Improved recycled concrete aggregate with good plant growth property and preparation method thereof

By combining biochar and biopolymer in recycled concrete aggregate, the strength and alkalinity problems of construction waste resource recycling and vegetative concrete are solved, and a good vegetation growth environment and engineering properties are improved. It is suitable for a variety of purposes Engineering applications.

CN119019107APending Publication Date: 2024-11-26SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411248281.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively utilize construction waste for resource utilization, and there are strength and alkalinity problems in the application of vegetation concrete, which affects vegetation growth.

Method used

Using the combination of biochar and biopolymer with regenerated concrete aggregates, the improved regenerated concrete aggregates with good plant properties are prepared by screening the optimal biopolymer species and proportions, including biochar, regenerated concrete aggregate and water. The carbon is 10%, and the biopolymer is 0.5% to 1.5%. By stirring and compacting, an environment suitable for vegetation growth is formed.

Benefits of technology

It improves the vegetation growth rate and reuse characteristics of recycled concrete aggregates, reduces alkalinity, provides an environmentally friendly and stable solution, and is suitable for engineering problems such as slope landslides, landfill leakage and tailings yards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an improved recycled concrete aggregate with good vegetation performance and a preparation method thereof, and the preparation method comprises the following steps: screening an improved material for improving the vegetation performance of the recycled concrete aggregate, and carrying out biochar improved concrete aggregate plant growth experiments with different biopolymer types and proportions; the optimal biopolymer type and proportion are determined by observing the plant growth germination rate and average height of the biochar improved concrete aggregate with different biopolymer types and proportions; the biopolymer, the biochar, the recycled concrete aggregate and water are mixed and compacted according to engineering requirements, and the biopolymer-biochar improved concrete aggregate meeting the engineering construction requirements is prepared. The method is suitable for different engineering requirements, and an environment-friendly and stable method is provided for preventing and treating various engineering problems such as side slope landslide, refuse landfill leakage and tailing storage yard instability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of geotechnical engineering, and specifically provides an improved recycled concrete aggregate with good vegetative properties and a preparation method thereof. Background Art

[0002] In order to cope with the growing problem of construction waste, the development principle of "reduction, reuse and circulation" should be followed. Recycling and reusing these construction wastes can reduce the dependence on natural aggregates, while reducing the storage cost of construction waste, releasing landfill capacity, and reducing greenhouse gas emissions. Studies have shown that the use of specific construction processes can process construction waste into recycled aggregate concrete with low structural strength, good permeability and low alkalinity. It has been applied to some projects with low strength requirements or non-structural concrete, such as river bank protection, road slope protection, roof greening, and resilient city construction, etc., realizing the recycling and reuse of construction waste, which has important social and economic benefits.

[0003] Biochar is an organic substance formed by the pyrolysis of various plants and biomass under high temperature and low oxygen conditions. It has the characteristics of large specific surface area, strong ion exchange capacity, low density, high porosity and high stability. Biochar can improve the water retention capacity of soil. At the same time, biochar can also effectively reduce the pH value of soil and provide nutrients required for plant growth, thereby improving soil engineering. Biopolymers are a class of macromolecular compounds synthesized by organisms, usually composed of repeating units. Common biopolymers include cellulose, chitosan and lignin. In recent years, biopolymers have been gradually used to improve soil engineering properties due to their wide sources, ecological and environmental protection, and excellent performance. In addition, the hydroxyl groups of biopolymers combine with soil particles to form a gel network, which effectively improves the water retention capacity of soil. The greater the amount of biopolymers, the better the water retention of soil. Compared with natural soil, polysaccharides and other substances in biopolymers can provide a better growth environment for vegetation growth. Therefore, this paper studies the vegetative properties of concrete, screens out the optimal types and proportions of biopolymers, and prepares a recycled concrete aggregate that can promote vegetation growth by adding biochar and biopolymers, thereby improving the reuse efficiency and engineering properties of recycled concrete aggregates, and providing a reference for the resource reuse of construction waste and various ecological protection projects. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide an improved recycled concrete aggregate with good vegetative properties and a preparation method. The material uses green and economical raw materials, and through a simple method, screens and configures recycled concrete aggregates that promote vegetative properties, and then applies them to engineering construction, providing a reference for the resource recycling of construction waste. It can not only solve the resource problem of recycling and reusing construction waste, but also prepare the optimal biopolymer-biochar improved concrete according to engineering needs, adapt to the needs of different projects, and provide an environmentally friendly and stable method for the prevention and control of various engineering problems such as slope landslides, landfill leakage, and tailings yard instability.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] An improved recycled concrete aggregate with good vegetative properties, comprising biochar, recycled concrete aggregate, biopolymer and water;

[0007] Among them, by weight: 90 to 100 parts of recycled concrete aggregate, 15 to 20 parts of water, 10% of the weight of the recycled concrete aggregate by biochar, and 0.5% to 1.5% of the weight of the recycled concrete aggregate by biopolymer.

[0008] Preferably, the recycled concrete aggregate is selected from crushed construction waste, and the particle size of the recycled concrete aggregate is less than 2 mm.

[0009] Preferably, the biochar is selected from peanut shells, the particle size of the biochar is less than 0.075 mm, the moisture content is less than 0.5%, and the pyrolysis temperature of the biochar is 200 degrees Celsius.

[0010] Preferably, the biopolymer is gellan gum, and the particle size of the biopolymer is less than 2 mm.

[0011] The preparation process of the improved recycled concrete aggregate with good vegetative properties comprises the following steps:

[0012] Step 1: Select biopolymer-biochar-aggregate mixtures made of different biopolymer types and proportions, measure the pH value and other physical and chemical properties of the mixtures and analyze them to determine the characteristic parameters of the physical and chemical properties;

[0013] Step 2: Pre-weigh the components of the materials, and fully mix the biopolymer-biochar-aggregate of different biopolymer types and proportions to obtain a mixed aggregate;

[0014] Step 3: adding water to the mixture so that the water content of the biopolymer-biochar mixed aggregate is greater than 14%, and stirring and mixing in a mixer for not less than 600 seconds, or manually stirring for not less than 1200 seconds;

[0015] Step 4: Pour the mixed biopolymer-biochar aggregate into a circular mold for compaction, with a compaction degree greater than 80%;

[0016] Step 5: Place the compacted biopolymer-biochar modified aggregates with different biopolymer types and ratios in an environment of 25±0.5℃ and 50% humidity for vegetation growth experiment;

[0017] Step 6: By recording the vegetation growth parameters, including germination rate and growth height, analyzing the results of the vegetation growth experiment, and selecting the type and proportion of biopolymer used in the modified aggregate with the best plant growth.

[0018] The present invention can screen out the optimal type and ratio of biopolymer-improved biochar-aggregate mixture, which can reduce the alkalinity of recycled concrete aggregate, increase vegetation growth rate and improve the reuse characteristics of aggregate. The present invention applies the biopolymer-biochar-improved concrete to engineering construction and engineering management with environmental protection requirements and lower strength requirements.

[0019] Beneficial effects: The present invention adopts a specific construction process to process construction waste into recycled aggregate concrete with lower structural strength, good water permeability and low alkalinity value. Biochar has the characteristics of large specific surface area, strong ion exchange capacity, low density, high porosity and high stability, and can further reduce the alkalinity of recycled aggregate concrete. Peanut shell biochar and gellan gum are the main admixtures in biopolymer-biochar improved concrete, which is the key to promoting the vegetative nature of concrete. The porosity of biochar can store more water and improve the water retention capacity of the soil. At the same time, as an organic matter formed by the pyrolysis of various plants and biomass, biochar can provide essential nutrients for plant growth; the hydroxyl groups of biopolymers combine with soil particles to form a gel network, which can also effectively improve the water retention capacity of the soil, and the greater the amount of biopolymer added, the better the water retention of the soil. Compared with natural soil, substances such as polysaccharides in biopolymers can provide a better growth environment for vegetation growth. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0021] An improved recycled concrete aggregate with good vegetative properties, comprising: biopolymer, biochar, recycled concrete aggregate and water; wherein, by weight, the concrete aggregate is 90 to 100 parts, and the water is 15 to 20 parts;

[0022] Biochar is 10% of the weight of recycled concrete aggregate;

[0023] The biopolymers are 0.5%, 1.0% and 1.5% by weight of the recycled concrete aggregate respectively;

[0024] The recycled concrete aggregate is crushed construction waste with a particle size of less than 2 mm and a moisture content of less than 0.5%; the raw material of the biochar is peanut shells with a particle size of less than 0.075 mm and a moisture content of less than 0.5%; the pyrolysis temperature of the biochar is 200 degrees Celsius; the biopolymer raw material is gellan gum; and the particle size of the biopolymer is less than 2 mm.

[0025] Weigh the components of the materials in advance, mix the biopolymer, biochar and recycled concrete aggregate to obtain a mixed soil, and measure the pH value of the mixture; the content of the biopolymer is 0.5%, 1.0% and 1.5% of the weight of the recycled concrete aggregate respectively. The content of biochar is 10% of the recycled concrete aggregate. Add the weighed water to the mixed soil so that the moisture content of the mixed soil is 14%, and stir and mix in a mixer for 600 seconds; after stirring, pour the mixture into a circular mold with a diameter of 80mm for molding, and then compact it with a compaction degree of 80%; then sow tall fescue seeds at 30±0.5℃ and 50% humidity to conduct a plant growth experiment: the density is 30g / m 2 ; Use drip irrigation to apply an equal and appropriate amount of water every day, and record the germination status and plant height every 24 hours.

[0026] The application of the improved recycled concrete aggregate with good vegetative properties includes: applying the biopolymer-biochar improved concrete to engineering construction and engineering management with environmental protection requirements and lower strength requirements.

[0027] Performance indicators:

[0028] 1. Conduct a vegetative test on the sample and obtain its plant growth image.

[0029] 2. Carry out vegetative experiments on the samples, and obtain parameters reflecting plant growth such as plant height through measurement and statistics.

[0030] The test results of Example 1-4 are shown in Table 1-3:

[0031] Table 1 Plant germination rate in recycled concrete with different biopolymer and biochar dosages

[0032]

[0033] Table 2 Average height of plants

[0034]

[0035] Table 3 Average height of plants

[0036]

[0037] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

Claims

1. An improved recycled concrete aggregate with good vegetative properties, characterized in that: Includes biochar, recycled concrete aggregate, biopolymers and water; Among them, by weight: 90 to 100 parts of recycled concrete aggregate, 15 to 20 parts of water, 10% of the weight of the recycled concrete aggregate by biochar, and 0.5% to 1.5% of the weight of the recycled concrete aggregate by biopolymer.

2. The improved recycled concrete aggregate with good vegetative properties according to claim 1, characterized in that: The recycled concrete aggregate is selected from crushed construction waste, and the particle size of the recycled concrete aggregate is less than 2 mm.

3. The improved recycled concrete aggregate with good vegetative properties according to claim 1, characterized in that: The biochar is selected from peanut shells, the particle size of the biochar is less than 0.075 mm, the moisture content is less than 0.5%, and the pyrolysis temperature of the biochar is 200 degrees Celsius.

4. The improved recycled concrete aggregate with good vegetative properties according to claim 1, characterized in that: The biopolymer is gellan gum, and the particle size of the biopolymer is less than 2 mm.

5. The process for preparing an improved recycled concrete aggregate with good vegetative properties as claimed in claim 1, 2, 3 or 4, characterized in that: The following steps are involved: Step 1: Select biopolymer-biochar-aggregate mixtures made of different biopolymer types and proportions, measure the pH value and other physical and chemical properties of the mixtures and analyze them to determine the characteristic parameters of the physical and chemical properties; Step 2: Pre-weigh the components of the materials, and fully mix the biopolymer-biochar-aggregate of different biopolymer types and proportions to obtain a mixed aggregate; Step 3: adding water to the mixture so that the water content of the biopolymer-biochar mixed aggregate is greater than 14%, and stirring and mixing in a mixer for not less than 600 seconds, or manually stirring for not less than 1200 seconds; Step 4: Pour the mixed biopolymer-biochar aggregate into a circular mold for compaction, with a compaction degree greater than 80%; Step 5: Place the compacted biopolymer-biochar modified aggregates with different biopolymer types and ratios in an environment of 25±0.5℃ and 50% humidity for vegetation growth experiment; Step 6: By recording the vegetation growth parameters, including germination rate and growth height, analyzing the results of the vegetation growth experiment, and selecting the type and proportion of biopolymer used in the modified aggregate with the best plant growth.