Terahertz photoelectric detector and preparation method thereof
By forming a heterojunction between graphene and perovskite in a terahertz photodetector and modifying the graphene surface through the Al2O3 film layer, the problems of low response speed and irradiation intensity of traditional detectors are solved, and high response is achieved terahertz band detection effect with high detection rate.
Patent Information
- Application Number
- CN202410802796.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-22
AI Technical Summary
The traditional graphene terahertz photodetector has low response speed and is difficult to resist the strong electric field of terahertz radiation, which limits its performance improvement in practical applications.
By sequentially setting the graphene film layer, the aluminum trioxide film layer and the perovskite film layer on the substrate, a heterojunction between graphene and perovskite is formed, and effective detection of terahertz waves is achieved using the Seebeck effect, and The graphene surface is modified by the Al2O3 film layer to improve the film formation quality of the perovskite film.
It realizes terahertz photodetection performance with high responsiveness and high detection rate, can effectively detect terahertz band signals, and improves the stability and performance of the device.
Smart Images

Figure CN119012715A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photoelectric detection devices, and in particular to a terahertz photoelectric detector and a preparation method thereof. Background Art
[0002] Terahertz (THz) spectrum is usually defined as the electromagnetic wave frequency in the range of 0.1-10 THz, which is between microwave and infrared regions. -22 J) It will not cause ionization damage to the human body or other biological tissues, and it is safer. At the same time, terahertz has a certain degree of penetration, and can easily penetrate non-metallic and non-polar materials and dielectric materials (such as foam plastics, paper, cloth, dry wood and ceramics that are opaque to visible light). The good penetration makes terahertz waves promising for transmission imaging. Compared with visible and infrared, the effect of air suspension scattering on terahertz waves is relatively small, and it can be used for imaging in smoke environments, but water vapor will have a large absorption of terahertz waves, which will cause terahertz waves to attenuate, and it should be reasonably avoided. Therefore, terahertz (THz) waves have broad application prospects in non-destructive testing, 6G communications, and national defense. As one of the important components in many applications, the research on terahertz detectors has attracted more attention from researchers. However, the traditional graphene terahertz photodetector has problems such as low light absorption and the delay characteristics of terahertz signal detection at room temperature, which hinders the further improvement of its terahertz wave detection performance. The most commonly used terahertz detectors have some limitations for specific applications. For example, the response speed of pyroelectric detectors and Golay cells is low, and it is difficult to respond to ultra-short terahertz pulse signals of the order of picoseconds in real time. Schottky diode detectors can only have a good response rate below 1THz, but their damage threshold energy is low, which makes it difficult for Schottky diode detectors to resist the strong electric field of terahertz radiation and easily damaged in practical applications.
[0003] To this end, the present invention provides a terahertz photoelectric detector and a method for preparing the same. Summary of the invention
[0004] In order to solve the above-mentioned shortcomings of the prior art such as low response speed and difficulty in resisting the strong electric field of terahertz radiation, the present invention provides a terahertz photodetector and a preparation method thereof.
[0005] A terahertz photoelectric detector and a preparation method thereof of the present invention are realized by the following technical solutions:
[0006] The first object of the present invention is to provide a terahertz photodetector, comprising a substrate, and a graphene film layer, an aluminum oxide film layer and a perovskite film layer stacked in sequence on the substrate; a heterojunction is formed between the graphene film layer and the perovskite film layer.
[0007] It should be noted that in order to avoid the influence of the substrate material on light absorption, in some feasible embodiments of the present invention, a quartz substrate or an ordinary glass substrate with high light transmittance is used as the substrate to achieve low absorption and provide a reference plane and mechanical support.
[0008] The present invention takes into account that the photothermoelectric effect (PTE) generated by the Seebeck coefficient difference between graphene and perovskite materials can achieve effective detection of terahertz waves. Therefore, the present invention attempts to sequentially arrange a graphene film layer and a perovskite film layer on a substrate, so as to form a heterojunction between the graphene film layer and the perovskite film layer, thereby enabling the obtained terahertz photodetector to achieve effective detection of terahertz waves. However, the present invention found in the actual exploration process that the perovskite prepared directly on the surface of the graphene layer has problems such as poor film quality and many defects, and thus the expected effect cannot be obtained, which limits the application of graphene and perovskite materials in the field of terahertz photodetectors. In order to solve the above technical problems, the present invention analyzes the reasons for the defects of the perovskite layer prepared directly on the surface of the graphene layer, and finds that it is mainly due to the high hydrophobicity of the graphene surface, which makes it difficult to prepare a perovskite film on the graphene surface by a solution method. Therefore, in some feasible embodiments of the present invention, the present invention first arranges a graphene film layer on the substrate, and uses the graphene film layer as the main terahertz light absorption layer to realize light absorption and excitation of hot carriers through the graphene film layer. Then, an aluminum oxide film layer (Al2O3 film layer) is arranged on the surface of the graphene film layer, and then a perovskite film layer is arranged, so as to realize the modification of the surface of the graphene film layer through the Al2O3 film layer, which not only improves the barrier to reduce the dark current, but also alleviates the inherent hydrophobicity of the graphene film, and improves the hydrophilicity of the surface of the graphene film layer, so as to facilitate the subsequent formation of a perovskite film layer with adjustable band gap, high absorption coefficient, and high carrier mobility, and enable a heterojunction to be formed between the graphene film layer and the perovskite film layer. And in order to ensure that the above effects can be achieved through the Al2O3 film layer, in some feasible embodiments of the present invention, the thickness of the Al2O3 film layer is 8 to 15nm.
[0009] In some feasible embodiments of the present invention, the thickness of the graphene film layer is 0.3-3 nm to ensure that light absorption and excitation of hot carriers are achieved through the graphene film layer.
[0010] In some feasible embodiments of the present invention, the thickness of the perovskite thin film layer is 400-600 nm to ensure excellent absorbance and thus improve its photoelectric conversion performance.
[0011] In some feasible embodiments of the present invention, the metal electrode layer A is arranged on the surface of the graphene film layer, and the metal electrode layer A is arranged around the Al2O3 film layer, that is, it is arranged in an L-shape on the graphene film layer to realize the collection of electrical signals at the graphene end. In order to ensure that the electrical signals at the graphene end can be collected through the metal electrode layer A, in some feasible embodiments of the present invention, the metal electrode layer A is a silver electrode or a gold electrode. In some feasible embodiments of the present invention, the thickness of the metal electrode layer A is 80 to 100 nm.
[0012] The surface of the perovskite film layer of the present invention is provided with a metal electrode layer B for collecting electrical signals on one side of the perovskite. In order to ensure that the metal electrode layer B can achieve the above-mentioned effects, in some feasible embodiments of the present invention, the metal electrode layer B includes a plurality of metal electrode sheets, and the plurality of metal electrode sheets are evenly spaced along the width direction of the perovskite film layer, so as to realize the collection of electrical signals in multiple regions on one side of the perovskite through the plurality of metal electrode sheets on the perovskite film layer. In other feasible embodiments of the present invention, the plurality of metal electrode sheets are silver electrodes or gold electrodes. In some feasible embodiments of the present invention, the thickness of the plurality of metal electrode sheets is 80 to 100 nm.
[0013] Based on the above, it can be known that the terahertz photodetector of the present invention is to successfully construct a perovskite / graphene heterostructure by setting an Al2O3 film layer between the graphene film layer and the perovskite film layer, so that the terahertz photodetector of the present invention can adjust and generate the Seebeck coefficient difference through the perovskite / graphene heterostructure to enhance the optical response of the terahertz photodetector. When the terahertz wave is irradiated to the terahertz photodetector of the present invention, it will trigger the free electron absorption effect in the graphene and perovskite, and at the same time activate the non-equilibrium carriers of the two, thereby generating the heating of the electron gas or thermionic phenomenon. In addition, there is a difference in the Seebeck coefficient between graphene and perovskite, and this difference will cause the terahertz wave to cause non-uniform heating at both ends of the terahertz photodetector, thereby forming a temperature gradient on both sides of the interface. This temperature difference prompts the equilibrium carriers to flow to the colder area. Due to the uneven distribution of carriers, a thermoelectromotive force (ΔV) is formed in the terahertz photodetector, which triggers the generation of photocurrent. This relationship is given by the formula shown in Formula 1:
[0014] ΔV=ΔS×ΔT Formula 1.
[0015] Where ΔS is the Seebeck coefficient difference between graphene and perovskite, and ΔT is the temperature difference across the interface. Usually, within a single material, the generated thermoelectric potential is basically negligible due to the small surface area and the insignificant difference in the absorption of terahertz waves in different regions. Similarly, in the case of metal electrodes, the resulting thermoelectric potential is almost negligible given the extremely low Seebeck coefficient of the metal.
[0016] The second object of the present invention is to provide a method for preparing the above-mentioned terahertz photoelectric detector, comprising the following steps:
[0017] Step 1: Using a wet transfer method, graphene is transferred to the surface of a substrate to form a graphene film layer on the surface of the substrate, thereby obtaining a substrate having a graphene film layer on the surface.
[0018] It should be noted that in order to ensure that the graphene film can be evenly attached to the substrate, in some feasible embodiments of the present invention, the following steps are specifically adopted:
[0019] 1) A graphene film is formed on the surface of a copper substrate by using a chemical vapor deposition method to obtain a copper substrate having a graphene film on the surface.
[0020] In order to reduce the preparation cost while ensuring that the nucleation and crystallization of carbon atoms can be promoted, in some feasible embodiments of the present invention, a copper substrate is used as a matrix and a chemical vapor deposition method is adopted to make graphene evenly deposited on the surface of the copper substrate and form a uniformly distributed graphene film.
[0021] In order to ensure that a graphene film can be formed on the surface of a copper substrate by chemical vapor deposition, in some feasible embodiments of the present invention, the specific process conditions and process parameters of the chemical vapor deposition method are: the copper substrate is placed in a CVD furnace, argon is used as a protective gas, and after heating to 1000°C, it is kept at 1000°C for 15 to 25 minutes; then the introduction of argon is stopped, and then methane is used as a carbon source, and methane is continuously introduced for 25 to 35 minutes, so that methane is cracked at high temperature to produce carbon atoms, and the carbon atoms quickly diffuse on the surface of the copper substrate and connect with each other to form a graphene lattice structure, thereby realizing the formation of a graphene film on the surface of the copper substrate. After the reaction is completed, the power supply is cut off, the introduction of methane gas is stopped, and then the protective gas argon is introduced to exhaust the methane gas, and the copper substrate with a graphene film on the surface is cooled to room temperature under a protective gas environment, so as to obtain a copper substrate with a graphene film on the surface.
[0022] 2) After fixing the copper substrate with the graphene film on the surface, spin-coating a layer of PMMA solution on the surface of the graphene film, followed by annealing to form a PMMA film on the surface of the graphene film, thereby obtaining a composite film material A with a copper / graphene / PMMA structure.
[0023] The present invention considers that PMMA has the advantages of being able to achieve large-area transfer and being easy to remove. Therefore, in some feasible embodiments of the present invention, a PMMA solution is used as a transfer material, and a PMMA film is formed by spin coating the PMMA solution on the surface of the graphene film, so that in the subsequent transfer process, the composite film material A can be evenly attached to the substrate surface through the PMMA film. In order to ensure the transfer effect, and in some feasible embodiments of the present invention, the mass concentration of the PMMA solution used is 1.5% to 2.5%.
[0024] In order to ensure that the spin-coated PMMA solution can form a PMMA film with uniform components, in some feasible embodiments of the present invention, the copper substrate with a graphene film on the surface is first cut to the required size, and then fixed on a square cover glass, and the PMMA solution is first spin-coated at a speed of 300 to 500 r / min for 4 to 6 seconds; then the PMMA solution is spin-coated at a speed of 1800 to 2200 r / min for 25 to 35 seconds to evenly spin-coat a layer of PMMA solution on the surface of the graphene film. The annealing temperature is 135 to 145° C., and the annealing is 5 to 15 minutes, so that the PMMA film is more closely combined with the graphene film to form a composite film material A with a copper / graphene / PMMA structure.
[0025] 3) Immersing the composite film material A in an ammonium persulfate solution to corrode and remove the copper substrate, thereby obtaining a composite film material B having a graphene / PMMA structure.
[0026] It should be noted that, in order to prevent the presence of the copper substrate from affecting the performance of the subsequently formed terahertz photodetector, the copper substrate in the composite film material A needs to be removed before the composite film material A is attached to the substrate. In some feasible embodiments of the present invention, an ammonium persulfate solution is used as a removal liquid, and the composite film material A is immersed in the ammonium persulfate solution to remove the copper substrate in the composite film material A, thereby obtaining a composite film material B having a graphene / PMMA structure.
[0027] In order to ensure that the ammonium persulfate solution can completely remove the copper substrate, in some feasible embodiments of the present invention, the mass fraction of ammonium persulfate in the ammonium sulfate solution used is 1.5% to 2.5%, the immersion temperature is room temperature, and the immersion time is 8 to 16 hours.
[0028] 4) Using a substrate to fish out the composite film material B, making the composite film material B flatly attached to the surface of the substrate, after drying, using acetone to remove the PMMA film in the composite film material B, and obtaining a substrate having a graphene film layer on the surface.
[0029] It should be noted that, in order to avoid interference from other impurities, before using the substrate to fish out the composite film material B, the substrate was ultrasonically cleaned for 15 minutes using deionized water, acetone, and anhydrous ethanol, respectively, to remove possible impurities.
[0030] It should also be noted that, due to the immersion treatment with ammonium persulfate solution, the surface of the obtained composite film material B may have residual ammonium persulfate solution and other impurities, so the composite film material B is first cleaned and then fished out with a substrate.
[0031] It should be noted that when using acetone to remove the PMMA film in the composite film material B, in order to completely remove the PMMA film, in some feasible embodiments of the present invention, the following method is used for removal: soak the composite film material B in acetone for 8 to 13 minutes, then transfer it to new acetone, and repeat this step at least 3 times to completely remove the PMMA.
[0032] Step 2: using a mask method and electron beam evaporation treatment to form an aluminum oxide thin film layer on the surface of the graphene thin film layer.
[0033] Considering that the melting point of Al2O3 is as high as 2050°C, the present invention adopts electron beam evaporation technology, and can adjust the refractive index of Al2O3 in high vacuum and control the coating evaporation rate to obtain a better Al2O3 film layer.
[0034] In order to ensure that the above effects can be achieved, in some feasible embodiments of the present invention, the following steps are adopted to form an Al2O3 thin film layer on the surface of the graphene thin film layer:
[0035] Place aluminum oxide coating material with a purity of 99.99% in a water-cooled crucible, use a mask process to place the substrate with a graphene film layer on the surface obtained in step 1 into the mask, and place them together above the chamber of a vacuum coating machine, and evacuate the vacuum coating machine to ≤3×10 -4 Pa, set the evaporation rate to 0.25-0.35 nm / s, and process for 30-40 s to form an Al2O3 thin film layer with a thickness of 8-15 nm.
[0036] Step 3, using a one-step anti-solvent spin-on deposition method or a two-step co-deposition method to form a MAPbI3 perovskite film or a FAPbI3 perovskite film on the surface of the Al2O3 film layer to form a perovskite film layer to obtain a substrate with a graphene / aluminum oxide / perovskite structure on the surface.
[0037] It should be noted that the present invention can form a perovskite film on the surface of the Al2O3 film layer by a one-step anti-solvent spin-on deposition method, or can form a perovskite film on the surface of the Al2O3 film layer by a two-step co-deposition method.
[0038] When a perovskite film is formed on the surface of an Al2O3 film layer by a one-step anti-solvent spin-film formation method, in some feasible embodiments of the present invention, the method is specifically implemented by the following steps:
[0039] 1) Weigh lead iodide and methylammonium iodide in an equal molar ratio and set aside.
[0040] 2) DMF and DMSO are mixed in a volume ratio of 3 to 5:1 to obtain a reaction solvent.
[0041] 3) Dispersing the weighed lead iodide and methylammonium iodide in the reaction solvent obtained above, with the ratio of lead iodide to the reaction solvent being 0.8-1.2 mol:1 mL, stirring for 8-12 h, and filtering to obtain a precursor solution.
[0042] 4) coating the precursor liquid on the surface of the Al2O3 thin film layer, and during coating, first spin coating the precursor liquid at a speed of 300-500 r / min for 4-6 seconds; then spin coating the precursor liquid at a speed of 1800-2200 r / min for 25-35 seconds to evenly spin coat a layer of the precursor liquid on the surface of the graphene film; and after spin coating the precursor liquid at a speed of 1800-2200 r / min for 10 seconds, drop coating the EA anti-solvent.
[0043] 5) After the spin coating is completed, the film is placed on a hot plate at 95 to 105° C. for annealing for 10 to 20 minutes to form a MAPbI3 perovskite film layer with a thickness of 400 to 600 nm on the surface of the Al2O3 film layer.
[0044] When a perovskite film is formed on the surface of an Al2O3 film layer by a two-step co-deposition method, in some feasible embodiments of the present invention, the process is specifically implemented by the following steps:
[0045] 1) DMF and DMSO were mixed in a volume ratio of 9:1 to obtain a mixed solvent.
[0046] 2) dispersing and dissolving lead iodide in a mixed solvent to obtain a lead iodide precursor solution having a lead iodide concentration of 1.5 mol / mL.
[0047] 3) dispersing and dissolving guanidine ammonium iodide in isopropyl alcohol (IPA) to obtain a guanidine ammonium iodide precursor solution having a guanidine ammonium iodide concentration of 0.58 mol / mL.
[0048] 4) The lead iodide precursor solution is filtered and coated on the surface of the Al2O3 thin film layer, and the spin coating amount during the coating process is 20-25 μL / cm 2 After spin coating, annealing is performed at 65-75°C for 1 min to form a lead iodide film with a thickness of 400-600 nm.
[0049] 5) After the lead iodide film is cooled to room temperature, the precursor solution of methylammonium iodide is filtered and coated on the lead iodide film, and the amount of spin coating during the coating process is 20-30 μL / cm 2 After the spin coating is completed, annealing is performed at 145-155°C for 10-20 minutes to form a FAPbI3 perovskite film, that is, a perovskite film layer is formed.
[0050] Step 4, using a mask method and vacuum thermal evaporation treatment, depositing a metal electrode layer A on the surface of the graphene film layer, and depositing a metal electrode layer B on the surface of the perovskite film layer, so as to obtain the terahertz photodetector.
[0051] In order to ensure that the deposited silver electrode can achieve the above technical effects, in some feasible embodiments of the present invention, the following steps are specifically used to deposit the silver electrode:
[0052] Using the mask method, a silver coating material with a purity of 99.99% was placed in a water-cooled crucible. The substrate with a graphene / aluminum oxide / perovskite structure on the surface obtained in step 3 was placed in the mask using a mask process, and the substrate was placed above the chamber of the vacuum coating machine. The vacuum coating machine was evacuated to 3×10 -1 Pa, turn on the molecular pump and evacuate to 1×10 -3 ,according to The evaporation rate is increased stepwise in a stepwise manner to achieve the principle of first slow and then fast, and silver is deposited in stages by stepwise increasing the evaporation rate, and finally a metal electrode layer A and a metal electrode layer B with a thickness of 90 nm are formed.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] The present invention takes low-cost, high-sensitivity and high-responsivity terahertz detectors as the object, adopts organic-inorganic metal halide perovskites with flexible band gap control and zero-band gap graphene as photosensitive materials, and obtains graphene perovskite heterojunction devices. Perovskite films with different band gaps are prepared by one-step and two-step processes, and the spectral response characteristics of the organic-inorganic hybrid perovskite film are adjusted by changing the stoichiometric ratio to achieve good ohmic contact with graphene. In order to increase the contact angle between graphene and perovskite, increase the potential barrier to achieve the tunneling effect, an aluminum oxide film is prepared by an electron beam evaporation process, and the evaporation rate is changed by high vacuum, thereby controlling the refractive index of aluminum oxide to form a good deposition on the graphene surface.
[0055] The terahertz detector prepared by the present invention has the excellent performance of room temperature operation, high responsiveness and high detection rate, and can form a high-quality perovskite / graphene heterojunction, thereby realizing effective detection in the terahertz band. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 It is a schematic diagram of the preparation process of the preparation method of the present invention.
[0057] Figure 2 It is a schematic diagram of the device structure of the terahertz photodetector of the present invention.
[0058] Figure 3 This is a physical photograph of the device structure of the terahertz photodetector of the present invention.
[0059] Figure 4 The Raman spectrum of the graphene film obtained in the preparation process of the present invention.
[0060] Figure 5 This is a cross-sectional scanning electron microscope image of the terahertz photodetector of Example 1.
[0061] Figure 6 This is a surface scanning electron microscope image of the perovskite film formed in Example 1.
[0062] Figure 7 This is a diagram showing the change in light-dark current of the terahertz photodetector of Example 1 under terahertz light.
[0063] Figure 8 This is a diagram showing the light-dark current variation of the terahertz photodetector of comparative example 2 under terahertz light. DETAILED DESCRIPTION
[0064] The technical solutions in the embodiments of the present invention will be described clearly and completely below. It should be noted that in the following embodiments of the present invention, the relevant equipment used includes: a vacuum coating machine can be used for vacuum thermal (electronic) deposition of metal and dielectric films to construct a complete perovskite optoelectronic device. Dandong Haoyuan DX-2700 X-ray diffractometer is used for deposition film structure analysis. MicroNanoD-5A atomic force microscope can scan the film surface morphology. UV4100 dual-beam UV / visible spectrophotometer is used to measure the absorption spectrum of perovskite films. South Korea's Ecopia HMS-5000 variable temperature fully automatic Hall effect meter is used to measure the carrier concentration and mobility of perovskite films. Agilent's B1500A semiconductor parameter analyzer can characterize the IV characteristics of perovskite optoelectronic devices. Keysight's DSOX4032A oscilloscope can measure and analyze the time domain characteristics of the device. The American Yiguang Technology QTest spectral measurement system is used for device external quantum efficiency testing. Based on TFC thin film design software and COMSOL finite element analysis software, combined with the 10-core 20-thread Intel workstation in the laboratory, it can be used for electromagnetic simulation of optical devices. The absorption and transmission spectra of the device in the terahertz band are tested by the terahertz time domain spectroscopy system (TDS). The entire time domain waveform of the terahertz pulse is obtained by the equivalent sampling principle, and the frequency domain spectrum of the sample can be obtained by Fourier transform.
[0065] Example 1
[0066] See also Figure 1 This embodiment provides a terahertz photodetector, which is manufactured by the following steps:
[0067] Step 1, wet transfer of graphene on glass substrate:
[0068] 1) A graphene film is formed on the surface of a copper substrate by using a chemical vapor deposition method to obtain a copper substrate having a graphene film on the surface.
[0069] 2) Cut the copper substrate with the graphene film on the surface to the required size, and then fix it on a square cover glass, first spin-coat the PMMA solution at a speed of 400 r / min for 5 seconds; then spin-coat the PMMA solution at a speed of 2000 r / min for 30 seconds to evenly spin-coat a layer of PMMA solution on the surface of the graphene film. The annealing temperature is 140°C for 10 minutes to form a composite film material A with a copper / graphene / PMMA structure so that the PMMA film and the graphene film are more closely combined.
[0070] 3) The composite film material A was immersed in a 2% by mass ammonium persulfate solution at room temperature for 12 hours, and then washed with deionized water to remove the residual ammonium persulfate solution, thereby obtaining a composite film material B.
[0071] 4) The glass substrate was ultrasonically cleaned for 15 minutes with deionized water, acetone, and anhydrous ethanol respectively to obtain a clean glass substrate, and the composite film material B was fished out with the clean glass substrate so that the composite film material B was attached to the glass substrate without wrinkles and flat, and then placed in a clean and dust-free place to dry naturally. Then, acetone was used to remove PMMA, and acetone was replaced by injecting three times with a syringe until PMMA was completely removed and dried naturally to obtain a graphene film that was successfully transferred.
[0072] Step 2, forming an aluminum oxide film (Al2O3 film layer) on the surface of the graphene film layer:
[0073] Aluminum oxide coating material with a purity of 99.99% was placed in a water-cooled crucible. The glass substrate with a graphene film layer on the surface obtained in step 1 was placed in the mask using a mask process. The glass substrate was placed above the chamber of a vacuum coating machine. The vacuum coating machine was evacuated to 3×10 -4 Pa, set the evaporation rate to 0.3nm / s, and process for 30s to form an Al2O3 thin film layer with a thickness of 10nm.
[0074] Step 3, forming a perovskite film on the surface of the Al2O3 film layer:
[0075] A one-step anti-solvent spin-film formation method is used to form a perovskite film on the surface of the Al2O3 film layer:
[0076] 1) Weigh lead iodide and methylammonium iodide in an equal molar ratio and set aside.
[0077] 2) DMF and DMSO were mixed in a volume ratio of 4:1 to obtain a reaction solvent.
[0078] 3) Dispersing the weighed lead iodide and methylammonium iodide in the reaction solvent obtained above, with the ratio of lead iodide to the reaction solvent being 1 mol:1 mL, stirring for 10 h, and filtering to obtain a precursor solution.
[0079] 4) coating the precursor liquid on the surface of the Al2O3 thin film layer, and during coating, first spin coating the precursor liquid at a speed of 400 r / min for 5 seconds; then spin coating the precursor liquid at a speed of 2000 r / min for 30 seconds to evenly spin coat a layer of the precursor liquid on the surface of the graphene film; and after spin coating the precursor liquid at a speed of 2000 r / min for 10 seconds, drop coating the EA anti-solvent.
[0080] 5) After the spin coating is completed, the film is placed on a hot plate at 100° C. for annealing for 15 minutes to form a MAPbI3 perovskite film layer on the surface of the Al2O3 film layer.
[0081] Step 4, depositing silver electrodes:
[0082] Using the mask method, a silver coating material with a purity of 99.99% was placed in a water-cooled crucible. The glass substrate with a graphene / aluminum oxide / perovskite structure on the surface obtained in step 3 was placed in the mask using a mask process, and the glass substrate was placed above the chamber of the vacuum coating machine. The vacuum coating machine was evacuated to 3×10 -1 Pa, turn on the molecular pump and evacuate to 1×10 -3 ,according to The evaporation rate is increased stepwise in a stepwise manner to achieve the principle of slow first and fast later, and the silver deposition is carried out in stages by stepwise increasing the evaporation rate, and finally a 90nm thick "L"-shaped silver electrode is deposited on the graphene surface, and three silver electrode sheets arranged in an array on the perovskite surface, namely electrode 1, electrode 2, and electrode 3. The structural schematic diagram of the obtained terahertz photodetector is shown in Figure 2 As shown, and the actual picture is as Figure 3 shown.
[0083] Example 2
[0084] This embodiment provides a terahertz photoelectric detector, which is manufactured by the following steps:
[0085] Step 1, wet transfer of graphene on glass substrate:
[0086] 1) A graphene film is formed on the surface of a copper substrate by using a chemical vapor deposition method to obtain a copper substrate having a graphene film on the surface.
[0087] 2) Cut the copper substrate with the graphene film on the surface to the required size, and then fix it on a square cover glass, first spin-coat the PMMA solution at a speed of 400 r / min for 5 seconds; then spin-coat the PMMA solution at a speed of 2000 r / min for 30 seconds to evenly spin-coat a layer of PMMA solution on the surface of the graphene film. The annealing temperature is 140°C for 10 minutes to form a composite film material A with a copper / graphene / PMMA structure so that the PMMA film and the graphene film are more closely combined.
[0088] 3) The composite film material A was immersed in a 2% by mass ammonium persulfate solution at room temperature for 12 hours, and then washed with deionized water to remove the residual ammonium persulfate solution, thereby obtaining a composite film material B.
[0089] 4) The glass substrate was ultrasonically cleaned for 15 minutes with deionized water, acetone, and anhydrous ethanol respectively to obtain a clean glass substrate, and the composite film material B was fished out with the clean glass substrate so that the composite film material B was attached to the glass substrate without wrinkles and flat, and then placed in a clean and dust-free place to dry naturally. Then, acetone was used to remove PMMA, and acetone was replaced by injecting three times with a syringe until PMMA was completely removed and dried naturally to obtain a graphene film that was successfully transferred.
[0090] Step 2, forming an aluminum oxide film on the surface of the graphene film layer:
[0091] Aluminum oxide coating material with a purity of 99.99% was placed in a water-cooled crucible. The glass substrate with a graphene film layer on the surface obtained in step 1 was placed in the mask using a mask process. The glass substrate was placed above the chamber of a vacuum coating machine. The vacuum coating machine was evacuated to 3×10 -4 Pa, set the evaporation rate to 0.3 nm / s, and process for 35 s to form an Al2O3 thin film layer with a thickness of 10 nm.
[0092] Step 3, forming a perovskite film on the surface of the Al2O3 film layer:
[0093] A two-step co-deposition method is used to form a perovskite film on the surface of the Al2O3 film layer:
[0094] 1) DMF and DMSO were mixed in a volume ratio of 9:1 to obtain a mixed solvent.
[0095] 2) dispersing and dissolving lead iodide in a mixed solvent to obtain a lead iodide precursor solution having a lead iodide concentration of 1.5 mol / mL.
[0096] 3) dispersing and dissolving guanidine ammonium iodide in isopropyl alcohol (IPA) to obtain a guanidine ammonium iodide precursor solution having a guanidine ammonium iodide concentration of 0.58 mol / mL.
[0097] 4) The lead iodide precursor solution is filtered and coated on the surface of the Al2O3 thin film layer, and the coating amount during the coating process is 20 μL / cm 2 After spin coating, annealing was performed at 70°C for 1 min to form a lead iodide film.
[0098] 5) After the lead iodide film is cooled to room temperature, the precursor solution of methylammonium iodide is filtered and coated on the lead iodide film, and the coating amount during the coating process is 25 μL / cm 2 After the spin coating is completed, annealing is performed at 150°C for 15 minutes to form a FAPbI3 perovskite film, that is, a perovskite film layer is formed.
[0099] Step 4, depositing silver electrodes:
[0100] Using the mask method, a silver coating material with a purity of 99.99% was placed in a water-cooled crucible. The glass substrate with a graphene / aluminum oxide / perovskite structure on the surface obtained in step 3 was placed in the mask using a mask process, and the glass substrate was placed above the chamber of the vacuum coating machine. The vacuum coating machine was evacuated to 3×10 -1 Pa, turn on the molecular pump and evacuate to 1×10 -3 ,according to The evaporation rate is increased step by step in a manner to achieve the principle of slow first and fast later. The silver deposition is carried out in stages by step-by-step increasing the evaporation rate, so as to form an "L"-shaped silver electrode with a thickness of 90nm deposited on the graphene surface, and three silver electrode sheets arranged in an array on the perovskite surface, namely electrode 1, electrode 2, and electrode 3.
[0101] Comparative Example 1
[0102] This comparative example provides a terahertz photodetector, which is prepared by the following steps:
[0103] Step 1, wet transfer of graphene on glass substrate:
[0104] 1) A graphene film is formed on the surface of a copper substrate by using a chemical vapor deposition method to obtain a copper substrate having a graphene film on the surface.
[0105] 2) Cut the copper substrate with the graphene film on the surface to the required size, and then fix it on a square cover glass, first spin-coat the PMMA solution at a speed of 400 r / min for 5 seconds; then spin-coat the PMMA solution at a speed of 2000 r / min for 30 seconds to evenly spin-coat a layer of PMMA solution on the surface of the graphene film. The annealing temperature is 140°C for 10 minutes to form a composite film material A with a copper / graphene / PMMA structure so that the PMMA film and the graphene film are more closely combined.
[0106] 3) The composite film material A was immersed in a 2% by mass ammonium persulfate solution at room temperature for 12 hours, and then washed with deionized water to remove the residual ammonium persulfate solution, thereby obtaining a composite film material B.
[0107] 4) The glass substrate was ultrasonically cleaned for 15 minutes with deionized water, acetone, and anhydrous ethanol respectively to obtain a clean glass substrate, and the composite film material B was fished out with the clean glass substrate so that the composite film material B was attached to the glass substrate without wrinkles and flat, and then placed in a clean and dust-free place to dry naturally. Then, acetone was used to remove PMMA, and acetone was replaced by injecting three times with a syringe until PMMA was completely removed and dried naturally to obtain a graphene film that was successfully transferred.
[0108] Step 2, forming an Al2O3 thin film layer on the surface of the graphene thin film layer:
[0109] Aluminum oxide coating material with a purity of 99.99% was placed in a water-cooled crucible. The glass substrate with a graphene film layer on the surface obtained in step 1 was placed into the mask using a mask process. The glass substrate was placed above the chamber of a vacuum coating machine. The vacuum coating machine was evacuated to 1×10 -3 Pa, set the evaporation rate to 0.1 nm / s, and process for 30 s to form an Al2O3 thin film layer with a thickness of 10 nm.
[0110] Step 3, forming a perovskite film on the surface of the Al2O3 film layer:
[0111] A one-step anti-solvent spin-film formation method is used to form a perovskite film on the surface of the Al2O3 film layer:
[0112] 1) Weigh lead iodide and methylammonium iodide in an equal molar ratio and set aside.
[0113] 2) DMF and DMSO were mixed in a volume ratio of 4:1 to obtain a reaction solvent.
[0114] 3) Dispersing the weighed lead iodide and methylammonium iodide in the reaction solvent obtained above, with the ratio of lead iodide to the reaction solvent being 1 mol:1 mL, stirring for 10 h, and filtering to obtain a precursor solution.
[0115] 4) coating the precursor liquid on the surface of the Al2O3 thin film layer, and during coating, first spin coating the precursor liquid at a speed of 400 r / min for 5 seconds; then spin coating the precursor liquid at a speed of 2000 r / min for 30 seconds to evenly spin coat a layer of the precursor liquid on the surface of the graphene film; and after spin coating the precursor liquid at a speed of 2000 r / min for 10 seconds, drop coating the EA anti-solvent.
[0116] 5) After the spin coating is completed, the film is placed on a hot plate at 100° C. for annealing for 15 minutes to form a MAPbI3 perovskite film layer on the surface of the Al2O3 film layer.
[0117] Step 4, depositing silver electrodes:
[0118] Using the mask method, a silver coating material with a purity of 99.99% was placed in a water-cooled crucible. The glass substrate with a graphene / aluminum oxide / perovskite structure on the surface obtained in step 3 was placed in the mask using a mask process, and the glass substrate was placed above the chamber of the vacuum coating machine. The vacuum coating machine was evacuated to 3×10 -1 Pa, turn on the molecular pump and evacuate to 1×10 -3 ,according to The evaporation rate is increased step by step in a step-by-step manner to achieve the principle of slow first and fast later. The silver deposition is carried out in stages by step-by-step increasing the evaporation rate, and finally a 90nm thick "L"-shaped silver electrode is deposited on the graphene surface, as well as three silver electrode sheets arranged in an array on the perovskite surface.
[0119] The difference between this comparative example and Example 1 is only that:
[0120] When preparing Al2O3 thin film layers, the process parameters of electron beam evaporation treatment are different, that is, the vacuum degree and evaporation rate are different.
[0121] The present invention also found that the aluminum oxide film formed in this comparative example had poor quality and many defects. This is because the refractive index of aluminum oxide is too low under low vacuum and low evaporation rate, resulting in poor film-forming effect. This shows that the process parameters of electron beam evaporation have an important influence on the formation of aluminum oxide films with high quality and good performance. Therefore, when forming an Al2O3 film layer on the surface of the graphene film layer, the process parameters of electron beam evaporation used in the present invention are preferably: vacuum degree ≤3×10 -4 Pa, the evaporation rate is 2.5~3.5nm / s.
[0122] Comparative Example 2
[0123] This comparative example provides a terahertz photodetector, which is prepared by the following steps:
[0124] Step 1, forming a perovskite film on the surface of a glass substrate:
[0125] One-step anti-solvent spin-on deposition method was used to form perovskite films on glass substrates:
[0126] 1) Weigh lead iodide and methylammonium iodide in an equal molar ratio and set aside.
[0127] 2) DMF and DMSO were mixed in a volume ratio of 4:1 to obtain a reaction solvent.
[0128] 3) Disperse the weighed lead iodide and methylammonium iodide in the reaction solvent obtained above, and the ratio of lead iodide to the reaction solvent is 1 mol:1 mL, and stir for 8 to 12 hours, filter, and obtain a precursor solution.
[0129] 4) coating the precursor solution on the surface of the glass substrate, and during coating, first spin coating the precursor solution at a speed of 400 r / min for 5 seconds; then spin coating the precursor solution at a speed of 2000 r / min for 30 seconds to evenly spin coat a layer of the precursor solution on the surface of the graphene film; and after spin coating the precursor solution at a speed of 2000 r / min for 10 seconds, drop coating the EA anti-solvent.
[0130] 5) After the spin coating is completed, the film is placed on a hot plate at 100° C. and annealed for 15 minutes to form a MAPbI3 perovskite thin film layer on the surface of the glass substrate.
[0131] Step 2, depositing silver electrodes:
[0132] Using the mask method, a silver coating material with a purity of 99.99% was placed in a water-cooled crucible. The glass substrate with a perovskite structure on the surface obtained in step 1 was placed in the mask using a mask process, and the glass substrate was placed above the chamber of the vacuum coating machine. The vacuum coating machine was evacuated to 3×10 -1 Pa, turn on the molecular pump and evacuate to 1×10 -3 ,according to The evaporation rate is increased step by step in a step-by-step manner to achieve the principle of slow first and fast later, and the silver deposition is carried out in stages by step-by-step increasing the evaporation rate, and finally a 90nm thick and "L"-shaped silver electrode is deposited on the surface of the substrate, as well as three silver electrode sheets arranged in an array on the surface of the perovskite.
[0133] The difference between this comparative example and Example 1 is only that:
[0134] In this comparative example, no graphene film layer and Al2O3 film layer are formed, and the terahertz photodetector is formed only with the perovskite film layer.
[0135] Experimental Section
[0136] (I) Raman spectroscopy test
[0137] The present invention takes the graphene film obtained in Example 1 as an example, and performs Raman spectroscopy test on it, and the test results are as follows: Figure 4 shown.
[0138] Depend on Figure 4 It can be seen that in the Raman spectrum, the generation of the D peak is mainly attributed to disorder induction or crystal defects, which indicates that the intensity of the D peak can be used to characterize the structural defects in graphene. -1 The D peak intensity at 2685 cm-1 is very low, indicating that the graphene has few defects and the quality of the graphene film is very high. The 2D peak and the G peak are the two main Raman peaks of two-dimensional graphene materials, at 2685 cm-1 and 2685 cm-2, respectively. -1 Position and 1580cm -1 The 2D peak intensity of the single-layer graphene is greater than the G peak, and increases with the number of layers. This shows that the graphene film obtained by the method of the present invention has small defects and high quality.
[0139] (II) Microscopic morphology test
[0140] 1) The present invention takes the terahertz photodetector obtained in Example 1 and the perovskite film formed in Example 1 as examples and performs scanning electron microscope tests on them respectively, and the test results are as follows: Figure 5 and Figure 6 shown.
[0141] in, Figure 5 This is a cross-sectional scanning electron microscope image of the terahertz photodetector of Example 1. It can be seen that from bottom to top, there are a glass substrate layer, a graphene film layer, an Al2O3 film layer, and a perovskite film layer. Figure 5 It can also be seen that the thickness of the Al2O3 film layer is 8 to 15 nm, and the thickness of the perovskite film is 400 to 600 nm.
[0142] Figure 6 This is a surface scanning electron microscope image of the perovskite film formed in Example 1. It can be seen that in the terahertz photodetector of Example 1, the MAPbI3 film particles are dense and evenly arranged, the average grain size can reach 732nm, and it shows very few pores. The high quality advantage of the MAPbI3 film grown on the Al2O3 film can be intuitively observed.
[0143] (III) Photoelectric detection performance test
[0144] The present invention takes the terahertz photodetectors of Example 1 and Comparative Example 2 as examples, and uses the method of detecting terahertz using the thermoelectric effect thereof to test the changes of the light-dark current thereof under terahertz illumination, and the test results are shown as follows: Figure 7 and Figure 8 shown.
[0145] Test method:
[0146] The IV characteristic curve test is based on Ohm's law and Kirchhoff's law. By applying different voltages to the two ends of the terahertz photodetector to measure the current generated, a curve with current and voltage as the horizontal and vertical coordinates is drawn. Analyzing the IV curve can explore the working state of the terahertz photodetector and understand the relevant characteristic parameters of the device, which can effectively evaluate the performance and stability of the optoelectronic device. The IV characteristic curve test process of the terahertz photodetector is divided into dark conditions and terahertz illumination conditions. The current obtained by applying a voltage to both ends of the device under dark conditions is the dark current, and the dark current curve is drawn. The current obtained by applying the same voltage under terahertz illumination is the photocurrent. Among them, the terahertz illumination conditions use a 1060nm femtosecond laser to obtain a femtosecond laser with a pulse width of 70ns, which is attenuated to 10mW-20mW by an attenuator, and then focused by a light focusing mirror onto the low-temperature grown GaAs at the rear end of the terahertz antenna. The 15V-20V AC voltage provided by the voltage source allows the rapid recombination of carriers on the GaAs surface to produce terahertz radiation, and ultimately 0.1THz-3.5THz light can be obtained.
[0147] Figure 7 The figure is a graph showing the change of light-dark current of the terahertz photodetector of Example 1 under terahertz illumination. It can be seen that the maximum light-dark current difference of the terahertz photodetector of Example 1 is about 78 μA when a voltage of 2 V is applied. Then, the responsivity R and the detection rate D* of the terahertz photodetector of Example 1 are calculated according to the formulas shown in Formula 2 and Formula 3, respectively. The calculation results show that the responsivity of the terahertz photodetector of Example 1 is 516 mA / W, and the detection rate is 2.24×10 7 Jones.
[0148]
[0149] Among them, I illu is the current under terahertz light irradiation; I dark is the current under dark conditions; P is the terahertz light power; E e is the terahertz light irradiance; A is the effective illumination area. And the terahertz light irradiance E e About 15.138mW / cm 2 , the effective illumination area A is 1×1μm 2 .
[0150] Figure 8The figure is a graph showing the change of light-dark current of the terahertz photodetector of comparative example 2 under terahertz illumination. It can be seen that the operating voltage of the terahertz photodetector of comparative example 2 can reach 1V, but the light-dark current difference is only 7μA. Similarly, the responsivity and detection rate of the terahertz photodetector of comparative example 2 are calculated according to the formulas shown in formulas 2 and 3 respectively. The calculation results show that the responsivity of the terahertz photodetector of comparative example 2 is 460.81mA / W, and the detection rate is 0.016×10 7 Jones.
[0151] And by comparing the detection performance of the terahertz photodetector of Example 1 and Comparative Example 2, it can be seen that compared with a single perovskite terahertz photodetector, the present invention can significantly improve the responsiveness and detection rate of the terahertz photodetector. This may be because the present invention forms a heterojunction between graphene and perovskite with the assistance of aluminum oxide. The high dielectric constant of Al2O3 not only increases the interface barrier, but also its hydrophilic structure enables MAPbI3 to generate high-quality films by solution method, and the high doping concentration of the perovskite material reduces the width of the barrier region. Therefore, electrons can tunnel through the barrier, generate a large amount of current and dominate the carrier transport behavior, resulting in very low contact resistance of the terahertz device. In addition, the Seebeck coefficient of different materials can cause changes in the contact resistance of the device, which is due to the different concentrations of hot carriers generated under terahertz light, resulting in carrier transport. In general, the introduction of 10nmAl2O3 not only improves the film formation difficulty caused by the high hydrophobicity of the perovskite film in the graphene film, but also increases the interface barrier, providing conditions for the tunneling effect, thereby achieving effective detection in the terahertz band.
[0152] The present invention takes low-cost, high-sensitivity and high-responsivity terahertz photodetectors as the preparation object, and regulates the synthesis of heterojunctions by changing the stoichiometric ratio of perovskite films and modifying the surface of graphene. The preparation of graphene films mainly involves transferring copper-based graphene prepared by CVD (chemical vapor deposition) to a substrate by a wet transfer method, and depositing an aluminum oxide film on the graphene film by an electron beam evaporation system using a mask process, which not only increases the potential barrier to reduce dark current, but also alleviates the inherent hydrophobicity of the graphene film, so that the perovskite film can be smoothly deposited. The perovskite film is prepared by using MAPbI3 or FAPbI3 through a mature one-step deposition method and a two-step deposition method, respectively, and the stoichiometric ratio between PbI2 and MAI or PbI2 and FAI is regulated to obtain a perovskite film with good crystallinity, large grain size and compactness under X-ray diffraction and scanning electron microscopy characterization.
[0153] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A terahertz photoelectric detector, characterized in that: It comprises a substrate, and a graphene film layer, an aluminum oxide film layer and a perovskite film layer which are sequentially stacked on the substrate; A heterojunction is formed between the graphene film layer and the perovskite film layer; A metal electrode layer A is disposed on the surface of the graphene film layer, and the metal electrode layer A is disposed around the aluminum oxide film layer; A metal electrode layer B is disposed on the surface of the perovskite film layer.
2. The terahertz photodetector according to claim 1, characterized in that: The perovskite thin film layer is MAPbI3 or FAPbI3.
3. The terahertz photodetector according to claim 1, characterized in that: The substrate is a quartz substrate or a common glass substrate.
4. The terahertz photodetector according to claim 1, characterized in that: The metal electrode layer A is a silver electrode or a gold electrode.
5. The terahertz photodetector according to claim 1, characterized in that: The metal electrode layer B includes a plurality of metal electrode sheets, and the plurality of metal electrode sheets are evenly spaced and distributed along the width direction of the perovskite thin film layer.
6. The terahertz photodetector according to claim 5, characterized in that: The plurality of metal electrode sheets are all silver electrodes or gold electrodes.
7. A method for preparing a terahertz photodetector according to any one of claims 1 to 6, characterized in that: The following steps are involved: Using a wet transfer method, the graphene is transferred to the surface of the substrate to form a graphene film layer on the surface of the substrate, thereby obtaining a substrate having a graphene film layer on the surface; Using a mask method and electron beam evaporation treatment, an aluminum oxide film layer is formed on the surface of the graphene film layer; A one-step anti-solvent spin-on deposition method or a two-step co-deposition method is used to form a MAPbI3 perovskite film or a FAPbI3 perovskite film on the surface of the aluminum oxide film layer to form a perovskite film layer; By using a mask method and vacuum thermal evaporation treatment, a plurality of metal electrode layers A are deposited on the surface of the graphene film layer, and a plurality of metal electrode layers B are deposited on the surface of the perovskite film layer, so as to obtain the terahertz photodetector.
8. The preparation method according to claim 7, characterized in that: The graphene film layer is formed by the following steps: A graphene film is formed on the surface of a copper substrate by chemical vapor deposition, and then a layer of PMMA solution is spin-coated on the surface of the graphene film, and annealed to form a PMMA film on the surface of the graphene film, thereby obtaining a composite film material A having a copper / graphene / PMMA structure; Using ammonium persulfate solution as a removal solution, immersing the composite film material A in the ammonium persulfate solution to remove the copper substrate, thereby obtaining a composite film material B having a graphene / PMMA structure; After the composite film material B is fished out with a substrate and dried, the PMMA film in the composite film material B is removed with acetone to obtain a substrate having a graphene film layer on the surface.
9. The preparation method according to claim 8, characterized in that: The mass fraction of ammonium persulfate in the ammonium persulfate solution is 1.5% to 2.5%.
10. The preparation method according to claim 7, characterized in that: When an aluminum oxide film layer is formed on the surface of the graphene film layer, the process parameters of the electron beam evaporation treatment are: vacuum degree ≤ 3×10 -4 Pa, the evaporation rate is 2.5~3.5nm / s.
Citation Information
Cited By
Bipolar response photoelectric detector and preparation method thereof
CN119584705A
Bipolar response photoelectric detector and preparation method thereof
CN119584705B
Organic-inorganic hybrid perovskite thin film, preparation method and terahertz functional device
CN120736989A
Terahertz metamaterial integrated multi-bandwidth ultra-high-speed pyroelectric detector and preparation method thereof
CN121240755A