Thermoplastic resin composition
By adding crosslinked polyhydroxyalkanoate resin particles with high gel fraction to the thermoplastic resin, the problem of insufficient impact resistance of the thermoplastic resin is solved, and the mechanical strength is improved and the biodegradability is maintained.
Patent Information
- Application Number
- CN202380031901.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-27
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-22
AI Technical Summary
After improving the softness of existing thermoplastic resins, they have not yet effectively improved their impact resistance.
The impact strength and mechanical strength are improved by adding crosslinked polyhydroxyalkanoate resin particles with a gel fraction of more than 50% to the thermoplastic resin.
It significantly improves the impact strength and mechanical strength of the thermoplastic resin, while maintaining biodegradability. It is suitable for modifiers or impact resistance modifiers.
Smart Images

Figure BDA0005067113260000231 
Figure BDA0005067113260000232 
Figure BDA0005067113260000251
Abstract
Description
Technical Field
[0001] The present invention relates to thermoplastic resin compositions. Background Art
[0002] Plastic waste has become a burden on the global environment, affecting the ecosystem, generating harmful gases when burned, and causing global warming due to the large amount of heat from combustion. Biodegradable plastics are being actively developed as materials that can solve these problems.
[0003] Patent Document 1 describes a biodegradable thermoplastic resin composition having excellent environmental compatibility, wherein 0.1 to 20 parts by weight of poly(3-hydroxyalkanoate) particles having an average particle size of 300 μm or less are added to 100 parts by weight of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-161802 Summary of the invention
[0007] Problems to be solved by the invention
[0008] According to the technique described in Patent Document 1, in which poly(3-hydroxyalkanoate) particles are blended with a thermoplastic resin, the flexibility of the thermoplastic resin can be improved, but it does not contribute to the improvement of the impact resistance of the thermoplastic resin.
[0009] In view of the above-mentioned current situation, an object of the present invention is to provide a thermoplastic resin composition having improved mechanical strength such as impact strength.
[0010] Solution to the problem
[0011] The present inventors have conducted intensive studies and have found that mechanical strength such as impact strength can be improved by adding crosslinked resin particles composed of a polyhydroxyalkanoate resin and satisfying a specific gel fraction to a thermoplastic resin, thereby completing the present invention.
[0012] That is, the present invention relates to a thermoplastic resin composition comprising 40 to 90 parts by weight of a thermoplastic resin (A) and a polyhydroxyalkanoate resin, and 10 to 60 parts by weight of crosslinked resin particles (B) having a gel fraction of 50% or more [wherein the total amount of (A) and (B) is 100 parts by weight].
[0013] Furthermore, the present invention also relates to a molded product of the thermoplastic resin composition.
[0014] Furthermore, the present invention also relates to a thermoplastic resin modifier, which comprises a polyhydroxyalkanoate resin and crosslinked resin particles (B) having a gel fraction of 50% or more.
[0015] Effects of the Invention
[0016] According to the present invention, a thermoplastic resin composition having improved mechanical strength such as impact strength can be provided.
[0017] The thermoplastic resin composition of the present invention contains crosslinked resin particles composed of a polyhydroxyalkanoate resin and is therefore advantageous from the viewpoint of biodegradability.
[0018] The crosslinked resin particles can be used as a modifier or impact resistance improver for thermoplastic resins. DETAILED DESCRIPTION
[0019] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0020] The thermoplastic resin composition of this embodiment contains at least a thermoplastic resin (A) and crosslinked resin particles (B) containing a polyhydroxyalkanoate resin and having a gel fraction of 50% or more. The thermoplastic resin composition has improved impact strength of the thermoplastic resin (A) and can exhibit good impact resistance.
[0021] First, the crosslinked resin particles (B) will be described.
[0022] <Crosslinked resin particles (B)>
[0023] The crosslinked resin particles (B) are particles composed of a polyhydroxyalkanoate resin as a main resin component. Hereinafter, the polyhydroxyalkanoate resin may be abbreviated as "PHA".
[0024] <PHA>
[0025] "PHA" is a general term for polymers containing hydroxyalkanoic acid as a monomer unit, and is generally biodegradable. PHA is an aliphatic polyester, preferably a polyester without an aromatic ring.
[0026] PHA is not particularly limited, and examples thereof include polyglycolic acid, poly(3-hydroxyalkanoate) resins, poly(4-hydroxyalkanoate) resins, and the like. As PHA, only one type may be used, or two or more types may be used in combination. Among them, poly(3-hydroxyalkanoate) resins are preferred. Hereinafter, poly(3-hydroxyalkanoate) resins may be referred to as "P3HA".
[0027] The above P3HA has the chemical formula: [-CHR-CH 2-CO-O-] represented by a 3-hydroxyalkanoic acid repeating unit (wherein R is C n H 2n+1 The P3HA preferably contains 50 mol % or more of the 3-hydroxyalkanoic acid repeating unit in all monomer repeating units (100 mol %), and more preferably contains 70 mol % or more.
[0028] P3HA is not particularly limited, and examples thereof include poly(3-hydroxybutyrate) (abbreviated as P3HB), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviated as P3HB3HH), etc. As P3HA, only one type may be used, or two or more types may be used in combination.
[0029] P3HA can be produced by microorganisms. Such microbial production of P3HA is usually composed of only D-form (R-form) hydroxyalkanoic acid repeating units. Among the microbial production of P3HA, P3HB and P3HB3HH are preferred from the viewpoint of easy industrial production, and P3HB3HH is more preferred.
[0030] In the case where P3HA contains 3-hydroxybutyric acid (3HB) repeating units, from the viewpoint of the balance between flexibility and strength, the composition ratio of 3HB repeating units in all monomer repeating units (100 mol%) is preferably 60 to 99 mol%, more preferably 65 to 97 mol%, and further preferably 67 to 95 mol%. By making the composition ratio of 3HB repeating units 60 mol% or more, the handling of cross-linked resin particles (B) becomes easy. On the other hand, by making the composition ratio of 3HB repeating units 99 mol% or less, there is a tendency to easily ensure the flexibility of cross-linked resin particles (B). It should be noted that the monomer composition ratio of P3HA can be measured by gas chromatography, etc. (for example, refer to International Publication No. 2014 / 020838). As P3HA, two or more compositions having different composition ratios of 3HB repeating units can be used in combination.
[0031] As a microorganism producing P3HA, it is not particularly limited as long as it is a microorganism with the ability to produce P3HA. For example, as a P3HB producing bacterium, the earliest one was Bacillus megaterium discovered in 1925. Other examples include natural microorganisms such as Cupriavidus necator (old classification: Alcaligenes eutrophus, Ralstonia eutropha), and Alcaligenes latus. Among these microorganisms, it is known that P3HB accumulates in the bacteria.
[0032] In addition, as a producer of copolymers of 3HB and other hydroxyalkanoates, Aeromonas caviae, which is a P3HB3HH producer, is known. In particular, in order to improve the productivity of P3HB3HH, preferably Alcaligenes eutrophus AC32 strain (Alcaligenes eutrophus AC32, FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, p4821-4830 (1997)) into which the genes of the P3HA synthase group are introduced is used. Microbial cells in which these microorganisms are cultured under appropriate conditions to accumulate P3HA in the cell body can be used. In addition, in addition to the above, genetically recombinant microorganisms into which various P3HA synthesis-related genes are introduced according to the P3HA to be produced can be used, and the culture conditions including the type of substrate can also be optimized.
[0033] The molecular weight of PHA is not particularly limited, and the weight average molecular weight is preferably 50,000 to 3,000,000, preferably 100,000 to 2,000,000, and more preferably 150,000 to 1,500,000. By making the weight average molecular weight above 50,000, the tendency of the strength of the cross-linked resin particles to decrease can be avoided, or the tendency of stickiness due to low molecular weight components can be avoided. On the other hand, PHA having a weight average molecular weight exceeding 3,000,000 is sometimes difficult to prepare itself or difficult to handle for the purpose of the present invention. The numerical value of the weight average molecular weight is a value measured before the cross-linking treatment of PHA is performed.
[0034] In the method for measuring the weight average molecular weight, gel permeation chromatography (GPC) ("High Performance Liquid Chromatography 20A System" manufactured by Shimadzu Corporation) can be used, and a polystyrene gel ("KG 4A" and "K-806M" manufactured by Showa Denko K.K., etc.) is used as a column, and chloroform is used as a mobile phase to obtain the molecular weight in terms of polystyrene. In this case, a calibration curve can be prepared using polystyrene with weight average molecular weights of 31400, 197000, 668000, and 1920000. As a column in the GPC, a column suitable for measuring the above molecular weight can be used.
[0035] <Gel fraction>
[0036] The cross-linked resin particles (B) have a cross-linked structure formed by bonding molecular chains of PHA. Since the cross-linked structure has a certain amount or more, the cross-linked resin particles (B) have a high gel fraction, specifically, a gel fraction of 50% or more. By showing such a high gel fraction, the effect of improving the mechanical strength of the thermoplastic resin (A), such as the impact strength, can be improved.
[0037] From the viewpoint of improving impact strength, the gel fraction is preferably 60% or more, more preferably 70% or more, further preferably 75% or more, and particularly preferably 80% or more. Alternatively, it may be 85% or more, or 90% or more. The upper limit of the gel fraction is not particularly limited, as long as it is 100% or less. From the viewpoint of production efficiency of the cross-linked resin particles (B) and improvement of impact strength, it is preferably 99.5% or less, more preferably 99% or less. Alternatively, it may be 98% or less, or 97% or less, or 96% or less.
[0038] The gel fraction is a value measured as follows. The dried product of the cross-linked resin particles (B) is added to chloroform at a concentration of 0.7% by weight and dissolved at 60°C for 30 minutes to obtain a chloroform solution. Then, after standing at room temperature for 3 hours, the chloroform solution is filtered using a membrane filter with a pore size of 0.45 μm. The gel remaining on the filter is dried, and the weight is measured together with the filter, and the gel fraction is calculated by the following formula.
[0039] Formula: Gel fraction = (weight of the filter including the dried gel - weight of the filter alone) / weight of the cross-linked resin particles used in the measurement × 100 (%)
[0040] <Average particle size>
[0041] The volume average particle size of the cross-linked resin particles (B) is preferably within the range of 0.1 μm or more and 10 μm or less. By having such a particle size, the mechanical strength such as the impact strength of the thermoplastic resin (A) can be further improved. From the perspective of practical use opportunities, the lower limit of the above-mentioned particle size is preferably 0.1 μm or more, more preferably 0.3 μm or more, and further preferably 0.5 μm or more. In addition, from the perspective of productivity (production of PHA, cross-linking treatment, etc.), the upper limit of the above-mentioned particle size is preferably 8 μm or less, more preferably 5 μm or less. Among them, by melt-kneading the cross-linked resin particles (B) and the thermoplastic resin (A), the original shape of the cross-linked resin particles (B) is sometimes destroyed and the volume average particle size is reduced.
[0042] The volume average particle size is a value measured in a state where the crosslinked resin particles (B) are dispersed in an aqueous solvent. As a measuring device, a general-purpose measuring device can be used, and an example of such a device is Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd.
[0043] <Peroxide>
[0044] The crosslinking form in the crosslinked resin particles (B) of this embodiment is not particularly limited, and crosslinking using peroxide is preferred. When peroxide is used, free radicals generated by decomposition of the peroxide act on PHA molecules, and molecular chains of PHA are directly bonded to each other, thereby forming the above-mentioned crosslinked structure.
[0045] The peroxide may be an organic peroxide or an inorganic peroxide. In order to more efficiently increase the gel fraction, an organic peroxide is preferred.
[0046] The organic peroxide is preferably at least one selected from diacyl peroxides, alkyl peroxides, dialkyl peroxides, hydroperoxides, peroxyketals, peroxycarbonates and peroxydicarbonates in consideration of heating temperature and time during crosslinking treatment.
[0047] Specific examples of such organic peroxides include butyl peroxyneododecanoate, octanoyl peroxide, dilauroyl peroxide, succinyl peroxide, a mixture of methylbenzoyl peroxide and benzoyl peroxide, benzoyl peroxide, bis(butylperoxy)trimethylcyclohexane, butyl peroxylaurate, dimethyldi(benzoylperoxy)hexane, bis(butylperoxy)methylcyclohexane, bis(butylperoxy)cyclohexane, butyl peroxybenzoate, butyl peroxyvalerate, diisopropylbenzene peroxide, di-tert-hexyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-butyl peroxymethylmonocarbonate. , tert-amyl peroxymethyl monocarbonate, tert-hexyl peroxymethyl monocarbonate, tert-heptyl peroxymethyl monocarbonate, tert-octyl peroxymethyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxymethyl monocarbonate, tert-butyl peroxyethyl monocarbonate, tert-amyl peroxyethyl monocarbonate, tert-hexyl peroxyethyl monocarbonate, tert-heptyl peroxyethyl monocarbonate, tert-octyl peroxyethyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxyethyl monocarbonate, tert-butyl peroxy-n-propyl monocarbonate, tert-amyl peroxy-n-propyl monocarbonate, tert-hexyl peroxy-n-propyl monocarbonate, tert-heptyl peroxy-n-propyl monocarbonate, tert-octyl peroxy-n-propyl monocarbonate, 1,1 ,3,3-Tetramethylbutyl peroxyn-propyl monocarbonate, tert-butyl peroxyisopropyl monocarbonate, tert-amyl peroxyisopropyl monocarbonate, tert-hexyl peroxyisopropyl monocarbonate, tert-heptyl peroxyisopropyl monocarbonate, tert-octyl peroxyisopropyl monocarbonate, 1,1,3,3-Tetramethylbutyl peroxyisopropyl monocarbonate, tert-butyl peroxyn-butyl monocarbonate, tert-amyl peroxyn-butyl monocarbonate, tert-hexyl peroxyn-butyl monocarbonate, tert-heptyl peroxyn-butyl monocarbonate, tert-octyl peroxyn-butyl monocarbonate, 1,1,3,3-Tetramethylbutyl peroxyn-butyl monocarbonate, tert-butyl peroxyisobutyl monocarbonate, tert-amyl peroxyisobutyl monocarbonate , tert-hexyl peroxyisobutyl monocarbonate, tert-heptyl peroxyisobutyl monocarbonate, tert-octyl peroxyisobutyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxyisobutyl monocarbonate, tert-butyl peroxysec-butyl monocarbonate, tert-amyl peroxysec-butyl monocarbonate, tert-hexyl peroxysec-butyl monocarbonate, tert-heptyl peroxysec-butyl monocarbonate, tert-octyl peroxysec-butyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxysec-butyl monocarbonate, tert-butyl peroxytert-butyl monocarbonate, tert-amyl peroxytert-butyl monocarbonate, tert-hexyl peroxytert-butyl monocarbonate, tert-heptyl peroxytert-butyl monocarbonate, tert-octyl peroxytert-butyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxysec-butyl monocarbonate,3-Tetramethylbutyl peroxy tert-butyl monocarbonate, tert-butyl peroxy 2-ethylhexyl monocarbonate, tert-amyl peroxy 2-ethylhexyl monocarbonate, tert-hexyl peroxy 2-ethylhexyl monocarbonate, tert-heptyl peroxy 2-ethylhexyl monocarbonate, tert-octyl peroxy 2-ethylhexyl monocarbonate, 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexyl monocarbonate, diisobutyl peroxide, isopropyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, bis(2-ethylhexyl) peroxydicarbonate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-butyl peroxyneoheptanoate, tert-hexyl peroxypivalate, peroxy tert-Butyl pivalate, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-bis(2-ethylhexanoyl peroxide)hexane, tert-hexyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisopropyl carbonate, 1,6-bis(tert-butylperoxycarbonyloxy)hexane, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxyacetate, tert-butyl peroxybenzoate, tert-amyl peroxy-3,5,5-trimethylhexanoate, 2,2-bis(4,4-di-tert-butylperoxycyclohexyl)propane, 2,2-di-tert-butylperoxybutane, etc. The organic peroxide may be used alone or in combination of two or more.
[0048] Among them, tert-butyl peroxyisopropyl monocarbonate, tert-amyl peroxyisopropyl monocarbonate, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, tert-amyl peroxy-2-ethylhexyl monocarbonate, tert-hexyl peroxy-2-ethylhexyl monocarbonate, tert-amyl peroxyisopropyl monocarbonate, di-tert-hexyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-hexyl peroxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-butyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, and 1,1,3,3-tetramethylbutyl peroxyneodecanoate are preferred organic peroxides because they can efficiently crosslink PHA.
[0049] The peroxide can set the heating temperature during the crosslinking treatment to a low level, and therefore, the peroxide preferably has a one-hour half-life temperature of 200°C or lower, more preferably 170°C or lower, and further preferably 140°C or lower. The lower limit may be 50°C or higher, 60°C or higher, or 70°C or higher.
[0050] Particularly preferred organic peroxides showing such a one-hour half-life temperature are tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy 2-ethylhexyl monocarbonate, di-sec-butyl peroxydicarbonate, tert-butyl peroxy 2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-hexyl peroxy 2-ethylhexanoate, 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-butyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, and 1,1,3,3-tetramethylbutyl peroxyneodecanoate.
[0051] When the above-mentioned peroxide is an inorganic peroxide, as the inorganic peroxide, considering the heating temperature and time during the crosslinking treatment, for example, hydrogen peroxide, potassium peroxide, calcium peroxide, sodium peroxide, magnesium peroxide, potassium persulfate, sodium persulfate, ammonium persulfate, etc. can be listed. Among them, from the viewpoint of the decomposition temperature of the heating temperature during the ease of operation and the heating temperature suitable for the crosslinking treatment, hydrogen peroxide, potassium persulfate, sodium persulfate and ammonium persulfate are preferably used. One inorganic peroxide can be used alone, or two or more can be used in combination. In addition, organic peroxide and inorganic peroxide can also be used in combination.
[0052] <Multifunctional compounds>
[0053] The crosslinked structure in the crosslinked resin particles (B) may be introduced using only a peroxide or using both a peroxide and a polyfunctional compound. The latter can increase the gel fraction of the crosslinked resin particles (B) with a small amount of peroxide.
[0054] The above-mentioned multifunctional compound refers to a compound having two or more functional groups capable of crosslinking PHA in one molecule. Although not particularly limited, it is preferably a compound reactive with free radicals generated by peroxides, and particularly preferably a compound having two or more free radical reactive groups in one molecule. The free radical reactive group is preferably at least one selected from vinyl, allyl, acryloyl, or methacryloyl.
[0055] Such a multifunctional compound is not particularly limited, and examples thereof include: allyl (meth)acrylate; allyl alkyl (meth)acrylates; allyloxyalkyl (meth)acrylates; multifunctional (meth)acrylates having two or more (meth)acrylate groups, such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and pentaerythritol (meth)acrylate; divinylbenzene, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. Allyl methacrylate, triallyl isocyanurate, butanediol di(meth)acrylate, and divinylbenzene are preferred, and allyl methacrylate and triallyl isocyanurate are particularly preferred.
[0056] When a crosslinked structure is formed in the presence of a polyfunctional compound, the obtained crosslinked resin particles (B) may generally contain a structure derived from the polyfunctional compound. In this case, molecular chains of PHA are bonded to each other via the structure derived from the polyfunctional compound.
[0057] The crosslinked resin particles (B) may be composed only of PHA having a crosslinked structure, or may further contain components other than PHA having a crosslinked structure. Components other than PHA having a crosslinked structure include, for example, resins other than PHA, antioxidants, hydrolysis inhibitors, anti-blocking agents, crystal nucleating agents, ultraviolet absorbers, etc.
[0058] The proportion of PHA in the crosslinked resin particles (B) is not particularly limited, and may be 50% by weight or more, preferably 70% by weight or more, more preferably 80% by weight or more, further preferably 90% by weight or more, and particularly preferably 95% by weight or more. It may be 99% by weight or more. The upper limit is not particularly limited, and may be 100% by weight or less.
[0059] As resins other than PHA, for example, aliphatic polyesters formed by polycondensation of aliphatic diols and aliphatic dicarboxylic acids, aliphatic aromatic polyesters using both aliphatic compounds and aromatic compounds as monomers, etc. Examples of the former include polyethylene succinate, polybutylene succinate (PBS), polyhexamethylene succinate, polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, polybutylene succinate adipate (PBSA), polyethylene sebacate, polybutylene sebacate, etc. Examples of the latter include poly(butylene adipate-co-butylene terephthalate) (PBAT), poly(butylene sebacate-co-butylene terephthalate), poly(butylene azelaate-co-butylene terephthalate), poly(butylene succinate-co-butylene terephthalate) (PBST), etc. The other resins may be used alone or in combination of two or more.
[0060] It is preferred that the cross-linked resin particles (B) are unfoamed, that is, substantially do not contain bubbles inside the particles, unlike the foamed resin particles disclosed in International Publication Nos. 2007 / 049694 and 2019 / 146555.
[0061] In the case of non-foaming, the apparent density of the crosslinked resin particles (B) shows a large value, preferably greater than 0.6 g / cm 3 , more preferably 0.7 g / cm 3 More preferably, 0.9 g / cm 3 The apparent density of the crosslinked resin particles (B) can be determined by the method described in JIS K0061 (method for measuring density and specific gravity of chemical products) or JIS Z8807 (method for measuring density and specific gravity of solids).
[0062] The average weight per particle of the crosslinked resin particles (B) is not particularly limited, but is a value much lower than 0.1 mg because the volume average particle size of the crosslinked resin particles (B) is as small as 10 μm or less.
[0063] The crosslinked resin particles (B) may be dried. The shape after drying may be powdery, granular, crumbly, flake, or the like, depending on the drying method.
[0064] <Method for producing crosslinked resin particles (B)>
[0065] An example of a method for producing crosslinked resin particles (B) is specifically described. Crosslinked resin particles (B) can be produced by crosslinking PHA in an aqueous dispersion containing PHA particles before crosslinking treatment in the presence of a peroxide. In order to efficiently crosslink PHA, the aqueous dispersion of PHA particles containing peroxide is preferably heated to a temperature suitable for the decomposition of the peroxide.
[0066] More specifically, the method for producing the crosslinked resin particles (B) preferably comprises a step (1) of preparing an aqueous dispersion of PHA particles in which PHA particles before crosslinking treatment are dispersed in water, a step (2) of adding a peroxide to the aqueous dispersion of PHA particles so that the peroxide is impregnated into the PHA particles, and a step (3) of heating the aqueous dispersion of PHA particles impregnated with the peroxide to a heating temperature to crosslink the PHA. More preferably, it further comprises a step (4) of maintaining the heating temperature after all the peroxide has been added.
[0067] In step (1), the aqueous dispersion of PHA particles may be an aqueous dispersion obtained by culturing PHA-producing microorganisms to accumulate PHA in the microorganisms, destroying the microorganisms in the culture solution, and separating and removing the microorganism components, or an aqueous dispersion obtained by concentrating or diluting the aqueous dispersion. According to such a method, the process can be carried out without separating the PHA particles from water during the period from the production of PHA particles to the crosslinking treatment in the culture of PHA-producing microorganisms.
[0068] Alternatively, the aqueous dispersion of PHA particles may be prepared by dispersing dried PHA particles in water. The aqueous dispersion may contain an organic solvent compatible with water in addition to water.
[0069] In the aqueous dispersion, the volume average particle size of the PHA particles is preferably within the same range as the volume average particle size of the cross-linked resin particles (B). In the case of PHA particles produced by a PHA-producing microorganism, the volume average particle size thereof can generally be within the above range, and therefore, an aqueous dispersion of PHA particles having a desired volume average particle size can be obtained without performing a special step for adjusting the particle size.
[0070] The concentration of the PHA particles in the aqueous dispersion is not particularly limited and can be appropriately set, and may be, for example, about 1 to 70% by weight, preferably about 5 to 50% by weight.
[0071] In order to improve the dispersibility of PHA particles and make the cross-linking reaction proceed uniformly, it is preferred that the aqueous dispersion of PHA particles contains a dispersant. As a dispersant, for example, anionic surfactants such as sodium sulfosuccinate dioctyl ester, sodium lauryl sulfate, sodium lauryl sulfate, sodium oleate, etc.; cationic surfactants such as dodecyl trimethylammonium chloride; nonionic surfactants such as glycerol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene polyoxypropylene glycols; polyvinyl alcohol, ethylene-modified polyvinyl alcohol, polyvinyl pyrrolidone, methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, sodium polyacrylate, potassium polyacrylate, polymethacrylic acid, sodium polymethacrylate, etc. Water-soluble polymers, etc., can be used. These dispersants can be used alone or in combination of two or more.
[0072] When a dispersant is used, the amount thereof added is not particularly limited, and may be, for example, 0.1 to 10 parts by weight, preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the PHA particles.
[0073] In step (2), peroxide is added to the aqueous dispersion of PHA particles obtained in step (1) to impregnate the PHA particles with the peroxide. As the peroxide, the above-mentioned peroxides can be used. The peroxide can be added in various forms such as solid and liquid. In addition, liquid peroxide diluted with a diluent or the like can also be added. The peroxide can be added all at once, or can be added continuously or in divided portions.
[0074] When a peroxide and the above-mentioned multifunctional compound are used in combination, in the step (2), the multifunctional compound is preferably also added to the aqueous dispersion of the PHA particles. As the multifunctional compound, the above-mentioned multifunctional compound can be used. The multifunctional compound can be added in various forms such as solid and liquid. In addition, a liquid multifunctional compound diluted with a diluent or the like can also be added. The multifunctional compound can be added all at once, or can be added continuously or in divided portions.
[0075] In order to impregnate the PHA particles with the peroxide and any polyfunctional compound, the water dispersion may be stirred after adding these compounds to the water dispersion of the PHA particles or while adding them, with the water dispersion temperature set to, for example, 0° C. or higher and lower than a temperature suitable for decomposition of the peroxide used in the next step (3), and the temperature may be maintained for, for example, about 1 minute to 5 hours. Specifically, the temperature of the water dispersion during impregnation may be about 10 to 60° C.
[0076] The amount of peroxide used can be appropriately set in consideration of the gel fraction of the cross-linked resin particles (B), and is, for example, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 8 parts by weight, further preferably 0.3 to 5 parts by weight, and particularly preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the PHA particles.
[0077] According to the production method of crosslinking PHA particles in an aqueous dispersion using a peroxide, crosslinking is performed while maintaining the particle size (volume) before crosslinking, and crosslinked resin particles are easily obtained. On the other hand, the method of crosslinking the resin by melt kneading in the presence of a peroxide is sometimes difficult to achieve.
[0078] In addition, according to the production method of crosslinking PHA particles in an aqueous dispersion using a peroxide, it is easy to control the temperature rise caused by the heat generated in the crosslinking reaction, which is advantageous in obtaining crosslinked resin particles having a stable crosslinked structure (quality) safely and efficiently.
[0079] The amount of the polyfunctional compound used can also be appropriately set in consideration of the gel fraction of the cross-linked resin particles (B). For example, it is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 15 parts by weight, further preferably 0.1 to 10 parts by weight, further preferably 0.2 to 5 parts by weight, and particularly preferably 0.3 to 3 parts by weight, relative to 100 parts by weight of the PHA particles.
[0080] In step (3), the aqueous dispersion of PHA particles impregnated with peroxide is heated to a temperature suitable for the decomposition of the peroxide. The heating temperature is preferably within a range of about 25°C based on the 1-hour half-life temperature of the peroxide described above. Specifically, the heating temperature is preferably 30 to 140°C, more preferably 50 to 135°C, and even more preferably 60 to 130°C. According to the present method, PHA can be crosslinked at a temperature lower than the melting temperature of PHA, so that the deterioration of PHA caused by heating during the crosslinking treatment can be avoided.
[0081] Next, in step (4), the heating temperature is preferably maintained. This allows the crosslinking reaction using the peroxide to proceed sufficiently. The time for maintaining the heating temperature is not particularly limited, but is preferably 1 minute to 15 hours, more preferably 1 hour to 10 hours.
[0082] After the cross-linking reaction is completed, the cross-linked resin particles (B) are separated from the aqueous dispersion and water is removed, thereby obtaining dried cross-linked resin particles (B). The method for separating the cross-linked resin particles (B) is not particularly limited, and for example, filtration, centrifugal separation, heat drying, freeze drying, spray drying, etc. can be used. For example, when spray drying is used, the dried cross-linked resin particles (B) can be obtained directly from the aqueous dispersion. In addition, by extruding the cross-linked resin particles (B) separately after separation from the aqueous dispersion, the cross-linked resin particles (B) can also be obtained in a granular shape while completely removing the residual water. In addition, a coagulation process using a coagulant and pH adjustment can also be implemented.
[0083] In the thermoplastic resin composition of the present embodiment, the amount of the cross-linked resin particles (B) is 10 to 60 parts by weight relative to 100 parts by weight of the total of the thermoplastic resin (A) and the cross-linked resin particles (B). When the cross-linked resin particles (B) are used in the above range, the mechanical strength such as the impact strength of the thermoplastic resin (A) can be improved. The above amount can be 15 parts by weight or more, 20 parts by weight or more, or 25 parts by weight or more. In addition, the upper limit of the above amount is preferably 55 parts by weight or less, more preferably 50 parts by weight or less, and particularly preferably 45 parts by weight or less.
[0084] <Thermoplastic resin (A)>
[0085] In the thermoplastic resin composition of the present embodiment, the thermoplastic resin (A) as the matrix resin is not particularly limited as long as it can be melted by heating and then cooled and solidified to be molded into a desired shape. Specifically, polyolefin resins such as polyethylene and polypropylene, acrylic resins such as polyvinyl chloride, polystyrene, polyvinyl acetate, polyurethane, polytetrafluoroethylene, and polymethyl methacrylate, AS resin, polyamide, polyacetal, polycarbonate, modified polyphenylene ether, polyester resin, cyclic polyolefin, etc. can be mentioned. These thermoplastic resins can be used alone or in combination of two or more.
[0086] As the thermoplastic resin (A), a polyester resin is particularly preferred. Examples of the polyester resin include PHAs such as polyglycolic acid, poly(3-hydroxyalkanoate) resins, and poly(4-hydroxyalkanoate) resins; polylactic acid; aliphatic polyesters such as polyesters formed by polycondensation of aliphatic diols and aliphatic dicarboxylic acids; and aliphatic aromatic polyesters using both aliphatic compounds and aromatic compounds as monomers. Examples of aliphatic polyesters other than PHA include polycaprolactone, polyethylene succinate, polybutylene succinate (PBS), polyhexanediol succinate, polyethylene adipate, polybutylene adipate, polyhexanediol adipate, polybutylene succinate adipate (PBSA), polyethylene sebacate, and polybutylene sebacate. Examples of aliphatic aromatic polyesters include poly(butylene adipate-co-butylene terephthalate) (PBAT), poly(butylene sebacate-co-butylene terephthalate), poly(butylene azelate-co-butylene terephthalate), poly(butylene succinate-co-butylene terephthalate) (PBST), polyethylene furandicarboxylate, etc. These polyester resins may be used alone or in combination of two or more.
[0087] Since the crosslinked resin particles (B) are composed of biodegradable PHA, the thermoplastic resin (A) preferably also contains a biodegradable resin. In this case, the biodegradability of the thermoplastic resin composition as a whole can be improved.
[0088] Furthermore, when the crosslinked resin particles (B) are produced from a plant-derived raw material, the thermoplastic resin (A) is also preferably a resin produced from a plant-derived raw material from the viewpoint of resource recycling.
[0089] When the thermoplastic resin (A) contains a biodegradable resin, the content ratio thereof is preferably 10 to 100% by weight, more preferably 30% by weight or more, further preferably 50% by weight or more, further preferably 70% by weight or more, and particularly preferably 90% by weight or more in the entire thermoplastic resin (A).
[0090] The biodegradable resin used as the thermoplastic resin (A) has an excellent effect of improving the impact resistance due to the crosslinked resin particles (B), so it is preferred to contain the above-mentioned aliphatic polyester, and particularly preferably contain PHA and / or polylactic acid. It should be noted that the PHA used as the thermoplastic resin (A) preferably does not have a crosslinked structure.
[0091] When the thermoplastic resin (A) contains PHA and / or polylactic acid, the content ratio thereof is preferably 10 to 100 wt %, more preferably 30 wt % or more, further preferably 50 wt % or more, further preferably 70 wt % or more, and particularly preferably 90 wt % or more in the entire thermoplastic resin (A).
[0092] The PHA that can be used as the thermoplastic resin (A) is not particularly limited, and examples thereof include polyglycolic acid, P3HA, and poly(4-hydroxyalkanoate) resins. As PHA, only one type may be used, or two or more types may be used in combination. Among them, P3HA is particularly preferred.
[0093] The P3HA that can be used as the thermoplastic resin (A) can be the same as the P3HA related to the cross-linked resin particles (B), and the various P3HAs mentioned above can be used. It is preferred that the P3HA used as the thermoplastic resin (A) is different from the P3HA used for the cross-linked resin particles (B), and more preferably a resin harder than the P3HA used for the cross-linked resin particles (B).
[0094] When P3HA used as a thermoplastic resin (A) contains 3-hydroxybutyric acid (3HB) repeating units, the composition ratio of 3HB repeating units in all monomer repeating units (100 mol%) is preferably 80 to 99 mol%, more preferably 82 to 97 mol%, from the viewpoint of the balance between flexibility and strength. By making the composition ratio of 3HB repeating units 80 mol% or more, the rigidity of P3HA can be further improved. On the other hand, by making the composition ratio of 3HB repeating units 99 mol% or less, there is a tendency that the flexibility of P3HA is further improved. As P3HA, two or more types having different composition ratios of 3HB repeating units can be used in combination.
[0095] The molecular weight of the PHA used as the thermoplastic resin (A) is not particularly limited, and the weight average molecular weight is preferably 50,000 to 3,000,000, preferably 100,000 to 2,000,000, and more preferably 150,000 to 1,500,000. By setting the weight average molecular weight to be 50,000 or more, sufficient rigidity and strength can be obtained for the thermoplastic resin composition of the present embodiment. On the other hand, for PHA having a weight average molecular weight exceeding 3,000,000, it is sometimes difficult to produce itself or difficult to handle to achieve the purpose of the present invention.
[0096] As the polylactic acid that can be used as the thermoplastic resin (A), conventionally known polylactic acids can be used, and the polylactic acid may be crystalline or amorphous.
[0097] The polylactic acid may be a homopolymer of lactic acid, or a copolymer of lactic acid and other monomers, or a blend thereof.
[0098] Examples of the other monomers include aliphatic hydroxycarboxylic acids other than lactic acid, aliphatic polyols, aliphatic polycarboxylic acids, and polyfunctional polysaccharides.
[0099] The lactic acid raw material for producing polylactic acid is not particularly limited, and L-lactic acid, D-lactic acid, DL-lactic acid, or a mixture thereof, L-lactide, D-lactide, meso-lactide, or a mixture thereof, etc. can be used. Lactic acid obtained by microbial fermentation of renewable raw materials derived from plants such as starch can be suitably used.
[0100] As a method for producing polylactic acid, a known method such as a dehydration polycondensation method and a ring-opening polymerization method can be applied without particular limitation.
[0101] The molecular weight of the polylactic acid (A) used as the thermoplastic resin (A) is not particularly limited, and the weight average molecular weight is preferably 50,000 to 1,000,000, preferably 70,000 to 700,000, and more preferably 100,000 to 400,000. By setting the weight average molecular weight to 50,000 or more, sufficient rigidity and strength can be obtained for the thermoplastic resin composition of the present embodiment. On the other hand, for polylactic acid having a weight average molecular weight exceeding 1,000,000, it is sometimes difficult to make itself, or difficult to operate to achieve the purpose of the present invention.
[0102] <Crystallization nucleating agent>
[0103] The thermoplastic resin composition may further contain a crystal nucleating agent. When the thermoplastic resin (A) is a crystalline resin, the crystallization during molding can be promoted by making the thermoplastic resin composition contain a crystal nucleating agent, thereby improving molding processability, productivity, etc. In addition, a thermoplastic resin composition having excellent heat resistance or mechanical properties can be obtained.
[0104] The above-mentioned crystal nucleating agent is not particularly limited, and a known crystal nucleating agent can be used, for example: talc, kaolinite, montmorillonite, mica, synthetic mica, clay, zeolite, silica, carbon black, graphite, boron nitride, zinc oxide, titanium oxide, tin oxide, calcium carbonate, magnesium carbonate, aluminum oxide, neodymium oxide, barium sulfate, sodium chloride, metal phosphate and other inorganic substances; erythritol, pentaerythritol, galactitol, mannitol, arabitol and other natural sugar alcohol compounds; chitin, chitosan and other polysaccharides; aliphatic alcohols (polyols), polyvinyl alcohol, polyethylene oxide and other polyols; sodium benzoate, benzyl alcohol, benzoic acid ... Potassium benzoate, lithium benzoate, calcium benzoate, magnesium benzoate, barium benzoate, lithium terephthalate, sodium terephthalate, potassium terephthalate, calcium oxalate, sodium laurate, potassium laurate, sodium myristate, potassium myristate, calcium myristate, sodium octadecanoate, calcium octadecanoate, sodium stearate, potassium stearate, lithium stearate, calcium stearate, magnesium stearate, barium stearate, sodium montanate, calcium montanate, sodium phenylacetate, sodium salicylate, potassium salicylate, zinc salicylate, aluminum dibenzoate, potassium dibenzoate, lithium dibenzoate, sodium β-naphthalate, sodium cyclohexanecarboxylate and other organic carboxylic acid metal salts, sodium p-toluenesulfonate, sodium sulfoisophthalic acid and other organic sulfonates, ethylenebisstearic acid amide, ethylenebislauric acid amide, palmitic acid amide, hydroxystearic acid amide, erucic acid amide, trimesic acid tri(tert-butylamide) and other carboxylic acid amides, laurate, palmitic acid, oleic acid, stearic acid, erucic acid, N-oleyl palmitate, N-oleyl oleate, N-oleyl stearic acid, N-stearyl oleate, N-stearyl stearic acid, N-stearyl erucic acid, methylene distearate, ethylene dilaurate, ethylene dicaprate, ethylene dioleate, ethylene distearate, ethylene dierucic acid, ethylene diisostearate, butylene diisostearate Carboxylates such as stearic acid esters and p-xylylene distearate; dicarboxylic acid derivatives such as dimethyl adipate, dibutyl adipate, diisodecyl adipate, and dibutyl sebacate; cyclic compounds having a functional group C=O and a functional group selected from NH, S, and O in the molecule such as indigo, quinacridone, and quinacridone fuchsin; sorbitol derivatives such as bisbenzylidene sorbitol and bis(p-methylbenzylidene) sorbitol; compounds containing nitrogen-containing heteroaromatic nuclei such as pyridine, triazine, and imidazole; phosphate compounds, bisamides of higher fatty acids, and metal salts of higher fatty acids; branched polylactic acid; low molecular weight poly 3-hydroxybutyrate, etc. These crystal nucleating agents can be used alone or in combination of two or more.
[0105] The content of the crystal nucleating agent is not particularly limited as long as it can promote the crystallization of the thermoplastic resin (A), and is preferably 0.05 to 12 parts by weight, more preferably 0.1 to 10 parts by weight, and further preferably 0.5 to 8 parts by weight relative to 100 parts by weight of the thermoplastic resin (A). When the content of the crystal nucleating agent is within the above range, the viscosity during molding and the decrease in the physical properties of the molded product can be suppressed, and the effect as a crystal nucleating agent can be obtained.
[0106] <Lubricant>
[0107] The thermoplastic resin composition may further contain a lubricant. By containing a lubricant, the surface smoothness of the obtained molded body can be improved. As the lubricant, there is no particular limitation, and examples thereof include: fatty acid metal salts such as magnesium stearate and calcium stearate, fatty acid amides such as behenic acid amide, stearic acid amide, erucic acid amide, oleic acid amide, methylene bis stearic acid amide, and ethylene bis stearic acid amide; polyethylene wax, oxidized polyester wax, glycerol monostearate, glycerol monobehenate, glycerol monolaurate, and other glycerol monofatty acid esters; organic acid monoglycerides such as succinic acid saturated fatty acid monoglyceride; sorbitan fatty acid esters such as sorbitan behenate, sorbitan stearate, and sorbitan laurate; polyglycerol fatty acid esters such as diglycerol stearate, diglycerol laurate, tetraglycerol stearate, tetraglycerol laurate, decaglycerol stearate, and decaglycerol laurate; higher alcohol fatty acid esters such as stearyl stearate, etc., but are not limited thereto. The lubricants may be used alone or in combination of two or more.
[0108] The content of the lubricant (the total content when using a plurality of lubricants) is not particularly limited as long as it can impart lubricity to the molded article, but is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 10 parts by weight, further preferably 0.1 to 10 parts by weight, further preferably 0.2 to 5 parts by weight, and particularly preferably 0.3 to 4 parts by weight, relative to 100 parts by weight of the thermoplastic resin (A). When the content of the lubricant is within the above range, leakage of the lubricant to the surface of the molded article can be avoided, and the effect as a lubricant can be obtained.
[0109] <Other ingredients>
[0110] The thermoplastic resin composition of the present embodiment may contain other components such as a plasticizer, an organic filler, an inorganic filler, an antioxidant, a hydrolysis inhibitor, a UV absorber, a colorant such as a dye or a pigment, and an antistatic agent within a range that does not impair the function of the obtained molded article.
[0111] The plasticizer is not particularly limited, and examples thereof include polyester plasticizers such as polypropylene glycol sebacate; aliphatic dibasic acid ester plasticizers such as di-1-butyl adipate, di-n-butyl sebacate, and di-2-ethylhexyl azelate; glycerol plasticizers such as diacetyl monolaurate, diacetyl monocaprylate, and diacetyl monocaprate; polycarboxylic acid ester plasticizers such as tri-2-ethylhexyl acetyl citrate and tributyl acetyl citrate; polyethylene glycol, polyol ... Polyalkylene glycol plasticizers such as propylene glycol, poly(ethylene oxide / propylene oxide) block and / or random copolymers, and polytetramethylene glycol; phosphate plasticizers such as diphenyl-2-ethylhexyl phosphate and diphenyl octyl phosphate; epoxy plasticizers such as epoxidized soybean oil and epoxidized linseed oil fatty acid butyl ester; castor oil plasticizers such as castor oil fatty acid esters, methyl ricinoleate, ethyl ricinoleate, isopropyl ricinoleate, butyl ricinoleate, ethylene glycol monoricinoleate, propylene glycol monoricinoleate, trimethylolpropane monoricinoleate, sorbitan monoricinoleate, castor oil fatty acid polyethylene glycol esters, castor oil ethylene oxide adducts, castor oil polyols, castor oil toluene, or castor oil diols, etc. These may be used alone or in combination of two or more.
[0112] The organic filler is not particularly limited, and examples thereof include woody materials such as sawdust, wood powder, sawdust, rice husks, rice flour, starch, corn starch, straw, wheat straw, natural rubber, and other natural materials; organic fibers such as plant natural fibers, animal natural fibers, and synthetic fibers; polyester, polyacrylic acid, polyamide, nylon, polyethylene, polyolefin, polyvinyl alcohol, polyvinyl chloride, polyurethane, polyacetal, aromatic polyamide, PBO (polyparaphenylene benzoic acid) and the like. Fillers made of synthetic resin materials such as poly(vinyl acetate), polyphenylene sulfide, acetyl cellulose, polybenzazole, polyarylate, polyvinyl acetate, and synthetic rubber.
[0113] As the above-mentioned plant-based natural fibers, for example, kenaf fibers, abaca fibers, bamboo fibers, jute fibers, hemp fibers, flax fibers, hemp fibers, sisal fibers, ramie fibers, hemp, cotton, banana fibers, coconut fibers, coconut, palm, paper mulberry, agarwood, bagasse, etc. In addition, regenerated fibers such as pulp, cellulose fibers, and rayon processed from plant fibers can also be cited. As animal-based natural fibers, wool, silk, cashmere, mohair, etc. can be cited.
[0114] As above-mentioned inorganic filler, it is not particularly limited, for example can be enumerated: quartz, fumed silica, anhydrous silicic acid, fused silica, crystalline silica, amorphous silica, filler formed by condensation of alkoxysilane, silicon dioxide inorganic fillers such as superfine amorphous silica, aluminum oxide, zircon, iron oxide, zinc oxide, titanium oxide, silicon nitride, boron nitride, aluminum nitride, silicon carbide, glass, silicone rubber, silicone resin, titanium oxide, carbon fiber, mica, graphite, carbon black, ferrite, graphite, diatomaceous earth, carclazyte, clay, talc, calcium carbonate, manganese carbonate, magnesium carbonate, barium sulfate, silver powder etc.These can be surface treated in order to improve the dispersibility in resin combination.In addition, these can be used alone, and two or more can be used in combination.
[0115] The antioxidant is not particularly limited, and examples thereof include phenolic antioxidants, phosphorus antioxidants, sulfur antioxidants, etc. These may be used alone or in combination of two or more.
[0116] The hydrolysis inhibitor is not particularly limited, and examples thereof include carbodiimide compounds, epoxy compounds, isocyanate compounds, Oxazoline compounds, etc. These may be used alone or in combination of two or more.
[0117] The ultraviolet absorber is not particularly limited, and examples thereof include benzophenone compounds, benzotriazole compounds, triazine compounds, salicylic acid compounds, cyanoacrylate compounds, nickel complex salt compounds, etc. These may be used alone or in combination of two or more.
[0118] The coloring agents such as the above-mentioned pigments and dyes are not particularly limited, and examples thereof include inorganic coloring agents such as titanium oxide, calcium carbonate, chromium oxide, cuprous oxide, calcium silicate, iron oxide, carbon black, graphite, titanium yellow, and cobalt blue, soluble azo pigments such as lake red, litho scarlet, and brilliant carmine, insoluble azo pigments such as dinitroaniline orange and fast yellow, phthalocyanine pigments such as monochlorophthalocyanine blue, polychlorophthalocyanine blue, and polybrominated phthalocyanine green, condensed polycyclic pigments such as indigo, perylene red, isoindolinone yellow, and quinacridone red, and dyes such as Oracet Yellow. These may be used alone or in combination of two or more.
[0119] The antistatic agent is not particularly limited, and examples thereof include low molecular weight antistatic agents such as fatty acid ester compounds, aliphatic ethanolamine compounds, and aliphatic ethanolamide compounds, and high molecular weight antistatic agents, etc. These may be used alone or in combination of two or more.
[0120] In addition, the thermoplastic resin composition of the present embodiment may also contain: a catalyst deactivator (hindered phenol compounds, sulfide compounds, vitamin compounds, triazole compounds, polyamine compounds, hydrazine derivative compounds, phosphorus compounds, etc.), a mold release agent (montanic acid and its salts, esters, half esters, stearyl alcohol, stearamide, polyethylene wax, etc.), a coloring inhibitor (phosphites, hypophosphites, etc.), a silane coupling agent (epoxy silane coupling agent, amino silane coupling agent, (meth) acrylic silane coupling agent, isocyanate silane coupling agent, etc.), a flame retardant (red phosphorus, phosphate ester, brominated polystyrene, brominated polyphenylene ether, Brominated polycarbonate, aluminum hydroxide, magnesium hydroxide, melamine and cyanuric acid or its salt, silicon compound, etc.), conductive agent (carbon black, etc.), sliding property improver (graphite, fluororesin, etc.), epoxy compound (glycidyl ether compound, glycidyl ester compound, polymer compound obtained by grafting or copolymerizing glycidyl compound, etc.), acid anhydride compound (maleic anhydride, succinic anhydride, polymer compound obtained by grafting or copolymerizing acid anhydride, etc.), carbodiimide compound (N,N'-di-2,6-diisopropylphenylcarbodiimide, 2,6,2',6'-tetraisopropyldiphenylcarbodiimide, polycarbodiimide, etc.), etc.
[0121] The content of each of the other components described above is not particularly limited as long as the effects of the invention can be exhibited, and can be appropriately set by a person skilled in the art.
[0122] [Method for producing thermoplastic resin composition]
[0123] The thermoplastic resin composition of the present embodiment can be manufactured by a known method. Specifically, it can be mentioned that the thermoplastic resin (A), the crosslinked resin particles (B), and the crystallization nucleating agent, lubricant and other components as optional components are melt-kneaded using an extruder, a kneader, a Banbury mixer, a mixing roll, etc. In the case of melt-kneading, it is preferred to mix while paying attention to the reduction of molecular weight caused by thermal decomposition. In addition, the above-mentioned thermoplastic resin composition can also be manufactured by dissolving each component in a soluble solvent and then removing the solvent.
[0124] When the product is produced by melt kneading, each component may be separately fed into an extruder etc., or each component may be mixed in advance and then fed into an extruder etc. For example, an aqueous dispersion of the thermoplastic resin (A) and an aqueous dispersion of the crosslinked resin particles (B) may be mixed and then dried to obtain a mixed powder, and the mixed powder may be fed into an extruder etc.
[0125] When melt kneading is performed by an extruder, the obtained thermoplastic resin composition can be processed into particle shapes such as strands, columns, elliptical columns, spheres, cubes, and rectangular parallelepiped shapes by extruding the resulting thermoplastic resin composition in a strand shape and then cutting the strands.
[0126] The resin temperature during melt kneading depends on the melting point, melt viscosity, etc. of the resin used and cannot be generally limited, but is preferably 140 to 220° C., more preferably 150 to 210° C., and even more preferably 160 to 200° C. from the viewpoint of avoiding thermal decomposition of the thermoplastic resin (A) and uniformly dispersing the crosslinked resin particles (B).
[0127] <Method for producing molded article>
[0128] The thermoplastic resin composition of this embodiment can be used to produce a molded body. The molding method is not particularly limited, and commonly used molding methods can be applied, including blown film molding, extrusion blow molding, injection blow molding, extrusion molding, calendaring molding, vacuum molding, injection molding, etc.
[0129] According to the present embodiment, a molded product having improved impact resistance, specifically, a sheet, a film, a blow molded product, an extrusion molded product, a vacuum molded product, or an injection molded product can be produced with good productivity in these molding methods.
[0130] The molded article composed of the thermoplastic resin composition of this embodiment can be suitably used in agriculture, fishery, forestry, horticulture, medicine, sanitary products, food industry, clothing, non-clothing materials, packaging, automobiles, building materials, and other fields.
[0131] In the following items, preferred aspects of the present disclosure are listed, but the present invention is not limited to the following items.
[0132] [Project 1]
[0133] A thermoplastic resin composition comprising:
[0134] 40 to 90 parts by weight of a thermoplastic resin (A), and
[0135] 10 to 60 parts by weight of crosslinked resin particles (B) containing a polyhydroxyalkanoate resin and having a gel fraction of 50% or more (wherein the total amount of (A) and (B) is 100 parts by weight).
[0136] [Project 2]
[0137] The thermoplastic resin composition according to claim 1, wherein the polyhydroxyalkanoate resin is a poly(3-hydroxyalkanoate) resin.
[0138] [Item 3]
[0139] The thermoplastic resin composition according to item 1 or 2, wherein the crosslinked resin particles (B) have a volume average particle size of 0.1 μm or more and 10 μm or less.
[0140] [Item 4]
[0141] The thermoplastic resin composition according to any one of items 1 to 3, wherein the crosslinked resin particles (B) are crosslinked using a peroxide.
[0142] [Item 5]
[0143] The thermoplastic resin composition according to any one of items 1 to 4, wherein the crosslinked resin particles (B) are crosslinked in the presence of a polyfunctional compound.
[0144] [Item 6]
[0145] The thermoplastic resin composition according to any one of items 1 to 5, wherein the crosslinked resin particles (B) are not foamed.
[0146] [Item 7]
[0147] The thermoplastic resin composition according to any one of items 1 to 6, wherein the ratio of the polyhydroxyalkanoate resin in the crosslinked resin particles (B) is 80% by weight or more.
[0148] [Item 8]
[0149] The thermoplastic resin composition according to any one of items 1 to 7, wherein the thermoplastic resin (A) comprises a biodegradable resin.
[0150] [Item 9]
[0151] The thermoplastic resin composition according to item 8, wherein the biodegradable resin is a polyester resin.
[0152] [Item 10]
[0153] The thermoplastic resin composition according to any one of items 1 to 9, further comprising a crystal nucleating agent and / or a lubricant.
[0154] [Item 11]
[0155] A molded article of the thermoplastic resin composition according to any one of items 1 to 10.
[0156] [Item 12]
[0157] The molded article according to item 11, which is a sheet, a film, a blow molded product, an extrusion molded product, a vacuum molded product, or an injection molded product.
[0158] [Item 13]
[0159] A thermoplastic resin modifier comprises crosslinked resin particles (B) containing a polyhydroxyalkanoate resin and having a gel fraction of 50% or more.
[0160] Example
[0161] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples at all.
[0162] [1] Measurement conditions
[0163] 1-1. Weight average molecular weight
[0164] The resin to be measured was dissolved in chloroform, heated in a hot water bath at 60°C for 30 minutes, the soluble component was filtered using a PTFE disposable filter with a pore size of 0.45 μm, and the filtrate was used to perform GPC measurement under the following conditions to determine the weight average molecular weight.
[0165] GPC measurement equipment: High performance liquid chromatography 20A system manufactured by Shimadzu Corporation
[0166] Column: KG 4A (1 piece), K-806M (2 pieces) manufactured by Showa Denko K.K.
[0167] Sample concentration: 1mg / ml
[0168] Eluent: Chloroform solution
[0169] Eluent flow rate: 1.0ml / min
[0170] Sample injection volume: 100μL
[0171] Analysis time: 30 minutes
[0172] Standard sample: Standard polystyrene
[0173] 1-2. Volume average particle size
[0174] The volume average particle size of the crosslinked resin particles or the uncrosslinked resin particles was measured in the state of the resin particle latex. As a measuring device, Microtrac MT3300EXI I manufactured by Nikkiso Co., Ltd. was used.
[0175] 1-3. Gel fraction
[0176] The dried cross-linked resin particles or uncross-linked resin particles were added in a concentration of 0.7% by weight relative to chloroform, and dissolved at 60°C for 30 minutes to obtain a chloroform solution. Then, after standing at room temperature for 3 hours, the chloroform solution was filtered using a membrane filter with a pore size of 0.45 μm. Chloroform was applied several times inside the container and on the filter to fully wash and filter, thereby preventing loss. The gel on the filter was dried, and the weight was measured together with the filter, and the gel fraction was calculated by the following formula.
[0177] Formula: Gel fraction = (weight of the filter including the dried gel - weight of the filter alone) / weight of the cross-linked resin particles or uncross-linked resin particles used in the measurement × 100 (%)
[0178] [2] Raw materials for cross-linked resin particles
[0179] 2-1. Uncrosslinked resin particles
[0180] PHA-1: poly(3-hydroxybutyrate-co-3-hydroxyhexanoate): (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 72 / 28 (mol / mol), weight average molecular weight Mw: 700,000 to 1.5 million
[0181] PHA-2: poly(3-hydroxybutyrate-co-3-hydroxyhexanoate): (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 68 / 32 (mol / mol), weight average molecular weight Mw: 700,000 to 1.5 million
[0182] PHA-3: Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate): (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 75 / 25 (mol / mol), weight average molecular weight Mw: 600,000 to 1.5 million
[0183] 2-2. Peroxide
[0184] PO-1: tert-butyl peroxypivalate ("LUPEROX 11" manufactured by ARKEMA Yoshitomi Co., Ltd., 1-hour half-life temperature: 76°C)
[0185] PO-2: tert-butyl peroxy 2-ethylhexanoate ("LUPEROX 26" manufactured by ARKEMA Yoshitomi Co., Ltd., 1-hour half-life temperature: 95°C)
[0186] PO-3: tert-Butyl peroxy-2-ethylhexyl monocarbonate ("Perbutyl E" manufactured by NOF Corporation, 1-hour half-life temperature: 119°C)
[0187] PO-4: di-sec-butyl peroxydicarbonate ("LUPEROX 225" manufactured by ARKEMA Yoshitomi Co., Ltd., 1-hour half-life temperature: 69°C)
[0188] 2-3. Multifunctional compounds
[0189] CA-1: Allyl methacrylate
[0190] CA-2: Triallyl isocyanurate
[0191] [3] Method for producing cross-linked resin particles
[0192] The crosslinked resin particles of Production Examples 1 to 19 were produced by the following procedures using the raw materials of the types described in the tables in the amounts described in the tables.
[0193] An aqueous dispersion of uncrosslinked resin particles dispersed in water (100 parts by weight in terms of solid content), 200 parts by weight of deionized water, a given amount of peroxide, 2 parts by weight of sodium dioctyl sulfosuccinate, and a given amount of a polyfunctional compound were added to an autoclave equipped with a stirrer, a baffle, a nitrogen inlet / outlet, and a thermometer, and stirring was started at room temperature while nitrogen substitution was performed in the autoclave.
[0194] Then, the contents in the autoclave were stirred at the temperature and time of the impregnation conditions described in the table, so that the peroxide and the multifunctional compound were impregnated into the inside of the uncrosslinked resin particles, and then the temperature was raised to the reaction temperature of the crosslinking conditions described in the table. After reaching the reaction temperature, the reaction was carried out at the reaction temperature for the reaction time of the crosslinking conditions described in the table, thereby obtaining an aqueous dispersion in which the crosslinked resin particles were dispersed in water.
[0195] After adjusting the pH of the aqueous dispersion, the dispersion was dried in an oven to obtain solidified crosslinked resin particles.
[0196] The volume average particle size and gel fraction of the crosslinked resin particles obtained in each Production Example were measured by the above-mentioned method. The results are shown in Table 1.
[0197] The volume average particle size and gel fraction of the uncrosslinked resin particles before the crosslinking reaction were measured by the above-mentioned method, and the results are shown as reference examples in Table 1. In Comparative Examples 2 to 4 and 8, the uncrosslinked resin particles or their aqueous dispersions were used.
[0198] [Table 1(1)]
[0199]
[0200] [Table 1(2)]
[0201]
[0202] [4] Physical property evaluation
[0203] 4-1. Components of the test piece
[0204] (a) Thermoplastic resin (A): Amounts listed in the table (parts by weight)
[0205] Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate (produced by Kaneka Co., Ltd., Kaneka Biodegradable Polymer PHBH (registered trademark)), (3-hydroxybutyrate) / (3-hydroxyhexanoate) = 94.4 / 5.6 (mol / mol), weight average molecular weight Mw: 530,000
[0206] (b) Crosslinked resin particles (B) or uncrosslinked resin particles prepared in Production Examples 1 to 19: Amounts (parts by weight) listed in the table
[0207] (c) Pentaerythritol (Neulizer P manufactured by Nippon Synthetic Chemical Co., Ltd.): 1 part by weight
[0208] (d) Behenic acid amide (BNT22H manufactured by Nippon Seika Co., Ltd.): 0.5 parts by weight
[0209] 4-2. Method for preparing test piece
[0210] (Examples 1 to 21 and Comparative Examples 1 to 4)
[0211] The mixture of (a), (b), (c) and (d) was kneaded for 180 seconds at a screw speed of 100 rpm using a twin-screw small kneader (Xplore MC5 manufactured by DSM) with the barrel temperature heated to the temperature listed in Table 2 to obtain a kneaded product. The kneaded product was dried at 80° C. for 4 hours in a dryer to sufficiently reduce the water content, and then press-molded into a given thickness at 165° C. to prepare a test piece.
[0212] (Example 22)
[0213] The aqueous dispersion containing the thermoplastic resin (A) particles and the aqueous dispersion containing the crosslinked resin particles (B) prepared in Production Example 11 were mixed at a weight ratio of 70 / 30% in terms of solid content, the pH was adjusted to 3.8, and then dried in an oven to obtain a resin mixture.
[0214] This resin mixture and the mixture of (c) and (d) were kneaded under the same conditions as above to prepare a test piece.
[0215] 4-3. Tensile impact strength measurement conditions
[0216] The 500 μm thick sheet prepared by the above method was aged at 23° C. and 50% RH for 7 days, then punched into JIS K 71603 type test pieces and subjected to a tensile impact test in accordance with JIS K 7160A method.
[0217] [Table 2(1)]
[0218]
[0219] [Table 2(2)]
[0220]
[0221] ※Slurry blend
[0222] As shown in Table 2, Examples 1, 4, and 7 to 22 in which the crosslinked resin particles (B) are blended with the thermoplastic resin (A) have larger values of tensile impact strength than Comparative Example 1 in which only the thermoplastic resin (A) is used, and the impact resistance is improved.
[0223] In addition, it can be seen that Examples 1, 4, 7 to 10, 12, 15 to 21 have greater tensile impact strength values than Comparative Example 3 in which uncrosslinked resin particles are blended at the same blending amount, and the impact resistance is greatly improved by crosslinking. The same results can be obtained by comparing Comparative Example 2 with Example 11 and by comparing Comparative Example 4 with Example 13.
[0224] [5] Physical property evaluation related to polylactic acid
[0225] 5-1. Components of the test piece
[0226] (a) Thermoplastic resin (A): Amounts listed in Table 3 (parts by weight)
[0227] Polylactic acid: 2003D manufactured by NatureWorks
[0228] (b) Crosslinked resin particles (B), PBAT, or uncrosslinked resin particles prepared in Production Example 1, 8, 11, 15, or 17: Amounts (parts by weight) listed in Table 3
[0229] PBAT: poly(butylene adipate-co-butylene terephthalate) (Ecoflex C1200 manufactured by BASF)
[0230] 5-2. Method for preparing test piece
[0231] (Examples 23 to 29 and Comparative Examples 5 to 8)
[0232] The mixture of (a) and (b) was kneaded for 180 seconds at a screw speed of 100 rpm using a twin-screw small kneader (DSM Xplore MC5) with the barrel temperature heated to 175°C to obtain a kneaded product. The kneaded product was dried at 90°C for 2 hours in a dryer to sufficiently reduce the water content, and then press-formed at 170°C to a given thickness to prepare a test piece.
[0233] 5-3. Tensile impact strength measurement conditions
[0234] The 500 μm thick sheet prepared by the above method was aged at 23° C. and 50% RH for 7 days, then punched into JIS K 71603 type test pieces and subjected to a tensile impact test in accordance with JIS K 7160A method.
[0235] [Table 3]
[0236]
[0237] As can be seen from Table 3, Examples 23 to 29 in which cross-linked resin particles (B) are added to polylactic acid as a thermoplastic resin (A) have larger values of tensile impact strength than Comparative Example 5 which is only polylactic acid, and the impact resistance of polylactic acid is improved by adding cross-linked resin particles (B).
[0238] In addition, it can be seen that the tensile impact strength values of Examples 23 to 29 are equal to or higher than those of Comparative Examples 6 to 8 in which PBAT or uncrosslinked resin particles are added instead of crosslinked resin particles (B), and the crosslinked resin particles (B) have a good effect of improving the impact resistance of polylactic acid. Comparing Comparative Example 7 with Example 25, the tensile impact strength when 10 parts by weight of crosslinked resin particles (B) are added greatly exceeds the tensile impact strength when 20 parts by weight of PBAT are added, which shows that the crosslinked resin particles (B) have a high effect of improving the impact resistance.
[0239] [6] Evaluation of bottle-shaped molded products
[0240] 6-1. Method for producing bottle-shaped molded article
[0241] (Examples 30, 31 and Comparative Example 9)
[0242] As raw materials, (a), (b), (c) and (d) described in the above "4-1. Components of test piece" were used. Among them, as (b), the crosslinked resin particles (B) prepared in Preparation Example 11 were used in the amounts (parts by weight) described in Table 4.
[0243] The mixture of (a), (b), (c) and (d) was kneaded in a twin-screw kneader (KZW15TWIN-45WG manufactured by TECHNOVEL) with the barrel temperature heated to 140 to 165°C at a screw speed of 80 rpm to obtain a kneaded product. The kneaded product was dried in a dryer at 80°C for 4 hours to sufficiently reduce the water content.
[0244] Then, a bottle-shaped molded body with a volume of 328 ml, a thickness of 1.2 mm, an opening diameter of 66 mm, and a height of 1010 mm was produced using a 30MT injection molding machine (Si-30IV manufactured by Toyo Machinery & Metal Co., Ltd.) at a barrel temperature of 140-165°C and a mold temperature of 40°C.
[0245] 6-2. Object drop test of bottle-shaped molded body
[0246] The bottle-shaped molded body produced by the above method and the water to be filled in the bottle-shaped molded body were placed in a thermostatic bath adjusted to the test temperature described in Table 4 and aged for 12 hours or more.
[0247] Then, the bottle-shaped molded body was capped with the amount of water listed in Table 4, and was vertically and freely dropped from the height listed in Table 4 continuously for 10 times as the upper limit. The state of the bottle-shaped molded body was immediately checked each time after the drop, and the test was terminated at the stage where cracks or cracks occurred. The results are shown in Table 4. The case where there were no cracks for 10 consecutive times was recorded as "○", and when cracks occurred, the number of times the cracks occurred was recorded with a number.
[0248] [Table 4]
[0249]
[0250] As can be seen from Table 4, in Comparative Example 9 in which the crosslinked resin particles (B) were not blended with the thermoplastic resin (A), cracks occurred in the bottle-shaped molded product when it was dropped for the first time under the conditions of 23°C, 100 g of water weight, and a drop height of 100 cm. On the other hand, in Examples 30 and 31 in which the crosslinked resin particles (B) were blended, no cracks occurred even when the product was dropped 10 times even when the water weight was increased to 200 g.
[0251] Furthermore, it can be seen that under the conditions of 2°C, 100 g of water weight, and 100 cm of drop height, cracks occurred in Comparative Example 9 in which the crosslinked resin particles (B) were not blended after the second drop, whereas in Examples 30 and 31 in which the crosslinked resin particles (B) were blended, no cracks occurred even after 10 drops. In Example 31, it can be seen that no cracks occurred even after 10 drops under the same conditions when the water weight was increased to 200 g.
[0252] From the above results, it is considered that the drop resistance of the bottle-shaped molded article is significantly improved by blending the crosslinked resin particles (B) in the thermoplastic resin (A).
Claims
1. A thermoplastic resin composition comprising: 40 to 90 parts by weight of a thermoplastic resin (A), and 10 to 60 parts by weight of crosslinked resin particles (B) containing a polyhydroxyalkanoate resin and having a gel fraction of 50% or more, in, The total amount of (A) and (B) is 100 parts by weight.
2. The thermoplastic resin composition according to claim 1, wherein The polyhydroxyalkanoate resin is a poly(3-hydroxyalkanoate) resin.
3. The thermoplastic resin composition according to claim 1 or 2, wherein The volume average particle size of the crosslinked resin particles (B) is 0.1 μm or more and 10 μm or less.
4. The thermoplastic resin composition according to claim 1 or 2, wherein The crosslinked resin particles (B) are crosslinked using a peroxide.
5. The thermoplastic resin composition according to claim 4, wherein The crosslinked resin particles (B) are further crosslinked in the presence of a polyfunctional compound.
6. The thermoplastic resin composition according to claim 1 or 2, wherein The crosslinked resin particles (B) are not foamed.
7. The thermoplastic resin composition according to claim 1 or 2, wherein The ratio of the polyhydroxyalkanoate resin in the crosslinked resin particles (B) is 80% by weight or more.
8. The thermoplastic resin composition according to claim 1 or 2, wherein The thermoplastic resin (A) includes a biodegradable resin.
9. The thermoplastic resin composition according to claim 8, wherein The biodegradable resin is a polyester resin. 10 . The thermoplastic resin composition according to claim 1 , further comprising a crystal nucleating agent and / or a lubricant.
11. A molded article of the thermoplastic resin composition according to claim 1 or 2. 12 . The molded article according to claim 11 , which is a sheet, a film, a blow-molded article, an extrusion-molded article, a vacuum-molded article, or an injection-molded article.
13. A thermoplastic resin modifier comprising crosslinked resin particles (B) containing a polyhydroxyalkanoate resin and having a gel fraction of 50% or more.
Citation Information
Cited By
Biaxial orientation polyester film
CN119408270A
Composition, article thereof, and preparation method therefor
WO2026138898A1