NiO-coated PPy composite material and preparation method and application thereof
By coating polypyrrole on the surface of NiO microspheres to form NiO@PPy composite material, the volume expansion and contraction problem of lithium-ion battery negative electrode material during charging and discharging is solved, the stability and electrochemical performance of the material are improved, and the high capacity is achieved and good cycle performance.
Patent Information
- Application Number
- CN202411200992.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The existing lithium-ion battery anode material has severe volume expansion and contraction during charging and discharging, resulting in structural instability, affecting cycling performance and Coulomb efficiency, and the capacity increase space of carbon-based materials is limited.
NiO@PPy composite material was used to prepare NiO microspheres by hydrothermal method, and polypyrrole was coated on the surface of NiO microspheres by chemical in situ polymerization to form a porous nanostructure, improving the mechanical stability and electrochemical properties of the material.
The structural stability and electrochemical performance of NiO@PPy composite materials are improved, and high reversible capacity, good cycling performance and excellent rate performance are shown, which avoids particle breakage and aggregation and improves electrical conductivity.
Smart Images

Figure CN119059579A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a NiO@PPy composite material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high capacity, good cycle performance, small irreversible capacity, good rate performance, and stable electrochemical performance in electrolytes, making them a hot research topic. At present, the most reported negative electrode materials for lithium-ion batteries are concentrated on carbon-based materials, including amorphous carbon materials and graphite carbon materials, but there is little room for the capacity of such materials to increase. In addition, there are silicon-based, tin-based, and transition metal oxide negative electrode materials for lithium-ion batteries. However, silicon-based and tin-based materials will experience severe volume expansion and contraction during charge and discharge, causing the structure of the active material to be unstable or collapse, thereby affecting its cycle performance and coulombic efficiency.
[0003] Transition metal oxides are one of the most promising negative electrode materials for lithium-ion batteries due to their high theoretical specific capacity, low electrode potential, low price, and environmental friendliness. The negative electrode composed of transition metal oxide nanostructures has a higher capacity than the most advanced graphite material (372mAh g -1 ) Significantly higher theoretical capacity (>600mAh g -1 Among them, nickel oxide (NiO) is easy to obtain and simple to prepare, and has a high theoretical specific capacity (about 718 mAh g -1 ), and is expected to become the next generation of lithium-ion battery negative electrode material.
[0004] The morphology and size of transition metal oxides are one of the key factors affecting the lithium storage performance of materials. For this reason, they are usually prepared into nanoscale materials or porous materials. The hybrid structure composed of carbon and transition metal oxides has high stability and can well balance capacity and rate capability. The transition metal oxides provide high capacity, while the carbon matrix provides good conductivity and stability. Reasonable regulation of the composite morphology between the two plays a positive role in slowing down the volume expansion of the material and preventing self-agglomeration. Summary of the invention
[0005] In view of the above background technology, the present invention provides a NiO@PPy (polypyrrole) composite material and its preparation method and application. The NiO@PPy composite material prepared by the present invention has a porous nanostructure and has excellent electrochemical properties as a negative electrode material for lithium ion batteries.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] In one aspect, the present invention provides a method for preparing a NiO@PPy composite material, comprising the following steps:
[0008] (1) Preparation of NiO microspheres
[0009] The nickel source and hexamethylenetetramine are subjected to hydrothermal reaction, and NiO microspheres are prepared by calcination;
[0010] (2) Preparation of NiO@PPy composite materials
[0011] The NiO microspheres, an oxidant, a pyrrole monomer, a halide ion dopant and a surfactant are reacted in a solution to obtain the NiO@PPy composite material.
[0012] As a preferred embodiment, in step (1), the nickel source is a nickel salt selected from at least one of nickel nitrate, nickel hydrochloride, nickel acetate and nickel sulfate;
[0013] Preferably, the molar ratio of nickel to hexamethylenetetramine in the nickel source is 1 to 1.6:2.
[0014] As a preferred embodiment, in step (1), the temperature of the hydrothermal reaction is 100-120°C;
[0015] Preferably, the hydrothermal reaction time is 4 to 6 hours, more preferably 5 hours.
[0016] As a preferred embodiment, in step (1), the calcination temperature is 300-400°C;
[0017] Preferably, the calcination time is 1.5 to 2 hours;
[0018] Preferably, the heating rate of the calcination is 1 to 3°C / min;
[0019] Preferably, the calcination is carried out in an air atmosphere.
[0020] In certain specific embodiments, in step (1), the hydrothermal reaction further includes washing and drying; the washing is washing with water and ethanol; the drying is drying at 60-80° C. for 10-12 hours.
[0021] As a preferred embodiment, in step (2), the oxidant is selected from at least one of ammonium persulfate, hydrogen peroxide, ferric oxide and ferric chloride;
[0022] Preferably, the dosage of the NiO microspheres and the oxidant is in the following relationship: 0.2-0.3 g of oxidant for every 60 mg of NiO microspheres;
[0023] Preferably, the halide ion dopant is selected from at least one of HCl, HBr and HF;
[0024] Preferably, the amount of the halide ion dopant used is 0.01 to 0.02 mol halide ion / 1 g NiO microspheres in terms of the amount of halide ion substance compared to the NiO microspheres;
[0025] Preferably, the dosage of the NiO microspheres and the pyrrole monomer is in the following relationship: 0.060 to 0.075 mL of pyrrole monomer for every 60 mg of NiO microspheres;
[0026] Preferably, the surfactant is selected from at least one of sodium dodecyl sulfate, ammonium dodecyl sulfonate and hexadecyltrimethylammonium bromide;
[0027] Preferably, the dosage of the NiO microspheres and the surfactant is in the following relationship: 2 to 10 mg of surfactant for every 60 mg of NiO microspheres.
[0028] As a preferred embodiment, in step (2), the reaction temperature is 0 to 5°C; the reaction time is 3 to 4 hours;
[0029] In certain specific embodiments, in step (2), the reaction further includes washing and drying treatment; the washing is washing with water and ethanol; the drying is drying at 60-80° C. for 10-12 hours.
[0030] In some specific embodiments, step (2) specifically includes:
[0031] S1. Preparing a dispersion containing NiO microspheres and a surfactant;
[0032] S2. The dispersion of step S1 is mixed with a halide ion dopant and a pyrrole monomer and stirred at 0 to 5°C;
[0033] S3. The mixture in step S2 is mixed with ammonium persulfate and stirred at 0-5°C.
[0034] In certain specific embodiments, in step S1, the preparation of the dispersion containing NiO microspheres and a surfactant is performed by adding NiO microspheres to a dispersion containing a surfactant, ultrasonically treating for 20 to 30 minutes, and stirring at 600 to 800 rpm for 3 to 4 hours; the dispersion containing a surfactant is prepared by dispersing the surfactant in water and stirring at 500 to 700 rpm for 20 to 30 minutes.
[0035] In some specific embodiments, in step S2, the mixing is to add the halide ion dopant and the pyrrole monomer into the dispersion of step S1; and the stirring is to stir at 600-800 rpm for 1-2 hours.
[0036] In certain specific embodiments, in step S3, the mixing is to add ammonium persulfate or its solution to the mixture obtained in step S2; and the stirring is to stir at 500-600 rpm for 3-4 hours.
[0037] In another aspect, the present invention provides a NiO@PPy composite material obtained by the above preparation method.
[0038] In another aspect, the present invention provides use of the above-mentioned NiO@PPy composite material in preparing a battery;
[0039] Preferably, use in preparing lithium ion batteries;
[0040] Preferably, the invention is used in preparing negative electrode materials for lithium-ion batteries.
[0041] The above technical solution has the following advantages or beneficial effects:
[0042] The present invention provides a core-shell structured NiO@PPy composite material, which is prepared by a hydrothermal method and a chemical in-situ polymerization method. During the polymerization process, polypyrrole is coated on the surface of a nanoflower NiO microsphere formed by self-assembly of a sheet structure, giving the composite material good mechanical stability and electrochemical properties. In addition, in the present invention, the NiO@PPy composite material not only improves the electrical conductivity of polypyrrole, but also has weak alkalinity, has little effect on the positive charge distribution of the polypyrrole main chain, is conducive to the transmission of charges, and thus has good electrochemical properties.
[0043] Compared with the prior art, the present invention has the following advantages:
[0044] (1) The core-shell structure of the NiO@PPy composite material prepared by the present invention can avoid particle breakage and aggregation, thereby ensuring the structural stability during the charge and discharge cycle; in addition, the polypyrrole coating improves the conductivity of the NiO microspheres, showing high reversible capacity, good cycle performance and excellent rate performance;
[0045] (2) The preparation method provided by the present invention first prepares the precursor Ni(OH)2 by a hydrothermal method, and then obtains NiO microspheres by calcination. In this process, the morphology of NiO microspheres can be regulated by controlling the reaction conditions, such as the ratio of raw materials, the calcination temperature, etc., so as to obtain NiO microspheres with uniform size and morphology;
[0046] (3) The NiO@PPy composite material provided by the present invention is a nanocomposite material with a large specific surface area, thereby exhibiting higher electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is a TEM image of the NiO@PPy nanocomposite material prepared in Example 1 of the present invention.
[0048] Figure 2 This is the cycle stability curve of the NiO@PPy nanocomposite material prepared in Example 1 of the present invention.
[0049] Figure 3 This is a rate performance diagram of the NiO@PPy nanocomposite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0050] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0051] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.
[0052] Example 1
[0053] This embodiment provides a NiO@ppy nanocomposite material, and the preparation process is as follows:
[0054] (1) Preparation of NiO microspheres
[0055] 2.91g Ni(NO3)2·6H2O and 2.80g hexamethylenetetramine were dissolved in 60mL ultrapure water in turn and stirred for 30min; the stirred solution was charged into 80mL Teflon-lined stainless steel autoclave and reacted in a 120℃ oven for 5h; the synthesized product was washed three times with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven at 80℃ for 12h; the dried sample was ground into a uniform powder with a mortar, and then placed in a tubular furnace for calcination in an air atmosphere. The calcination process was 300℃ for 2h, and the heating rate was 1℃ / min to obtain a NiO microsphere sample.
[0056] (2) Preparation of NiO@ppy nanocomposites
[0057] Weigh 5 mg of sodium dodecyl sulfate and disperse it in 50 mL of deionized water, and stir it at 600 rpm for 30 min; weigh 60 mg of NiO microsphere sample and add it to the above solution, ultrasonically treat it for 30 min, and then stir it at 600 rpm and room temperature for 3 h, which is recorded as solution A;
[0058] 1 mL of 1 mol / L HCl solution and 0.060 mL of pyrrole monomer were added to solution A successively, and stirred at 600 rpm for 1 h in an ice-water bath, which was recorded as solution B.
[0059] Weigh 0.2 g of ammonium persulfate and dissolve it in 10 mL of H2O, stir to obtain a uniform solution C; add solution C dropwise into solution B, and stir at 500 rpm in an ice-water bath for 3 h; wash the product with deionized water and anhydrous ethanol for 3 times, respectively, and place the washed black solid sample in a vacuum drying oven at 80°C for 12 h to obtain a NiO@ppy nanocomposite material.
[0060] Performance Testing
[0061] 1. Figure 1 This is a TEM image of the NiO@ppy nanocomposite material synthesized in this example. It can be seen from the image that the nanocomposite material has a flower-like structure formed by self-assembly of sheets, and the PPy layer is evenly and tightly coated on the NiO surface to form a core-shell structure.
[0062] 2. The NiO@ppy nanocomposite material or the NiO microspheres prepared in step (1) are respectively put into a mortar with Ketjen black and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1, and ground and mixed evenly, and an appropriate amount of N-methylpyrrolidone (NMP) is added to form a slurry and further ground and mixed; the slurry is evenly coated on a copper foil and dried in a vacuum oven at 120°C. After drying, a copper foil cut piece with active material is obtained as an electrode sheet, and the loading amount is selected to be 1 mg / cm 2 The disc electrode sheet is placed in a sealed bag for later use. The disc electrode sheet is used as the negative electrode to prepare a CR-2032 button battery. The preparation process is carried out in a glove box filled with inert argon gas. The water oxygen value in the glove box is controlled within 0.01ppm. The electrolyte is a commercial lithium battery electrolyte with 1.0 mol / L LiPF6 as the solute and an electrolyte solvent with a volume ratio of 1:1:1 of ethylene carbonate: dimethyl carbonate: diethyl carbonate.
[0063] The above batteries were tested on a blue electricity tester for 1Ag -1 Cycle life test, test results see Figure 2 From the figure, we can see that although NiO microspheres have a higher specific capacity, they continue to decay during the cycle, decaying to 150 mAh g after 500 cycles. -1 , its cycle stability is only 14.2%, while the capacity of NiO@PPy can be maintained at 400mAhg after 500 cycles. -1 The cycle stability is about 70.1%.
[0064] The above batteries were tested for rate performance on a blue battery tester, with the test voltage range of 0.01 to 3V. The test results are shown in Figure 3 .from Figure 3 It can be seen that NiO microspheres have a -1 When the temperature was 1056, 986, 905, 864, 718, 394, and 107 mAh g -1 The average discharge capacity, when the current density is restored to 0.1A -1 When the capacity is restored to 865mAh g -1 . NiO@PPy nanomaterials at 0.1, 0.2, 0.4, 0.5, 1, 2, 4Ag -1 When the power consumption is 812, 634, 500, 468, 382, 273, and 138 mAh g -1 The average discharge capacity, when the current density is restored to 0.1A -1 When the capacity is restored to 726mAh g -1 It can be seen that although NiO has a higher specific capacity at low current, it has a lower specific capacity at 1, 2, and 4A g -1 The capacity of NiO@PPy decreases significantly at high current, while NiO@PPy has better stability under high current.
[0065] Example 2
[0066] This embodiment provides a NiO@PPy nanocomposite material, and the preparation process is as follows:
[0067] (1) Preparation of NiO microspheres
[0068] 3.50g Ni(NO3)2·6H2O and 2.80g hexamethylenetetramine were dissolved in 60mL ultrapure water in turn and stirred for 25min; the stirred solution was charged into an 80ml Teflon-lined stainless steel autoclave and reacted in an oven at 110℃ for 5h; the synthesized product was washed four times with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven at 70℃ for 10h; the dried sample was ground into a uniform powder with a mortar, and then placed in a tubular furnace for calcination in an air atmosphere. The calcination process was 250℃ for 1.5h, and the heating rate was 2℃ / min to obtain a NiO microsphere sample.
[0069] (2) Preparation of NiO@ppy nanocomposites
[0070] Weigh 5 mg of sodium dodecyl sulfate and disperse it in 50 mL of deionized water, and stir it at 700 rpm for 20 min; weigh 60 mg of NiO microsphere sample and add it to the above solution, ultrasonically treat it for 20 min, and then stir it at 700 rpm and room temperature for 3 h, which is recorded as solution A;
[0071] 1 mL of 1 mol / L HCl solution and 0.065 mL of pyrrole monomer were added to solution A successively, and stirred at 600 rpm for 1 h in an ice-water bath, which was recorded as solution B.
[0072] Weigh 0.2 g of ammonium persulfate and dissolve it in 10 mL of H2O, stir to obtain a uniform solution C; add solution C dropwise into solution B, and stir at 500 rpm in an ice-water bath for 3 h; wash the product with deionized water and anhydrous ethanol for 4 times, respectively, and place the washed black solid sample in a vacuum drying oven at 80°C for 12 h to obtain a NiO@ppy nanocomposite material.
[0073] Example 3
[0074] This embodiment provides a NiO@PPy nanocomposite material, and the preparation process is as follows:
[0075] (1) Preparation of NiO microspheres
[0076] 4.37g Ni(NO3)2·6H2O and 2.80g hexamethylenetetramine were dissolved in 60mL ultrapure water and stirred for 30min. The stirred solution was placed in an 80mL Teflon-lined stainless steel autoclave and reacted in a 100℃ oven for 5h. The synthesized product was washed with deionized water and anhydrous ethanol three times, and then dried in a vacuum drying oven at 65℃ for 12h. The dried sample was then ground into a uniform powder with a mortar, and then placed in a tubular furnace for calcination in an air atmosphere. The calcination process was 200℃ for 2h, and the heating rate was 2℃ / min to obtain a NiO microsphere sample.
[0077] (2) Preparation of NiO@ppy nanocomposites
[0078] Weigh 5 mg of sodium dodecyl sulfate and disperse it in 50 mL of deionized water, and stir it at 500 rpm for 30 min; weigh 60 mg of NiO microsphere sample and add it to the above solution, ultrasonically treat it for 30 min, and then stir it at 500 rpm and room temperature for 3 h, which is recorded as solution A;
[0079] 1 mL of 1 mol / L HCl solution and 0.070 mL of pyrrole monomer were added to solution A successively, and stirred at 600 rpm for 1 h in an ice-water bath, which was recorded as solution B.
[0080] Weigh 0.2 g of ammonium persulfate and dissolve it in 10 mL of H2O, stir to obtain a uniform solution C; add solution C dropwise into solution B, and stir at 500 rpm in an ice-water bath for 3 h; wash the product with deionized water and anhydrous ethanol for 4 times, respectively, and place the washed black solid sample in a vacuum drying oven at 80°C for 12 h to obtain a NiO@ppy nanocomposite material.
[0081] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a NiO@PPy composite material, It is characterized in that The following steps are involved: (1) Preparation of NiO microspheres The nickel source and hexamethylenetetramine are subjected to hydrothermal reaction, and NiO microspheres are prepared by calcination; (2) Preparation of NiO@PPy composite materials The NiO microspheres, an oxidant, a pyrrole monomer, a halide ion dopant and a surfactant are reacted in a solution to obtain the NiO@PPy composite material.
2. The preparation method according to claim 1, It is characterized in that In step (1), the nickel source is a nickel salt selected from at least one of nickel nitrate, nickel hydrochloride, nickel acetate and nickel sulfate; Preferably, the molar ratio of nickel to hexamethylenetetramine in the nickel source is 1 to 1.6:
2.
3. The preparation method according to claim 1, It is characterized in that In step (1), the temperature of the hydrothermal reaction is 100-120° C.; Preferably, the hydrothermal reaction time is 4 to 6 hours, more preferably 5 hours.
4. The preparation method according to claim 1, It is characterized in that In step (1), the calcination temperature is 300-400°C; Preferably, the calcination time is 1.5 to 2 hours; Preferably, the heating rate of the calcination is 1 to 3°C / min; Preferably, the calcination is carried out in an air atmosphere.
5. The preparation method according to claim 1, It is characterized in that In step (2), the oxidant is selected from at least one of ammonium persulfate, hydrogen peroxide, ferric oxide and ferric chloride; Preferably, the dosage of the NiO microspheres and the oxidant is in the following relationship: 0.2-0.3 g of oxidant corresponds to every 60 mg of NiO microspheres.
6. The preparation method according to claim 1, It is characterized in that The halide ion dopant is selected from at least one of HCl, HBr and HF; Preferably, the amount of the halide ion dopant used is 0.01-0.02 mol halide ion / 1 g NiO microspheres in terms of the amount of halide ion substance compared to the NiO microspheres.
7. The preparation method according to claim 1, It is characterized in that The dosage relationship of the NiO microspheres and the pyrrole monomer is: every 60 mg of NiO microspheres corresponds to 0.060 to 0.075 mL of pyrrole monomer; Preferably, the surfactant is selected from at least one of sodium dodecyl sulfate, ammonium dodecyl sulfonate and hexadecyltrimethylammonium bromide; Preferably, the dosage of the NiO microspheres and the surfactant is in the following relationship: 2 to 10 mg of surfactant for every 60 mg of NiO microspheres.
8. The preparation method according to claim 1, It is characterized in that In step (2), the reaction temperature is 0 to 5°C; and the reaction time is 3 to 4 hours.
9. The NiO@PPy composite material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the NiO@PPy composite material according to claim 9 in preparing a battery; Preferably, use in preparing lithium ion batteries; Preferably, the invention is used in preparing negative electrode materials for lithium-ion batteries.
Citation Information
Patent Citations
Method for preparing flower form nickelous oxide
CN101269850A
Globular-flower shaped nickel oxide / polypyrrole / graphene composite material and preparation method therefor
CN107706000A
Preparation method of spherical N-doped C-coated metal oxide negative electrode material with multi-stage structure
CN108258223A
Nickel oxide composite material, and preparation method and application thereof
CN113224301A
Fabrication of supercapacitor electrode based on amorphous carbon coated Nickel oxide nanofibers using electrospinning, vapor deposition polymerization and heat treatment
KR101576739B1