Two-component silicone rubber adhesive for bonding metal and resin and preparation method thereof

Through the design of two-component silicone rubber adhesive, the preparation of auxiliary agents is solved by using aminosilane coupling agent and epoxy silane coupling agent, and the thermal stress and bonding problems of metal and resin-based composite materials in the spacecraft are achieved. Low density, high temperature performance and effective adhesiveness simplify process flow.

CN119019976APending Publication Date: 2024-11-26湖北航聚科技股份有限公司
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411104412.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The difference in thermal expansion coefficients of metal and resin-based composite materials in spacecraft leads to thermal stress crushing or tearing of rigid adhesives, resulting in structural failure, and effective bonding between silicone rubber and phenolic resin and epoxy resin is difficult to achieve.

Method used

Using two-component silicone rubber adhesive, including components A and components B, component A consists of silicone rubber base glue, reinforcement filler and light filler, component B consists of crosslinking agent, catalyst and coupling by aminosilane The additive is composed of the additive prepared by the agent and the epoxy silane coupling agent. The additive is prepared by the epoxy ring-opening reaction of the aminosilane coupling agent and the epoxy silane coupling agent to improve adhesion.

Benefits of technology

It realizes the low density and high temperature resistance of silicone rubber adhesives, can deep cure, realizes effective bonding with composite materials such as phenolic resins and epoxy resins, and realizes effective bonding between metal and silicone rubber without special treatment of metal surfaces. Connect, simplify the process flow and eliminate the differences in thermal deformation between different materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990313310000081
    Figure BDA0004990313310000081
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of high polymer materials, and discloses a double-component silicone rubber adhesive for bonding metal and resin and a preparation method of the double-component silicone rubber adhesive. The silicone rubber adhesive comprises a component A and a component B, wherein the component A comprises the following raw materials in parts by mass: 100 parts of silicone rubber base rubber, 10-40 parts of reinforcing filler and 5-15 parts of light filler; the component B comprises the following raw materials in parts by mass: 2-10 parts of a cross-linking agent, 0.1-1 part of a catalyst and 0.5-1.5 parts of an auxiliary agent; wherein the auxiliary agent is prepared through an epoxy ring-opening reaction of an amino silane coupling agent and an epoxy silane coupling agent. The silicone rubber adhesive can realize effective bonding of metal and a composite material, and is applied to spacecrafts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer material preparation, in particular to a two-component silicone rubber adhesive for bonding metal and resin and a preparation method thereof. Background Art

[0002] Resin-based composite materials are widely used in spacecraft due to their light weight, high strength and functional designability. Therefore, under the premise of meeting the bonding performance, the pursuit of lightweight spacecraft urgently requires the use of resin-based composite materials; however, for different parts of the spacecraft, especially the parts where metal and resin-based composite materials are used together, the thermal expansion coefficients of the two materials are quite different. The resulting thermal stress will crush or tear the rigid adhesive, thereby causing the spacecraft structure to fail.

[0003] Silicone rubber system is the best choice for low density and high strength requirements in high temperature environments above 200°C. Compared with single-component silicone rubber adhesives, two-component silicone rubber adhesives have the advantages of closed space curing and deep curing, but silicone rubber has low surface energy and small intermolecular forces, and cannot naturally form effective bonding with many materials. When silicone rubber is bonded to metal materials, effective bonding can be achieved through special treatments such as surface grinding and primer coating, but effective bonding between silicone rubber and composite materials such as phenolic resin and epoxy resin is difficult to achieve.

[0004] Therefore, it is necessary to provide a two-component silicone rubber adhesive for bonding metal and resin and a preparation method to solve the above problems. Summary of the invention

[0005] Based on the above, the purpose of the present invention is to provide a two-component silicone rubber adhesive for metal and resin bonding and a preparation method, so as to achieve effective bonding of metal and composite materials and be applied in spacecraft.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A two-component silicone rubber adhesive for bonding metal and resin, comprising component A and component B;

[0008] Component A includes the following raw materials in parts by weight: 100 parts of silicone rubber base, 10-40 parts of reinforcing filler, and 5-15 parts of lightweight filler;

[0009] Component B includes the following raw materials in parts by weight: 2-10 parts of a cross-linking agent, 0.1-1 parts of a catalyst, and 0.5-1.5 parts of an auxiliary agent;

[0010] The auxiliary agent is prepared by epoxy ring-opening reaction of an aminosilane coupling agent and an epoxysilane coupling agent.

[0011] As a preferred solution of a two-component silicone rubber adhesive for bonding metal and resin, the silicone rubber base adhesive includes α,ω-dihydroxypolydimethylsiloxane.

[0012] As a preferred solution of a two-component silicone rubber adhesive for bonding metal to resin, the reinforcing filler includes fumed silica.

[0013] As a preferred solution of a two-component silicone rubber adhesive for bonding metal to resin, the lightweight filler includes hollow glass microspheres.

[0014] As a preferred solution of a two-component silicone rubber adhesive for bonding metal and resin, the crosslinking agent includes one or more of tetraethyl orthosilicate, tetramethyl orthosilicate, and tetrapropyl orthosilicate.

[0015] As a preferred solution of a two-component silicone rubber adhesive for bonding metals and resins, the catalyst includes one or more of dibutyltin dilaurate, dimethyltin dilaurate, dioctyltin, and stannous isooctanoate.

[0016] As a preferred embodiment of a two-component silicone rubber adhesive for bonding metals and resins, the aminosilane coupling agent includes one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane.

[0017] As a preferred solution of a two-component silicone rubber adhesive for bonding metal and resin, the epoxysilane coupling agent includes one or both of 3-(2,3-epoxy)propyltrimethoxysilane and 3-(2,3-epoxy)propyltriethoxysilane.

[0018] As a preferred solution for a two-component silicone rubber adhesive for bonding metals and resins, the preparation method of the auxiliary agent specifically includes: mixing an aminosilane coupling agent and an epoxysilane coupling agent in a molar ratio of 1:(1-4), heating to 80°C-150°C, allowing the amine in the aminosilane coupling agent to undergo a ring-opening reaction with the epoxy group in the epoxysilane coupling agent, and stirring the reaction for 1h-4h.

[0019] A method for preparing a two-component silicone rubber adhesive for bonding metal and resin, which is used to prepare the two-component silicone rubber adhesive for bonding metal and resin as described in any one of the above, and the preparation method comprises the following steps:

[0020] Grind the silicone rubber base, add reinforcing filler and continue grinding, take out and disperse, add light filler, stir evenly, vacuum degas, and press out to obtain component A;

[0021] The cross-linking agent, catalyst and auxiliary agent are fully stirred to form component B;

[0022] The components A and B are fully mixed to obtain a two-component silicone rubber adhesive for bonding metals and resins.

[0023] The beneficial effects of the present invention are:

[0024] The invention provides a two-component silicone rubber adhesive for bonding metal and resin, which has low density and high temperature resistance. The adhesive also uses an auxiliary agent prepared by epoxy ring-opening reaction of an aminosilane coupling agent and an epoxysilane coupling agent to improve the adhesion of the silicone rubber adhesive. Therefore, the silicone rubber adhesive can be deeply cured to achieve effective bonding with composite materials such as phenolic resin and epoxy resin. At the same time, effective bonding with metal is achieved without special treatment of the metal surface, which greatly simplifies the process flow. The thermal deformation difference between different materials is eliminated by elastic deformation, and the adhesive is applied in the bonding of spacecraft metal and composite materials. DETAILED DESCRIPTION

[0025] For ease of understanding of the present invention, the present invention will be described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. Unless otherwise defined, all technical and scientific terms used in the present invention belong to the technical field of the present invention.

[0026] The present embodiment provides a two-component silicone rubber adhesive for bonding metal and resin, including component A and component B; component A includes the following raw materials in parts by mass: 100 parts of silicone rubber base glue, 10-40 parts of reinforcing filler, and 5-15 parts of lightweight filler; component B includes the following raw materials in parts by mass: 2-10 parts of cross-linking agent, 0.1-1 part of catalyst, and 0.5-1.5 parts of auxiliary agent; wherein the auxiliary agent is prepared by epoxy ring-opening reaction of aminosilane coupling agent and epoxysilane coupling agent. The silicone rubber adhesive has the characteristics of low density and high temperature resistance, realizes effective bonding of metal and composite materials, and is used in spacecraft.

[0027] This embodiment also provides a method for preparing a two-component silicone rubber adhesive for bonding metal and resin, the preparation method comprising the following steps:

[0028] Pour the silicone rubber base into the opened three-roll grinder, wait for the silicone rubber base to be evenly distributed on the first two rollers, add the reinforcing filler, grind and mix at least three times until the reinforcing filler is evenly dispersed in the silicone rubber base, take it out and transfer it to the planetary disperser, add the light filler, rotate at 20-35Hz, stir for 10-30min, vacuum degas for 30min, press out, seal and set aside as component A;

[0029] Add the weighed crosslinking agent, catalyst and auxiliary agent into the container, stir thoroughly with a mixer, seal and set aside as component B;

[0030] When it is needed, component A and component B are fully mixed to obtain a two-component silicone rubber adhesive for bonding metal and resin.

[0031] Specifically, the silicone rubber base includes α, ω-dihydroxypolydimethylsiloxane; the reinforcing filler includes fumed silica; the lightweight filler includes hollow glass microspheres; the cross-linking agent includes one or more of tetraethyl orthosilicate, tetramethyl orthosilicate, and tetrapropyl orthosilicate; and the catalyst includes one or more of dibutyltin dilaurate, dimethyltin dilaurate, dioctyltin, and stannous isooctanoate.

[0032] Specifically, the preparation method of the auxiliary agent includes: mixing an aminosilane coupling agent and an epoxysilane coupling agent in a molar ratio of 1:(1-4), heating to 80°C-150°C, allowing the amine in the aminosilane coupling agent to undergo a ring-opening reaction with the epoxy group in the epoxysilane coupling agent, stirring the reaction for 1h-4h, and sealing and placing in a cool place for standby use.

[0033] More specifically, the aminosilane coupling agent includes one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane; the epoxysilane coupling agent includes one or two of 3-(2,3-epoxy)propyltrimethoxysilane and 3-(2,3-epoxy)propyltriethoxysilane.

[0034] The present invention will be further described below by means of specific examples.

[0035] Example 1

[0036] A two-component silicone rubber adhesive for bonding metals and resins comprises the following raw materials in parts by mass: 100 parts of α,ω-dihydroxypolydimethylsiloxane, 30 parts of fumed silica, 8 parts of hollow glass microspheres, 5 parts of tetraethyl orthosilicate, 0.5 parts of dibutyltin dilaurate, and 1 part of an auxiliary agent; wherein the raw materials for preparing the auxiliary agent include N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and 3-(2,3-epoxy)propyltrimethoxysilane.

[0037] A method for preparing a two-component silicone rubber adhesive for bonding metal and resin comprises:

[0038] Preparation of the auxiliary agent: N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and 3-(2,3-epoxy)propyltrimethoxysilane were mixed in a molar ratio of 1:3, heated to 80°C, stirred for reaction for 1 hour, and sealed and placed in a cool place for use;

[0039] Preparation of component A: Weigh each raw material according to the weight ratio, pour 100 parts of α, ω-dihydroxy polydimethylsiloxane into an open three-roll mill, wait until α, ω-dihydroxy polydimethylsiloxane is evenly distributed on the first two rollers, then gradually add 30 parts of fumed silica, grind and mix three to four times until the fumed silica is fully and evenly dispersed in the silica gel, take it out, transfer it to a planetary dispersion center, add 8 parts of hollow glass microspheres, rotate at 35 Hz, stir for 30 minutes, vacuum degas for 30 minutes, press out, seal and set aside;

[0040] Preparation of component B: weigh the raw materials according to the weight ratio, add 5 parts of tetraethyl orthosilicate, 0.5 parts of dibutyltin dilaurate, and 0.5 parts of the auxiliary agent into a container, stir thoroughly with a mixer, and seal for later use;

[0041] The obtained components A and B were fully mixed and cured at room temperature for 7 days.

[0042] Example 2

[0043] A two-component silicone rubber adhesive for bonding metals and resins comprises the following raw materials in parts by mass: 100 parts of α,ω-dihydroxypolydimethylsiloxane, 10 parts of fumed silica, 5 parts of hollow glass microspheres, 2 parts of tetramethyl orthosilicate, dioctyltin, and 0.5 parts of an auxiliary agent; wherein the raw materials for preparing the auxiliary agent include γ-aminopropyltrimethoxysilane and 3-(2,3-epoxy)propyltriethoxysilane.

[0044] A method for preparing a two-component silicone rubber adhesive for bonding metal and resin comprises:

[0045] Preparation of the auxiliary agent: γ-aminopropyltrimethoxysilane and 3-(2,3-epoxy)propyltriethoxysilane were mixed in a molar ratio of 1:1, heated to 115°C, stirred for reaction for 2.5 hours, and sealed and placed in a cool place for later use;

[0046] Preparation of component A: Weigh each raw material according to the weight ratio, pour 100 parts of α, ω-dihydroxy polydimethylsiloxane into an open three-roll mill, wait until α, ω-dihydroxy polydimethylsiloxane is evenly distributed on the first two rollers, then gradually add 10 parts of fumed silica, grind and mix three to four times until the fumed silica is fully and evenly dispersed in the silica gel, take it out, transfer it to a planetary dispersion center, add 5 parts of hollow glass microspheres, rotate at 20 Hz, stir for 10 minutes, vacuum degas for 30 minutes, press out, seal and set aside;

[0047] Preparation of component B: weigh the raw materials according to the weight ratio, add 2 parts of tetraethyl orthosilicate, 0.1 parts of dibutyltin dilaurate, and 0.1 parts of the auxiliary agent into a container, stir thoroughly with a mixer, and seal for later use;

[0048] The obtained components A and B were fully mixed and cured at room temperature for 7 days.

[0049] Example 3

[0050] A two-component silicone rubber adhesive for bonding metals and resins comprises the following raw materials in parts by mass: 100 parts of α,ω-dihydroxypolydimethylsiloxane, 40 parts of fumed silica, 15 parts of hollow glass microspheres, 10 parts of tetrapropyl orthosilicate, 1 part of stannous isooctanoate, and 1.5 parts of an auxiliary agent; wherein the raw materials for preparing the auxiliary agent comprise N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane and 3-(2,3-epoxy)propyltrimethoxysilane.

[0051] A method for preparing a two-component silicone rubber adhesive for bonding metal and resin comprises:

[0052] Preparation of the auxiliary agent: N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane and 3-(2,3-epoxy)propyltrimethoxysilane were mixed in a molar ratio of 1:4, heated to 150°C, stirred for reaction for 4 hours, and sealed and placed in a cool place for use;

[0053] Preparation of component A: Weigh each raw material according to the weight ratio, pour 100 parts of α, ω-dihydroxy polydimethylsiloxane into an open three-roll mill, wait until α, ω-dihydroxy polydimethylsiloxane is evenly distributed on the first two rollers, then gradually add 40 parts of fumed silica, grind and mix three to four times until the fumed silica is fully and evenly dispersed in the silica gel, take it out, transfer it to a planetary dispersion center, add 15 parts of hollow glass microspheres, rotate at 25 Hz, stir for 20 minutes, vacuum degas for 30 minutes, press out, seal and set aside;

[0054] Preparation of component B: weigh the raw materials according to the weight ratio, add 10 parts of tetraethyl orthosilicate, 1 part of dibutyltin dilaurate, and 1 part of the auxiliary agent into a container, stir thoroughly with a mixer, and seal for later use;

[0055] The obtained components A and B were fully mixed and cured at room temperature for 7 days.

[0056] In order to further illustrate the key points of this patent, a comparative case is added for illustration.

[0057] Comparative Example 1

[0058] A two-component silicone rubber adhesive for bonding metal and resin, comprising the following raw materials in parts by weight: 100 parts of α,ω-dihydroxy polydimethylsiloxane, 30 parts of fumed silica, 8 parts of hollow glass microspheres, 5 parts of tetraethyl orthosilicate, 0.5 parts of dibutyltin dilaurate, and 1 part of γ-aminopropyltriethoxysilane

[0059] A method for preparing a two-component silicone rubber adhesive for bonding metal and resin comprises:

[0060] Preparation of component A: Weigh each raw material according to the weight ratio, pour 100 parts of α, ω-dihydroxy polydimethylsiloxane into an open three-roll mill, wait until α, ω-dihydroxy polydimethylsiloxane is evenly distributed on the first two rollers, then gradually add 30 parts of fumed silica, grind and mix three to four times until the fumed silica is fully and evenly dispersed in the silica gel, take it out, transfer it to a planetary dispersion center, add 8 parts of hollow glass microspheres, rotate at 35 Hz, stir for 30 minutes, vacuum degas for 30 minutes, press out, seal and set aside;

[0061] Preparation of component B: weigh the raw materials according to the weight ratio, add 5 parts of tetraethyl orthosilicate, 0.5 parts of dibutyltin dilaurate, and 0.5 parts of γ-aminopropyltriethoxysilane into a container, stir thoroughly with a stirrer, and seal for later use;

[0062] The obtained components A and B were fully mixed and cured at room temperature for 7 days.

[0063] The performance tests were performed on the silicone rubber adhesives prepared in Examples 1-3 and Comparative Example 1. The test results are shown in Table 1.

[0064] Test method: Clean the substrate specimens to be bonded (such as the aluminum alloy sheet, epoxy resin sheet and phenolic resin sheet) with acetone. After the solvent dries naturally, prepare shear pieces according to GB / T 13936-2014 Determination of tensile shear strength of bonding between vulcanized rubber and metal. Curing at room temperature for 7 days, test. The size of the aluminum alloy, epoxy resin and phenolic resin bonding specimens used is 2×100×25mm. According to the "1A type" dumbbell sample described in GB / T528-2009, the dumbbell-shaped specimens are punched out to test the tensile strength. The density is tested according to method A in GB / T 533-2008. The aluminum alloy shear specimens are heat treated at 200℃ and 300℃ for 10 minutes, and then the shear strength is tested.

[0065] Table 1 Silicone rubber adhesive performance test

[0066]

[0067] It can be seen from the above table that the silicone rubber adhesives prepared in Examples 1-3 have a low density and excellent high temperature resistance and tensile strength, and excellent bonding performance with metals and composite materials; comparing Example 1 with Comparative Example 1, Comparative Example 1 only uses γ-aminopropyltriethoxysilane as an auxiliary agent, and it can be obtained that when the auxiliary agent is not prepared by the epoxy ring-opening reaction of an aminosilane coupling agent and an epoxysilane coupling agent, the silicone rubber adhesive prepared in Comparative Example 1 has poor bonding performance, high temperature resistance, and tensile strength with metals and composite materials.

[0068] Therefore, the silicone rubber adhesive prepared by the present application has a low density and excellent high temperature resistance and tensile strength, can achieve effective bonding of metals and composite materials, and is used in spacecraft.

[0069] The above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention is described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.

Claims

1. A two-component silicone rubber adhesive for bonding metal and resin, characterized in that: It includes component A and component B; Component A includes the following raw materials in parts by weight: 100 parts of silicone rubber base, 10-40 parts of reinforcing filler, and 5-15 parts of lightweight filler; Component B includes the following raw materials in parts by weight: 2-10 parts of a cross-linking agent, 0.1-1 parts of a catalyst, and 0.5-1.5 parts of an auxiliary agent; The auxiliary agent is prepared by epoxy ring-opening reaction of an aminosilane coupling agent and an epoxysilane coupling agent.

2. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The silicone rubber base glue includes α,ω-dihydroxy polydimethylsiloxane.

3. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The reinforcing filler includes fumed silica.

4. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The lightweight filler includes hollow glass microspheres.

5. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The crosslinking agent includes one or more of tetraethyl orthosilicate, tetramethyl orthosilicate, and tetrapropyl orthosilicate.

6. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The catalyst includes one or more of dibutyltin dilaurate, dimethyltin dilaurate, dioctyltin, and stannous isooctanoate.

7. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The aminosilane coupling agent includes one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane.

8. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The epoxysilane coupling agent includes one or two of 3-(2,3-epoxy)propyltrimethoxysilane and 3-(2,3-epoxy)propyltriethoxysilane.

9. The two-component silicone rubber adhesive for bonding metal and resin according to claim 1, characterized in that: The preparation method of the auxiliary agent specifically comprises: mixing an aminosilane coupling agent and an epoxysilane coupling agent in a molar ratio of 1:(1-4), heating to 80°C-150°C, allowing the amine in the aminosilane coupling agent to undergo a ring-opening reaction with the epoxy group in the epoxysilane coupling agent, and stirring the reaction for 1h-4h.

10. A method for preparing a two-component silicone rubber adhesive for bonding metal and resin, for preparing the two-component silicone rubber adhesive for bonding metal and resin according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: Grind the silicone rubber base, add reinforcing filler and continue grinding, take out and disperse, add light filler, stir evenly, vacuum degas, and press out to obtain component A; The cross-linking agent, catalyst and auxiliary agent are fully stirred to form component B; The components A and B are fully mixed to obtain a two-component silicone rubber adhesive for bonding metals and resins.

Citation Information

Cited By

  • Binder for bonding metal and silicone rubber as well as preparation method and application of binder

    CN119709119A

  • Adhesive for internal thermal insulation layer of solid rocket engine as well as preparation method and application of adhesive

    CN120173554A

  • Adhesive for thermal insulation layer in solid rocket engine, preparation method and application thereof

    CN120173554B

  • Interface coupling agent for composite insulator and preparation method thereof

    CN122060440A