High-temperature alloy bar drawing head treatment method
Through the same pulling head processing and welding treatment as the high-temperature alloy rod material, the problems of high rolling difficulty and high material loss during the cold drawing of high-temperature alloy rods are solved, and efficient drawing process and material yield improvement are achieved.
Patent Information
- Application Number
- CN202310583963.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
During the cold drawing process of high-temperature alloy rods, especially large-diameter materials, rolling is difficult, and the pulling head is prone to breaking, resulting in high material loss and low material yield.
The pulling head is made of the same material as the high-temperature alloy rod to be cold-drawn, and the 25-45° bevel and 2-5mm blunt edge are processed at one end. It is fixed by welding and fixing of the high-temperature alloy welding material to ensure that during the drawing process Keep cracking and polishing at the welds to smooth the transition.
The smooth pulling of high-temperature alloy rods is achieved, which reduces material losses and improves the yield rate. The pulling head can be reused, and the material surface is not damaged, which improves the reliability of the pulling process.
Smart Images

Figure CN119016530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high-temperature alloy material processing, and in particular relates to a high-temperature alloy bar drawing head processing method. Background Art
[0002] Before cold drawing high-temperature alloy bars, a drawing head needs to be made. Usually, one end of the bar is rolled thin with a rolling mill so that it can pass through the die hole for easy drawing. For hard and brittle materials such as high-temperature alloys, especially large-diameter bars, it is difficult to roll them. The rolling mill cannot roll them and they need to be rolled repeatedly. The large deformation makes the drawing head very easy to break during drawing, which has a great impact on subsequent cold drawing production. In addition, the larger the diameter of the bar, the higher the material loss caused by the drawing head, which reduces the yield rate.
[0003] The Chinese patent application number is 2018114732677, which discloses a continuous drawing device for straight bars and a method for drawing bars using the same. The continuous drawing device for straight bars and the method for drawing bars using the same include a drawing mechanism, which includes a first trolley and a second trolley arranged along the stretching direction of the bars, the first trolley reciprocates between a first initial position and a first end position, the second trolley reciprocates between a second initial position and a second end position, and the first trolley and the second trolley move in opposite directions. The present invention simultaneously clamps the first trolley and the second trolley in stages, the first front clamping device / the second front clamping device respectively grasp the head of the bar, and the first rear clamping device / the second rear clamping device alternately grasp and draw the bar, not only continuously receiving the fed bars, but also realizing the continuous and uninterrupted transmission of the straight bars from the first trolley to the second trolley, thereby realizing continuous and high-speed drawing. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the present invention provides a method for processing a high-temperature alloy bar drawing head, and the specific technical scheme is as follows: A method for processing a high-temperature alloy bar drawing head comprises the following steps: Step 1: Making a drawing head from a material that is the same as or similar to the high-temperature alloy bar to be cold drawn; Step 2: Process one end of the high-temperature alloy bar to be cold drawn and one end of the drawing head into a shape with a 25-45° groove and a 2-5mm blunt edge; Step 3: Butt the groove end of the high-temperature alloy rod processed in step 2 with the groove end of the drawing head, align the centers, and tilt the tail of the drawing head downward by 1-2°. Select welding materials that match the high-temperature alloy of the drawing head to be drawn, and weld and fix the upper part of the butt joint between the high-temperature alloy rod of the drawing head to be drawn and the drawing head; Step 4: Rotate it 180 degrees as a whole and weld it along the groove of the high-temperature alloy bar to be drawn to the groove of the drawing head; Step 5: Rotate the whole piece 180° and weld the other side of the joint in the same way. Repeat the above steps several times until the joint is fully welded.
[0005] Furthermore, in step 1, the drawing head is cylindrical, with a diameter smaller than the hole diameter of the cold drawing die and a length of 100-200 mm.
[0006] The welding material in step 3 is a high temperature alloy welding material. For example, for GH4169, GH2132, etc., welding wires of the same material can be used, or special ERNiCr series welding wires can be used. This can ensure that the weld joint is well fused and has a high enough strength so that it will not break during the drawing process. For GH3128, the commonly used high-temperature alloy welding materials are GH118 and GH3128, among which GH118 is a nickel-based alloy welding wire that can be used in high temperature, strong corrosion and oxidation environments, and has good corrosion resistance and oxidation resistance. GH3128 welding material is also a nickel-based alloy welding wire that can be used for welding GH3128 and other high-temperature alloys, and has good corrosion resistance, oxidation resistance and high temperature performance; for GH3044, the commonly used high-temperature alloy welding materials are GH3030 and GH3044, among which GH3030 is a nickel-based alloy welding wire that can be used for welding GH3044 and other high-temperature alloys, and has good corrosion resistance, oxidation resistance and high temperature performance. GH3044 welding material is also a nickel-based alloy welding wire that can be used for welding GH3044 and other high-temperature alloys, and has good corrosion resistance, oxidation resistance and high temperature performance.
[0007] Preferably, the method further comprises step 6: processing the surface of the weld, grinding the weld to be smooth, and ensuring a smooth transition from the drawn head bar to the weld.
[0008] This method is generally applicable to the cold drawing of high-temperature alloys with a diameter of more than 10 mm, and the larger the diameter, the better the effect of this method. This method has reliable strength and can ultimately achieve a smooth drawing process, reducing the material consumption of the rolling head. Only a very small amount of raw materials are used to complete the drawing process, greatly improving the yield rate, without damaging the material surface and affecting the surface quality of the material. The drawing head of this method can be reused and can be processed and used again after being cut off. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a schematic diagram of a drawing head with a bevel; Figure 2 is a schematic diagram of a high-temperature alloy rod with a groove; Figure 3 This is a schematic diagram of the docking operation implemented in step 3 of the method of the present invention; Figure 4 This is a schematic diagram of the docking operation implemented in step 4 of the method of the present invention; Figure 5 This is a schematic diagram of the operation of implementing step 5 of the method of the present invention; Figure 6 It is a schematic diagram of the product finally obtained by the method of the present invention.
[0010] Among them: 1-cold drawn head; 11-cold drawn head groove; 12-cold drawn head blunt edge; 2-high temperature alloy rod; 21-high temperature alloy rod groove; 22-high temperature alloy rod blunt edge; 3-pad; 4-welding machine. Implementation Example
[0011] A method for processing a high-temperature alloy bar drawing head comprises the following steps: Step 1: Making a drawing head from a material that is the same as or similar to the high-temperature alloy bar to be cold drawn; Step 2: If Figure 1 and Figure 2 As shown, one end of the high-temperature alloy rod to be processed by the drawing head and one end of the drawing head are processed into a shape with a 25-45° groove and a 2-5mm blunt edge; Step 3: If Figure 3 As shown, align the centers of the high-temperature alloy rod to be drawn and the drawing head, butt the groove end of the high-temperature alloy rod processed in step 2 with the groove end of the drawing head, select a high-temperature alloy welding material that matches the high-temperature alloy of the head to be drawn, and weld and fix the upper part of the butt joint between the high-temperature alloy rod to be drawn and the drawing head; Step 4: Figure 4 As shown, the whole is rotated 180° and welded along the groove of the high-temperature alloy bar to be drawn to the groove of the drawing head; Step 5: Figure 5 As shown, rotate it 180° as a whole and weld the other side of the joint in the same way; repeat the above operation several times until the joint is fully welded. Figure 6 shown.
[0012] Furthermore, in step 1, the drawing head is cylindrical, with a diameter smaller than the hole diameter of the rolling head die and a length of 100-200 mm. Example
[0013] A method for processing a high-temperature alloy bar drawing head comprises the following steps: Step 1: A drawing head is made of a material that is the same as or similar to the high-temperature alloy rod to be cold-drawn. The drawing head is cylindrical, with a diameter smaller than the hole diameter of the rolling head die and a length of 100-200 mm; Step 2: Process one end of the high-temperature alloy bar to be processed by the drawing head and one end of the drawing head into a shape with a 25-45° groove and a 2-5mm blunt edge; Step 3: Align the centers of the high-temperature alloy rod to be drawn and the drawing head, butt the groove end of the high-temperature alloy rod processed in step 2 with the groove end of the drawing head, select welding materials matching the high-temperature alloy of the drawing head, and weld and fix the upper part of the butt joint between the high-temperature alloy rod to be drawn and the drawing head; Step 4: Rotate it 180 degrees as a whole and weld it along the groove of the high-temperature alloy bar to be drawn to the groove of the drawing head; Step 5: Rotate the whole piece 180° and weld the other side of the joint in the same way. Repeat the above steps several times until the joint is fully welded. Step 6: Treat the weld surface and grind it smooth. The weld height should not be higher than the hole diameter of the drawing die, and the weld should transition smoothly from the bar to the drawing head.
Claims
1. A method for cold drawing a high temperature alloy bar, characterized in that The following steps are involved: Step 1: A drawing head is made of a material that is the same as or similar to the high-temperature alloy bar to be cold drawn; Step 2: Process one end of the high-temperature alloy bar to be cold drawn and one end of the drawing head into a shape with a 25-45° groove and a 2-5mm blunt edge; Step 3: Butt the groove end of the high-temperature alloy rod processed in step 2 with the groove end of the drawing head, align the centers, tilt the tail of the drawing head downward by 1-2°, select welding materials matching the high-temperature alloy rod to be drawn, and weld and fix the upper part of the butt joint between the high-temperature alloy rod to be drawn and the drawing head; Step 4: Rotate it 180 degrees as a whole and weld it along the groove of the high-temperature alloy bar to be drawn to the groove of the drawing head; Step 5: Rotate the whole piece 180° and weld the other side of the joint in the same way. Repeat the above steps several times until the joint is fully welded.
2. The method for processing a high-temperature alloy rod drawing head according to claim 1, characterized in that In step 1, the drawing head is cylindrical, and its diameter is less than Cold drawn The hole diameter and length of the mold are 100-200mm.
3. The method for processing a high-temperature alloy rod drawing head according to claim 1, characterized in that The welding material in step 3 is a high-temperature alloy welding material.
4. The method for processing a high-temperature alloy rod drawing head according to claim 1, characterized in that The step 6 is also included: treating the weld surface, grinding the weld smooth, ensuring that the weld height is no higher than the aperture of the drawing die, and the entire weld has a smooth transition.
Citation Information
Patent Citations
Method for forming large-diameter stainless steel square tube
CN102716934A
Forming method of precise high-temperature alloy pipe with small caliber and thick wall for aviation
CN103934304A
Pipe head clamping tool for drawing colored rare metal pipe
CN106734287A
Bar straight strip continuous drawing device and bar drawing method realized by utilizing bar straight strip continuous drawing device
CN110153207A
PROCESS FOR INCREASING THE YIELD IN THE MANUFACTURE OF DRAWN PRODUCTS FROM BAR MATERIAL
DE2425696A1
Cited By
Wire drawing process of wire rod
CN120772259A