Laminated battery cell as well as preparation equipment and preparation method thereof

By connecting the electrode sheet and the separator at room temperature and normal pressure, the laminated battery cell is prepared using a folding structure, which solves the poor battery performance problems caused by high temperature and high pressure treatment, improves the liquid absorption effect and interface quality of the battery, and achieves better battery performance.

CN119009378APending Publication Date: 2024-11-22EVE ENERGY CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411389163.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the high-temperature and high-pressure thermal composite electrode and diaphragm process, the existing lithium battery laminate battery cells cause the diaphragm to decrease, affect the battery liquid absorption effect, and cause poor interface conditions, resulting in poor battery performance.

Method used

The electrode sheet is connected to the diaphragm with a normal temperature and pressure conductive adhesive, and the laminated battery cell is prepared through a folded structure to avoid high temperature and high pressure treatment. PVDF-HFP is used as the normal temperature and pressure conductive adhesive to ensure adhesion and conductivity.

Benefits of technology

It improves the liquid absorption effect and interface quality of the battery, improves battery performance, reduces the investment in processing equipment, and ensures conductive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009378A_ABST
    Figure CN119009378A_ABST
Patent Text Reader

Abstract

The invention discloses a laminated battery cell and preparation equipment and a preparation method thereof, the laminated battery cell is prepared by folding a battery cell structure, the battery cell structure comprises a first pole piece, a diaphragm and a second pole piece, the first pole piece is located on one side of the diaphragm, and the first pole piece is connected with the diaphragm through a normal-temperature normal-pressure conductive adhesive; and the second pole pieces are alternately arranged on the sides, away from the first pole pieces, of the diaphragms, and the second pole pieces are connected with the diaphragms through normal-temperature and normal-pressure conductive adhesives. The normal-temperature and normal-pressure conductive adhesive disclosed by the invention has relatively good adhesion performance at normal temperature and normal pressure, and also has relatively good conductivity, so that the problem of poor battery performance caused by high-temperature and high-pressure thermal compounding of a pole piece and a diaphragm in the existing laminated cell processing process is solved, the condition of poor liquid absorption effect and interface of the battery is improved, and the service life of the battery is prolonged. And the battery performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of battery processing technology, and in particular relates to a laminated battery cell and a preparation device and method thereof. Background Art

[0002] The stacked cells of lithium batteries are prepared using a Z-type stacking process, in which the positive electrode sheets, negative electrode sheets and separators are compounded through a thermal composite process and then stacked in a Z-shape to form a core package.

[0003] At present, the technology for compounding pole pieces and diaphragms is to coat hot-melt adhesive on the diaphragm, and then use a hot pressing process to bond the diaphragm and the pole piece together through the adhesive. However, during the hot pressing process, the temperature of the composite roller exceeds 50°C and the pressure needs to exceed 1.2T. Only under the action of high temperature and high pressure can the diaphragm and the pole piece be pressed together. However, the rubber particles on the diaphragm will be flattened, resulting in a decrease in the air permeability of the diaphragm, affecting the liquid absorption effect of the battery. After full charge, the battery interface is prone to purple spots, black spots and other poor interface conditions, resulting in poor battery performance. Summary of the invention

[0004] The embodiments of the present application provide a laminated battery cell and a preparation device and method thereof to solve the problem of poor battery performance caused by high temperature and high pressure thermal composite electrodes and diaphragms in the existing laminated battery cell processing process.

[0005] In a first aspect, an embodiment of the present application provides a laminated battery cell, which is prepared by folding a battery cell structure, and the battery cell structure includes:

[0006] First pole piece;

[0007] A diaphragm, wherein the first pole piece is arranged on one side of the diaphragm, and the first pole piece is connected to the diaphragm through a conductive adhesive at normal temperature and pressure;

[0008] The second pole piece is arranged along the second pole piece on a side of the diaphragm away from the first pole piece, and the second pole piece is connected to the diaphragm on its side through the normal temperature and pressure conductive adhesive.

[0009] Optionally, two diaphragms are provided, namely a first diaphragm and a second diaphragm, the first pole piece is located between the first diaphragm and the second diaphragm, the two sides of the first pole piece are respectively connected to the first diaphragm and the second diaphragm through the conductive adhesive at normal temperature and pressure, the second pole piece is provided on the side of the first diaphragm facing away from the first pole piece and the side of the second diaphragm facing away from the first pole piece, and along the length direction of the diaphragm, multiple second pole pieces are alternately provided on the first diaphragm and the second diaphragm.

[0010] Optionally, the first pole piece is a negative pole piece, and the second pole piece is a positive pole piece.

[0011] Optionally, the negative electrode sheet is a continuous electrode sheet, and the negative electrode sheet corresponds to a plurality of the positive electrode sheets.

[0012] Optionally, a diaphragm is provided, and the first pole piece and the second pole piece are alternately arranged on both sides of the diaphragm, the first pole piece is located on one side of the diaphragm, and one side of the first pole piece is connected to one side of the diaphragm through the conductive adhesive at room temperature and pressure, and the second pole piece is located on the other side of the diaphragm, and one side of the second pole piece is connected to the other side of the diaphragm through the conductive adhesive at room temperature and pressure.

[0013] Optionally, the normal temperature and pressure conductive adhesive is PVDF-HFP

[0014] In a second aspect, an embodiment of the present application provides a device for preparing a laminated battery cell, comprising:

[0015] A first pole piece preparation unit, used for preparing a first pole piece;

[0016] A first glue spraying mechanism, disposed downstream of the first pole piece preparation unit, for spraying a normal temperature and pressure conductive adhesive onto a surface of the first pole piece;

[0017] A diaphragm unwinding mechanism, arranged downstream of the first glue spraying mechanism, for conveying the diaphragm;

[0018] A first composite mechanism is arranged downstream of the diaphragm unwinding mechanism, and comprises two first pressure rollers arranged opposite to each other. After the first pole piece and the diaphragm pass through the first pressure rollers, a first composite tape is prepared. The pressure applied by the first pressure rollers is P1, wherein 0.05T≤P1≤0.1T;

[0019] A second pole piece preparation unit, disposed downstream of the first composite mechanism, for preparing a second pole piece;

[0020] A second glue spraying mechanism, disposed downstream of the second pole piece preparation unit, for spraying the normal temperature and pressure conductive adhesive onto the surface of the second pole piece connected to the first composite tape;

[0021] A second composite mechanism is arranged downstream of the second glue spraying mechanism, and comprises two second pressure rollers arranged opposite to each other. The first composite tape and the second pole piece are passed through the second pressure rollers to prepare a battery cell structure. The pressure applied by the second pressure roller is P2, wherein 0.05T≤P2≤0.1T;

[0022] The folding mechanism is used to fold the battery cell structure to prepare a laminated battery cell.

[0023] Optionally, two first glue spraying mechanisms are provided, and the two first glue spraying mechanisms are used to spray the normal temperature and pressure conductive adhesive onto the two side surfaces of the first pole piece respectively.

[0024] Optionally, two second glue spraying mechanisms are provided, and the two second glue spraying mechanisms are respectively used to spray the normal temperature and pressure conductive adhesive onto one side surface of the second pole piece on both sides of the diaphragm.

[0025] Optionally, the spraying area of ​​the normal temperature and pressure conductive adhesive on the first pole piece is S1, wherein 0.8A1≤S1≤A1, and A1 is the area of ​​one side surface of the first pole piece;

[0026] And / or, the spraying area of ​​the normal temperature and pressure conductive adhesive on the second pole piece is S2, wherein 0.8A2≤S2≤A2, and A2 is the area of ​​one side surface of the second pole piece.

[0027] Optionally, the spraying thickness of the conductive adhesive at room temperature and pressure on the first pole piece is D1, wherein 1 μm≤D1≤2 μm;

[0028] And / or, the thickness of the conductive adhesive sprayed on the second pole piece at room temperature and pressure is D2, wherein 1 μm≤D2≤2 μm.

[0029] Optionally, the room temperature and pressure conductive adhesive is PVDF-HFP.

[0030] In a third aspect, the present application also provides a method for preparing a laminated battery cell, comprising the following steps:

[0031] Prepare a first pole piece and a second pole piece;

[0032] Spraying a normal temperature and pressure conductive adhesive on both sides of the first pole piece, composite-connecting the first pole piece with two layers of diaphragms, spraying the normal temperature and pressure conductive adhesive on one side of the second pole piece, composite-connecting the second pole piece with a side of the diaphragm away from the first pole piece, and preparing a battery cell structure;

[0033] The battery cell structure is folded to prepare a laminated battery cell.

[0034] Optionally, the room temperature and pressure conductive adhesive is PVDF-HFP.

[0035] The embodiments of the present application provide a laminated battery cell and a preparation device and method thereof. The laminated battery cell includes a first pole piece, a second pole piece and a diaphragm. The first pole piece and the diaphragm are compositely connected by a conductive adhesive at room temperature and pressure, and the second pole piece and the diaphragm are compositely connected by a conductive adhesive at room temperature and pressure. The conductive adhesive at room temperature and pressure has good adhesion properties at room temperature and pressure, and also has good conductivity. This overcomes the problem of poor battery performance caused by high temperature and high pressure thermal composite pole pieces and diaphragms in the existing laminated battery cell processing process, improves the battery's liquid absorption effect and poor interface conditions, and improves battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0037] In order to more completely understand the present application and its beneficial effects, the following description will be given in conjunction with the accompanying drawings. In the following description, the same reference numerals represent the same parts.

[0038] Figure 1 A cross-sectional schematic diagram of a first form of a laminated battery cell provided in an embodiment of the present application.

[0039] Figure 2 A cross-sectional schematic diagram of a second form of a laminated battery cell provided in an embodiment of the present application.

[0040] Figure 3 A cross-sectional schematic diagram of a third form of a laminated battery cell provided in an embodiment of the present application.

[0041] Figure 4 The first form of cross-section of the battery cell structure provided in the embodiment of the present application is a schematic diagram.

[0042] Figure 5 The cross-section of the second form of the battery cell structure provided in the embodiment of the present application is a schematic diagram.

[0043] Figure 6 The cross-section of the third form of the battery cell structure provided in the embodiment of the present application is a schematic diagram.

[0044] Figure 7 Schematic diagram of the equipment for preparing the laminated battery cell provided in the embodiment of the present application.

[0045] The accompanying drawings are marked as follows:

[0046] 10. laminated battery cell; 110. first pole piece; 120. diaphragm; 121. first diaphragm; 122. second diaphragm; 130. second pole piece;

[0047] 100, first pole piece preparation unit; 200, first glue spraying mechanism; 300, diaphragm unwinding mechanism; 400, first composite mechanism; 410, first pressure roller; 500, second pole piece preparation unit; 600, second glue spraying mechanism; 700, second composite mechanism; 710, second pressure roller; 800, folding mechanism. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0049] See also Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5 and Figure 6 , an embodiment of the present application provides a laminated battery cell 10, which is prepared by folding a battery cell structure, and the battery cell structure includes a first pole piece 110, a diaphragm 120 and a second pole piece 130. The first pole piece 110 is arranged on one side of the diaphragm 120, and the first pole piece 110 and the diaphragm 120 are connected by a conductive adhesive at normal temperature and pressure. In some embodiments, the conductive adhesive at normal temperature and pressure is PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene). The second pole piece 130 is arranged on the side of the diaphragm 120 away from the first pole piece 110, and the second pole piece 130 is connected to the diaphragm 120 by a conductive adhesive at normal temperature and pressure. The polarity of the first pole piece 110 is opposite to that of the second pole piece 130. A first pole ear is provided on the first pole piece 110, and a second pole ear is provided on the second pole piece 130, and the first pole ear and the second pole ear extend out of the diaphragm 120.

[0050] In the embodiment of the present application, the first pole piece 110 and the second pole piece 130 are connected to the diaphragm 120 by a conductive adhesive at normal temperature and pressure. In the process of compounding the first pole piece 110, the second pole piece 130 and the diaphragm 120, high temperature and high pressure are not required. At normal temperature and pressure (temperature of 25°C and pressure of 1.01325Pa), the first pole piece 110, the second pole piece 130 and the diaphragm 120 can be bonded, and the conductive performance is good. The processing process is simple, and the investment in processing equipment is reduced.

[0051] In some embodiments, the normal temperature and pressure conductive adhesive is PVDF-HFP. PVDF-HFP has good cohesion and good adhesion effect at normal temperature and pressure. At room temperature (25°C), the conductivity of PVDF-HFP is as high as 3.2ms / cm, the electrochemical temperature window can reach 5V, the lithium ion migration number is 0.63, and it has good interfacial compatibility with lithium metal. This improves the cycle stability and safety of lithium batteries.

[0052] In some embodiments, see Figure 1 and Figure 4 , two layers of diaphragms 120 are arranged in the cell structure, namely a first diaphragm 121 and a second diaphragm 122, and the first diaphragm 121 and the second diaphragm 122 are arranged at intervals. The first diaphragm 121 and the second diaphragm 122 both extend along the first direction. The first diaphragm 121 and the second diaphragm 122 have the same shape and size. The first pole piece 110 is located between the first diaphragm 121 and the second diaphragm 122. Along the first direction, the first pole piece 110 is arranged at intervals, and both sides of the first pole piece 110 are coated with a normal temperature and pressure conductive adhesive. One side of the first pole piece 110 is bonded to the first diaphragm 121 by a normal temperature and pressure conductive adhesive, and the other side of the first pole piece 110 is bonded to the second diaphragm 122 by a normal temperature and pressure conductive adhesive. The second pole piece 130 is arranged on the side of the first diaphragm 121 away from the first pole piece 110 and the side of the second diaphragm 122 away from the first pole piece 110. Along the first direction, the second pole pieces 130 located on one side of the first diaphragm 121 and the second pole pieces 130 located on one side of the second diaphragm 122 are alternately arranged in sequence.

[0053] For example, see Figure 1 and Figure 4 , the first pole piece 110 and the second pole piece 130 are both single electrodes, a plurality of first pole pieces 110 are arranged at intervals along the first direction, and a plurality of second pole pieces 130 are arranged at intervals along the first direction. The first pole piece 110 and the second pole piece 130 are arranged in alignment. The first direction is the X-axis direction. When the first pole piece 110 is a negative pole piece, the second pole piece 130 is a positive pole piece. When the first pole piece 110 is a positive pole piece, the second pole piece 130 is a negative pole piece.

[0054] See also Figure 4 and Figure 5, along the first direction, adjacent negative electrode sheets are spaced a certain distance apart. Both sides of the negative electrode sheet are coated with a conductive adhesive at room temperature and pressure, and the two sides of the negative electrode sheet are respectively bonded and connected to the first diaphragm 121 and the second diaphragm 122. One side of the positive electrode sheet is coated with a conductive adhesive at room temperature and pressure, and the positive electrode sheet is bonded and connected to the diaphragm 120 on its side. Along the thickness direction of the negative electrode sheet, the negative electrode sheet and the positive electrode sheet are arranged in alignment. Both the positive electrode sheet and the negative electrode sheet are rectangular sheet structures, the length dimension of the positive electrode sheet is smaller than the length dimension of the negative electrode sheet, and the width dimension of the positive electrode sheet is smaller than the width dimension of the negative electrode sheet. The projections of all negative electrode sheets in the diaphragm 120 fall within the range of the diaphragm 120.

[0055] In some embodiments, the first electrode sheet 110 is a positive electrode sheet, and the second electrode sheet 130 is a negative electrode sheet. Along the first direction, a plurality of positive electrode sheets are arranged in sequence and spaced apart. The number of the second electrode sheets 130 is two more than the number of the first electrode sheets 110. Along the thickness direction, the second electrode sheet 130 is arranged in alignment with the first electrode sheet 110, and the projection of the first electrode sheet 110 completely falls within the projection range of the second electrode sheet 130. The surfaces of both sides of the positive electrode sheet are sprayed with a conductive adhesive at normal temperature and pressure, and the positive electrode sheet is bonded and connected to the first diaphragm 121 and the second diaphragm 122 on both sides. The negative electrode sheet is arranged on the side of the first diaphragm 121 away from the positive electrode sheet and the side of the second diaphragm 122 away from the positive electrode sheet. Along the first direction, the negative electrode sheet on the side of the first diaphragm 121 and the negative electrode sheet on the side of the second diaphragm 122 are arranged alternately.

[0056] In some embodiments, the first electrode sheet 110 is a negative electrode sheet, and the second electrode sheet 130 is a positive electrode sheet.

[0057] For example, see Figure 2 and Figure 5 , along the first direction, adjacent negative electrodes are connected. Multiple first electrodes 110 are connected in a long strip-shaped structure, and the first electrode 110 is a continuous structure. The size of the first electrode 110 is smaller than the size of the diaphragm 120. The projection of the first electrode 110 on the diaphragm 120 falls completely within the range of the diaphragm 120. Both sides of the first electrode 110 are coated with a conductive adhesive at room temperature and pressure, and the first electrode 110 is bonded to the diaphragm 120. Alternatively, a conductive adhesive at room temperature and pressure is coated on the first electrode 110 in an area aligned with the second electrode 130, and the electrode 110 is bonded to the diaphragm 120 within the coating range. Along the first direction, the projections of the positive electrode sheets on the first diaphragm 120 are arranged in sequence at intervals, and the distance between any adjacent positive electrode sheets is the same.

[0058] In some embodiments, see Figure 3 and Figure 6, a plurality of first pole pieces 110, a diaphragm 120 and a plurality of second pole pieces 130 are arranged in the cell structure. The first pole piece 110 is located on one side of the diaphragm 120, and the first pole piece 110 is arranged at intervals along the first direction, and the second pole piece 130 is located on the other side of the diaphragm 120, and the second pole piece 130 is arranged at intervals along the first direction. Along the first direction, the first pole piece 110 and the second pole piece 130 are alternately arranged at intervals. One side of the first pole piece 110 is connected to one side of the diaphragm 120 by a conductive adhesive at normal temperature and pressure, and the second pole piece 130 is located on the other side of the diaphragm 120, and one side of the second pole piece 130 is connected to the other side of the diaphragm 120 by a conductive adhesive at normal temperature and pressure.

[0059] See also Figure 7 The embodiment of the present application also provides a laminated battery cell preparation device, including a first electrode preparation unit 100, a first glue spraying mechanism 200, a diaphragm unwinding mechanism 300, a first composite mechanism 400, a second electrode preparation unit 500, a second glue spraying mechanism 600, a second composite mechanism 700 and a folding mechanism 800 arranged in sequence along the production line.

[0060] In this embodiment, see Figure 7 , the first electrode sheet preparation unit 100 is used to prepare the first electrode sheet 110. The first electrode sheet preparation unit 100 includes an unwinding mechanism and a cutting mechanism, and a electrode sheet material roll is wound on the unwinding mechanism. When the first electrode sheet 110 is a positive electrode sheet, a positive electrode sheet material roll is wound on the corresponding unwinding mechanism. When the first electrode sheet 110 is a negative electrode sheet, a negative electrode sheet material roll is wound on the corresponding unwinding mechanism. The cutting mechanism is used to cut the material roll into multiple first electrode sheets 110. When the first electrode sheet 110 is a positive electrode sheet, the cutting mechanism cuts out multiple positive electrode sheets. When the first electrode sheet 110 is a negative electrode sheet, the cutting mechanism cuts out multiple negative electrode sheets or a continuous negative electrode sheet.

[0061] In this embodiment, see Figure 7 The first glue spraying mechanism 200 is disposed downstream of the first electrode preparation unit 100. The first glue spraying mechanism 200 is used to spray a normal temperature and pressure conductive adhesive onto a surface of the cut first electrode 110 connected to the diaphragm 120. In some embodiments, the normal temperature and pressure conductive adhesive is PVDF-HFP.

[0062] In this embodiment, see Figure 7, the diaphragm unwinding mechanism 300 is arranged downstream of the first glue spraying mechanism 200. When two diaphragms 120 are provided, the diaphragm unwinding mechanism 300 includes a first diaphragm unwinding roll, a second diaphragm unwinding roll and a cutting mechanism. The first diaphragm unwinding roll and the second diaphragm unwinding roll are wound with diaphragm rolls, and the first diaphragm unwinding roll is used to unwind the diaphragm roll, and is cut into the first diaphragm 121 by the cutting mechanism. The second diaphragm unwinding roll is used to unwind the diaphragm material, and is cut into the second diaphragm 122 by the cutting mechanism. The first diaphragm unwinding roll is located on one side of the first pole piece 110, and the second diaphragm unwinding roll is located on the other side of the first pole piece 110. During the unwinding process of the first diaphragm 121 and the second diaphragm 122, the first diaphragm 121 and the second diaphragm 122 are respectively bonded and connected to the first pole piece 110.

[0063] In this embodiment, see Figure 7 , the first composite mechanism 400 is arranged downstream of the diaphragm unwinding mechanism 300. The first composite mechanism 400 includes two first pressure rollers 410 arranged opposite to each other. The first pressure roller 410 does not need to be heated, and compared with the composite roller, it has a simple structure and is easy to maintain. The first electrode piece 110 and the diaphragm 120 after bonding are composited into a first composite belt after passing through the first pressure roller 410. The pressure applied by the first pressure roller 410 is P1, where 0.05T≤P1≤0.1T. The value of P1 can be 0.05T, 0.06T, 0.75T, 0.08T, 0.95T, 0.1T or other unlisted values. The pressure applied by the first pressure roller 410 on the diaphragm 120 and the first electrode piece 110 is relatively small, which reduces the probability of damage to the conductive particles in the conductive adhesive at room temperature and pressure due to excessive pressure, and ensures the conductivity of the conductive adhesive at room temperature and pressure.

[0064] In this embodiment, see Figure 7 , the second pole sheet preparation unit 500 is arranged downstream of the first composite mechanism 400. The second pole sheet preparation unit 500 includes an unwinding mechanism and a cutting mechanism, and a pole sheet material roll is wound on the unwinding mechanism. When the second pole sheet 130 is a positive pole sheet, the corresponding pole sheet material roll is wound with a positive pole sheet material roll, and when the second pole sheet 130 is a negative pole sheet, the corresponding pole sheet material roll is wound with a negative pole sheet material roll. The cutting mechanism is used to cut the material roll into a plurality of second pole sheets 130. The second pole sheet preparation unit 500 is provided with two unwinding mechanisms and two cutting mechanisms, one of which is located on one side of the first pole sheet 110. The other unwinding mechanism and cutting mechanism are located on the other side of the first pole sheet 110.

[0065] In this embodiment, see Figure 7, the second glue spraying mechanism 600 is arranged downstream of the second pole piece preparation unit 500. Two second glue spraying mechanisms 600 are arranged. One second glue spraying mechanism 600 is arranged on one side of the first pole piece 110, and the other second glue spraying mechanism 600 is arranged on the other side of the first pole piece 110. One second glue spraying mechanism 600 is used to spray a normal temperature and pressure conductive adhesive on the surface of the second pole piece 130 on the side of the first diaphragm 121. The other is used to spray a normal temperature and pressure conductive adhesive on the surface of the second pole piece 130 on the side of the second diaphragm 122. In some embodiments, the normal temperature and pressure conductive adhesive is PVDF-HFP.

[0066] In this embodiment, see Figure 7 , the second composite mechanism 700 is arranged downstream of the second glue spraying mechanism 600. The second composite mechanism 700 includes two second pressure rollers 710 arranged opposite to each other. The first composite tape and the second pole piece 130 are composited into a battery cell structure after passing through the second pressure roller 710. The pressure applied by the second pressure roller 710 is P2, where 0.05T≤P2≤0.1T. The value of P2 can be 0.05T, 0.06T, 0.75T, 0.08T, 0.95T, 0.1T or other unspecified values. The pressure applied by the second pressure roller 710 on the second pole piece 130 and the first composite tape is relatively small, which reduces the probability of damage to the conductive particles in the conductive adhesive at room temperature and pressure due to excessive pressure, and ensures the conductivity of the conductive adhesive at room temperature and pressure.

[0067] In this embodiment, the folding mechanism 800 is disposed downstream of the second composite mechanism 700, and the folding mechanism 800 is used to fold the cell structure, thereby forming a stacked cell. For example, the folding mechanism 800 forms a Z-shaped folded cell structure.

[0068] In the embodiment of the present application, the first spraying mechanism 200 sprays a normal temperature and pressure conductive adhesive onto the surface of the first pole piece 110, and the second spraying mechanism 600 sprays a normal temperature and pressure conductive adhesive onto the surface of the second pole piece 130. The first composite mechanism 400 applies a P1 pressure to the first pole piece 110 and the diaphragm 120, and the second composite mechanism 700 applies a P2 pressure to the first pole piece 110, the diaphragm 120, and the second pole piece 130. The first composite mechanism 400 and the second composite mechanism 700 use a pressure roller, and no heating is required, and the normal temperature and pressure conductive adhesive is not affected by high temperature and high pressure. While ensuring the bonding effect of the diaphragm 120 with the negative electrode sheet and the positive electrode sheet, the conductive performance of the normal temperature and pressure conductive adhesive is guaranteed, and the battery performance is good.

[0069] In some embodiments, the first electrode sheet 110 is a negative electrode sheet, and the second electrode sheet 130 is a positive electrode sheet. The first electrode sheet preparation unit 100 can prepare a single-structure negative electrode sheet, or a continuous-structure negative electrode sheet. A single-structure negative electrode sheet refers to one negative electrode sheet corresponding to one positive electrode sheet. A continuous-structure negative electrode sheet refers to one negative electrode sheet corresponding to multiple positive electrode sheets.

[0070] In some embodiments, see Figure 7 , two first glue spraying mechanisms 200 are provided, and the two first glue spraying mechanisms 200 are respectively used to spray the normal temperature and pressure conductive adhesive to the two side surfaces of the first pole piece 110. Exemplarily, the first glue spraying mechanism 200, one first glue spraying mechanism 200 is provided on both sides of the first pole piece 110, and the two first glue spraying mechanisms 200 simultaneously spray the normal temperature and pressure conductive adhesive to the two side surfaces of the cut first pole piece 110. In some embodiments, the normal temperature and pressure conductive adhesive is PVDF-HFP.

[0071] For example, see Figure 7 , two layers of diaphragms 120 are provided, namely a first diaphragm 121 and a second diaphragm 122. One side of the first pole piece 110 is bonded and connected to the first diaphragm 121, and the other side is bonded and connected to the second diaphragm 122. Therefore, both sides of the first pole piece 110 need to be sprayed with a normal temperature and pressure conductive adhesive. At this time, two first glue spraying mechanisms 200 are provided to facilitate the glue spraying operation.

[0072] In some embodiments, see Figure 7 , two second glue spraying mechanisms 600 are provided, and the two second glue spraying mechanisms 600 are respectively used to spray the surface of one side of the second pole piece 130 on both sides of the diaphragm 120 with the normal temperature and pressure conductive adhesive. Exemplarily, one second glue spraying mechanism 600 is provided on one side of the first pole piece 110, and the other second glue spraying mechanism 600 is provided on the other side of the first pole piece 110. One second glue spraying mechanism 600 is used to spray the surface of the second pole piece 130 on the side of the first diaphragm 121 with the normal temperature and pressure conductive adhesive.

[0073] In other embodiments, a first glue spraying mechanism 200 and a second glue spraying mechanism 600 are provided. The first glue spraying mechanism 200 is used to spray a normal temperature and pressure conductive adhesive onto a surface of the first pole piece 110 and the diaphragm 120 on one side thereof. The second glue spraying mechanism 600 is used to spray a normal temperature and pressure conductive adhesive onto a surface of the second pole piece 130 and the diaphragm 120 on one side thereof.

[0074] Exemplarily, a diaphragm 120 is provided, the first pole piece 110 is bonded to one side of the diaphragm 120 by a conductive adhesive at room temperature and pressure, and the second pole piece 130 is bonded to the other side of the diaphragm 120 by a conductive adhesive at room temperature and pressure. Extending along the length direction of the diaphragm 120, the first pole piece 110 and the second pole piece 130 are alternately provided.

[0075] In some embodiments, the spraying area of ​​the normal temperature and pressure conductive adhesive on the first pole piece 110 is S1, wherein 0.8A1≤S1≤A1, and A1 is the area of ​​one side surface of the first pole piece 110. The value of S1 can be 0.8A1, 0.9A1, A1 or other unspecified values.

[0076] In the embodiment of the present application, the glue spraying area of ​​the first pole piece 110 occupies 80% or more of the surface of one side of the first pole piece 110 . The glue spraying area is relatively large, the first pole piece 110 is firmly bonded to the diaphragm 120 , and the conductivity of the conductive adhesive at room temperature and pressure is not affected.

[0077] In some embodiments, the spraying area of ​​the normal temperature and pressure conductive adhesive on the second pole piece 130 is S2, wherein 0.8A2≤S2≤A2, and A2 is the area of ​​one side surface of the second pole piece 130. The value of S2 can be 0.8A2, 0.9A2, A2 or other unspecified values.

[0078] In the embodiment of the present application, the glue spraying area of ​​the second pole piece 130 occupies 80% or more of the surface of one side of the second pole piece 130 . The glue spraying area is larger, the second pole piece 130 is firmly bonded to the diaphragm 120 , and the conductivity of the conductive adhesive at room temperature and pressure is not affected.

[0079] In some embodiments, the thickness of the conductive adhesive sprayed on the first pole piece 110 at room temperature and pressure is D1, wherein 1 μm≤D1≤2 μm. The value of D1 can be 1 μm, 1.2 μm, 1.5 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2 μm or other unspecified values.

[0080] In some embodiments, the thickness of the conductive adhesive sprayed on the second pole piece 130 at room temperature and pressure is D2, wherein 1 μm ≤ D2 ≤ 2 μm. The value of D2 may be 1 μm, 1.2 μm, 1.5 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2 μm or other unspecified values. The value of D2 may be the same as or different from the value of D1.

[0081] The spraying thickness of the normal temperature and normal pressure conductive adhesive on the first pole piece 110 and the second pole piece 130 is moderate, which meets the requirements of bonding, conductivity and other performances while reducing the probability of excessive spraying of the normal temperature and normal pressure conductive adhesive and glue overflow after passing through the pressure roller.

[0082] The present application also provides a method for preparing a laminated battery cell, comprising the following steps:

[0083] S1, preparing a first pole piece 110 and a second pole piece 130;

[0084] S2, spraying a conductive adhesive at room temperature and pressure on both sides of the first pole piece 110, compositely connecting the first pole piece 110 with the two layers of the diaphragm 120, spraying a conductive adhesive at room temperature and pressure on one side of the second pole piece 130, compositely connecting the second pole piece 130 with the side of the diaphragm 120 facing away from the first pole piece 110, and preparing a battery cell structure;

[0085] S3, fold the battery cell structure to prepare a stacked battery cell.

[0086] In the embodiment of the present application, the first pole piece 110 and the second pole piece 130 can be prepared simultaneously or separately, and the preparation of the first pole piece 110 and the second pole piece 130 is completed before the first pole piece 110 and the second pole piece 130 are bonded to the diaphragm 120.

[0087] In some embodiments, the room temperature and pressure conductive adhesive is PVDF-HFP.

[0088] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0089] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features.

[0090] The laminated battery cells and their preparation equipment and preparation methods provided in the embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the methods and core ideas of the present application. At the same time, for technical personnel in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A laminated battery cell (10), characterized in that: The laminated battery cell is prepared by folding the battery cell structure, and the battery cell structure comprises: A first pole piece (110); A diaphragm (120), wherein the first pole piece (110) is arranged on one side of the diaphragm (120), and the first pole piece (110) and the diaphragm (120) are connected by a conductive adhesive at normal temperature and pressure; A second pole piece (130), the second pole piece (130) is arranged on a side of the diaphragm (120) away from the first pole piece (110), and the second pole piece (130) is connected to the diaphragm (120) via the normal temperature and pressure conductive adhesive.

2. The laminated battery core (10) according to claim 1, characterized in that: Two diaphragms (120) are provided, namely a first diaphragm (121) and a second diaphragm (122); the first pole piece (110) is located between the first diaphragm (121) and the second diaphragm (122); the two sides of the first pole piece (110) are respectively connected to the first diaphragm (121) and the second diaphragm (122) through the conductive adhesive at normal temperature and pressure; the second pole piece (130) is provided on a side of the first diaphragm (121) away from the first pole piece (110) and a side of the second diaphragm (122) away from the first pole piece (110); along the length direction of the diaphragm (120), a plurality of the second pole pieces (130) are alternately provided on the first diaphragm (121) and the second diaphragm (122).

3. The laminated battery core (10) according to claim 2, characterized in that: The first pole piece (110) is a negative pole piece, and the second pole piece (130) is a positive pole piece.

4. The laminated battery core (10) according to claim 3, characterized in that: The negative electrode sheet is a continuous electrode sheet, and the negative electrode sheet corresponds to a plurality of positive electrode sheets.

5. The laminated battery core (10) according to claim 1, characterized in that: A diaphragm (120) is provided, and the first pole piece (110) and the second pole piece (130) are alternately arranged on both sides of the diaphragm (120), the first pole piece (110) is located on one side of the diaphragm (120), and one side of the first pole piece (110) is connected to one side of the diaphragm (120) through the conductive adhesive at room temperature and normal pressure, and the second pole piece (130) is located on the other side of the diaphragm (120), and one side of the second pole piece (130) is connected to the other side of the diaphragm (120) through the conductive adhesive at room temperature and normal pressure.

6. The laminated battery core (10) according to any one of claims 1 to 5, characterized in that: The normal temperature and normal pressure conductive adhesive includes PVDF-HFP.

7. A device for preparing a laminated battery cell, characterized in that: include: A first pole piece preparation unit (100), used for preparing a first pole piece (110); A first glue spraying mechanism (200), arranged downstream of the first pole piece preparation unit (100), and used for spraying a normal temperature and pressure conductive adhesive onto the surface of the first pole piece (110); A diaphragm unwinding mechanism (300), disposed downstream of the first glue spraying mechanism (200), and used for conveying the diaphragm (120); A first composite mechanism (400) is arranged downstream of the diaphragm unwinding mechanism (300), and comprises two first pressure rollers (410) arranged opposite to each other. After the first pole piece (110) and the diaphragm (120) pass through the first pressure rollers (410), a first composite tape is prepared. The pressure applied by the first pressure rollers (410) is P1, wherein 0.05T≤P1≤0.1T; A second pole piece preparation unit (500), arranged downstream of the first composite mechanism (400), and used for preparing a second pole piece (130); A second adhesive spraying mechanism (600) is arranged downstream of the second pole piece preparation unit (500) and is used for spraying the normal temperature and pressure conductive adhesive onto the surface of the second pole piece (130) connected to the first composite tape; A second composite mechanism (700) is arranged downstream of the second glue spraying mechanism (600), and comprises two second pressure rollers (710) arranged opposite to each other, the first composite tape and the second pole piece (130) are passed through the second pressure rollers (710) to prepare a battery cell structure, and the pressure applied by the second pressure rollers (710) is P2, wherein 0.05T≤P2≤0.1T; The folding mechanism (800) is used to fold the battery cell structure to prepare a laminated battery cell (10).

8. The equipment for preparing laminated battery core according to claim 7, characterized in that: Two first glue spraying mechanisms (200) are provided, and the two first glue spraying mechanisms (200) are used to spray the normal temperature and pressure conductive adhesive onto the surfaces of both sides of the first pole piece (110) respectively.

9. The equipment for preparing laminated battery core according to claim 8, characterized in that: Two second glue spraying mechanisms (600) are provided, and the two second glue spraying mechanisms (600) are respectively used to spray the normal temperature and pressure conductive adhesive onto the surface of one side of the second pole piece (130) on both sides of the diaphragm (120).

10. The equipment for preparing laminated battery core according to claim 7, characterized in that: The spraying area of ​​the normal temperature and pressure conductive adhesive on the first pole piece (110) is S1, wherein 0.8A1≤S1≤A1, and A1 is the area of ​​a side surface of the first pole piece (110); Alternatively, the spraying area of ​​the normal temperature and pressure conductive adhesive on the second pole piece (130) is S2, wherein 0.8A2≤S2≤A2, and A2 is the area of ​​one side surface of the second pole piece (130).

11. The equipment for preparing laminated battery core according to claim 7, characterized in that: The normal temperature and pressure conductive adhesive sprayed on the first pole piece (110) has a thickness D1, wherein 1 μm≤D1≤2 μm; And / or, the normal temperature and pressure conductive adhesive sprayed on the second pole piece (130) has a thickness D2, wherein 1 μm≤D2≤2 μm.

12. The equipment for preparing laminated battery core according to any one of claims 7 to 11, characterized in that: The normal temperature and normal pressure conductive adhesive includes PVDF-HFP.

13. A method for preparing a laminated battery core, characterized in that: The steps include: Preparing a first pole piece (110) and a second pole piece (130); A normal temperature and pressure conductive adhesive is sprayed on both sides of the first pole piece (110), the first pole piece (110) is compositely connected with two layers of diaphragms (120), the normal temperature and pressure conductive adhesive is sprayed on one side of the second pole piece (130), the second pole piece (130) is compositely connected with a side of the diaphragm (120) facing away from the first pole piece (110), and a battery cell structure is prepared; The battery cell structure is folded to prepare a laminated battery cell (10).

14. The method for preparing a laminated battery core according to claim 13, characterized in that: The normal temperature and normal pressure conductive adhesive includes PVDF-HFP.

Citation Information

Cited By

  • Stacked battery cell, and fabrication apparatus and method therefor

    EP4746174A1

  • Stacked battery cell, and fabrication apparatus and method therefor

    WO2026065718A1