosion resistance test data is consistent with that in Examples 1 to 5, but the metal film and substrate bonding test data and elongation at break test data of Examples 1 to 5 are much better than the test data of Comparative Example 1; in the test data of Comparative Example 2, although the elongation at break test data is slightly higher than some data in Examples 1 to 5, the metal film and substrate bonding test data and electrolyte corrosion resistance test data are far inferior to the data in Examples 1 to 5; in Comparative Example 3, although the metal film and substrate bonding test data is slightly higher than that in Example 2, its elongation at break test data and electrolyte corrosion resistance test data are much lower than those in Examples 1 to 5. Based on the above data, it can be seen that the comprehensive mechanical properties of the AlSiCrO transition layer are better than those of the AlO transition layer, SiO transition layer and CrO transition layer.
[0182] Embodiment 1, embodiment 6, embodiment 7 and embodiment 8 are AlSiCrO, AlSiZrO, AlSiTiO and AlSiCrZrTiO transition layers respectively. The overall performance of the four transition layers is not much different. Among them, the bonding strength test performance of the metal film of the AlSiCrO transition layer with the substrate is better.
[0183] Comparative Examples 3 to 5 are CrO transition layer, ZrO transition layer, and TiO transition layer, respectively. The overall performance of the three transition layers is not much different. However, in the test performance of the bonding strength between the metal film and the substrate, the CrO transition layer is better, in the test performance of the elongation at break, the TiO transition layer is better, and in the test performance of the electrolyte corrosion resistance, the ZrO transition layer is better.
[0184] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A composite film, characterized in that The composite film comprises a substrate and an AlSiMO film layer disposed on the surface of the substrate, wherein M comprises one or more of Cr, Zr, and Ti; The molar content of Al is 30%-70%; The molar content of Si is 4%-15%; The molar content of M is 1%-10%; The molar content of O is 25%-45%, and the substrate includes a metal material or a non-metal material.
2. The composite film according to claim 1, characterized in that The substrate is a polymer film layer.
3. The composite film according to claim 2, characterized in that The composite film further comprises a metal film layer, and the metal film layer is arranged on a side of the AlSiMO film layer away from the polymer film layer.
4. The composite film according to claim 3, characterized in that The thickness of the AlSiMO film layer is 5nm-100nm; And / or, the thickness of the polymer film layer is 3um-100um; And / or, the thickness of the metal film layer is 0.5um-3um.
5. The composite membrane according to any one of claims 2 to 4, characterized in that The material of the polymer film layer includes a composite of one or more of polyethylene terephthalate, polymethyl methacrylate, polycarbonate or polyethylene naphthalate.
6. The composite film according to claim 5, characterized in that The material of the metal film layer includes metal aluminum, nickel or copper.
7. A method for preparing a composite membrane, characterized in that: The following steps are involved: Put the polymer film into a vacuum furnace and evacuate it; The magnetron sputtering target is turned on, an AlSiM alloy target is selected, a mixed gas of Ar gas and O2 is introduced, and an AlSiMO film layer is deposited on the surface of the polymer film.
8. The method for preparing a composite film according to claim 7, characterized in that: After the step of placing the polymer film in a vacuum furnace and evacuating the vacuum, the following steps are also included: The ion source is turned on to clean and activate the surface of the polymer membrane.
9. The method for preparing a composite membrane according to claim 7 or 8, characterized in that: In terms of weight, the proportions of the AlSiM alloy target are Al 60wt%-90wt%, Si 8wt%-25wt%, and M2wt%-15wt%.
10. The method for preparing a composite membrane according to claim 7 or 8, characterized in that: After the AlSiMO film layer is deposited on the surface of the polymer film, the method further includes depositing a metal film layer on the surface of the AlSiMO film layer.
11. The method for preparing a composite membrane according to any one of claims 7 or 8, characterized in that: In the step of placing the polymer film in a vacuum furnace for evacuation, the background vacuum degree of the vacuum furnace is greater than or equal to 1.0×10 -2 Pa; And / or, the ratio of Ar gas to O2 is (2:1)-(1:2); And / or, the amount of O2 introduced is 100ml / min-500ml / min; And / or, the magnetron sputtering target includes a high-power pulsed magnetron sputtering target, a DC magnetron sputtering target, a medium-frequency magnetron sputtering target or a radio frequency magnetron sputtering target; And / or, the target power of the magnetron sputtering target is 10KW-100KW.
12. The method for preparing a composite film according to claim 8, characterized in that: The ions of the ion source are inert gas ions; And / or, the power of the ion source is 1KW-10KW.
13. A current collector, characterized in that: The current collector comprises a composite film according to any one of claims 3 to 6, wherein the composite film comprises a polymer film, the AlSiMO film layers are provided on two opposite sides of the polymer film, and each AlSiMO film layer is provided with a metal film layer on a side away from the polymer film.
14. A pole piece, characterized in that: The pole piece includes a current collector and an active material layer stacked in sequence, wherein the current collector is the composite film as claimed in claim 13.
15. A battery, characterized in that: include: A cathode electrode sheet, an anode electrode sheet, an isolation membrane and an electrolyte, wherein the cathode electrode sheet and / or the anode electrode sheet is the electrode sheet as claimed in claim 14.
Citation Information
Cited By
Composite current collector based on PP (Polypropylene) base film / PET (Polyethylene Terephthalate) base film and production process
CN121123160A
Composite current collector based on pp-based film / pet-based film and production process
CN121123160B