Nickel-based compound-amorphous chromium family heterojunction self-supporting electrode and preparation method and application thereof
By forming a nickel-based compound-amorphous chromium group heterojunction self-supporting electrode on carbon cloth fibers, the problem of limited hybridization methods of existing nickel-based compound-based heterostructure is solved, the catalytic efficiency and durability are improved, and the catalytic efficiency and durability are achieved. Efficient catalysis of hydrogen electrolysis reaction.
Patent Information
- Application Number
- CN202410996057.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing hybridization and synergistic methods of nickel-based compound-based heterostructures are limited, resulting in low density of catalytic active sites and low catalytic efficiency.
Using a nickel-based compound-amorphous chromium group heterojunction self-supporting electrode, amorphous nanocrystalline-amorphous chromium group heterojunction thin layer is covered on carbon cloth fibers, and amorphous is formed by electrodeposition and annealing conversion method. The heterojunction structure of nickel-based compounds and chromium group metals increases catalytic activity sites and improves electrocatalytic stability.
It improves the catalytic efficiency of hydrogen electrolytic reaction (HER) and its durability in electrolytes, provides a more flexible hybridization method and higher electrocatalytic stability, and is suitable for industrial production.
Smart Images

Figure CN119020806A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalytic materials, and in particular relates to a nickel-based compound-amorphous chromium heterojunction self-supporting electrode and a preparation method and application thereof. Background Art
[0002] As a zero-carbon energy with high calorific value and clean and pollution-free, hydrogen plays an important role in energy transformation. The production of hydrogen by water electrolysis has the advantages of safety, environmental protection, scale control, and high product purity. However, the hydrogen evolution reaction (HER) by water electrolysis is limited by slow reaction kinetics and requires high-performance catalytic electrodes. Although precious metal platinum-based materials have high HER electrocatalytic activity, their low stability and high cost make it difficult to achieve large-scale application. Nickel-based materials are widely used because of their multiple chemical states, excellent electron donation and acceptance capabilities, and low price. However, single-phase nickel-based compounds have problems such as insufficient number of active sites and lack of controllability as electrocatalysts. Therefore, by introducing other components and constructing heterostructures, the purpose of increasing the active site density and regulating the electronic structure is achieved.
[0003] The method disclosed in the document entitled "A nickel foam with heterojunction nanosheets grown on the surface and its preparation method and application" with Chinese patent application number 202210504090.2 grows crystal-crystallized heterojunction nanosheets of NiO and Ni3S2 on the surface of nickel foam, which is applied to lithium-sulfur batteries. The document entitled "A nickel compound-phosphide sub-nanometer hybrid self-supporting electrode, preparation method and application" with Chinese patent application number 202410798698.X discloses a nickel compound-phosphide sub-nanometer hybrid self-supporting electrode with dual-functional catalytic properties of hydrogen evolution and oxygen evolution, heat-treated under different atmospheres to make the amorphous thin layer in situ crystallize and transform, and obtain different nickel compound-phosphide sub-nanometer hybrid structures. A simple chemical plating-heat treatment method is used to cover the surface of carbon cloth fiber with an amorphous nickel-phosphide thin layer, and then in situ crystallization and transformation in different anion source atmospheres, thereby obtaining a series of heterogeneous thin layers of nickel compounds and phosphides in sub-nanometer hybrid. However, the nickel-based compound-based heterostructure disclosed in the above two patent documents is a crystal-crystal heterojunction composed of different compound grains. The fixed crystal structure of the crystalline material limits the hybridization and synergy between the heterogeneous components. Therefore, the density of catalytic active sites is still low and the catalytic efficiency is not high. Summary of the invention
[0004] The purpose of the present invention is to solve the problem of limited hybridization and synergistic modes of existing nickel-based compound-based heterostructures of crystalline-crystalline heterojunctions, and to provide a nickel-based compound-amorphous chromium family heterojunction self-supporting electrode and a preparation method thereof. The prepared amorphous self-supporting electrode can improve catalytic efficiency and durability in electrolyte; the present invention also provides applications of the self-supporting electrode.
[0005] To achieve the above-mentioned purpose, the technical solution adopted by the nickel-based compound-amorphous chromium heterojunction self-supporting electrode provided by the present invention is: it is composed of a nickel-based compound nanocrystal-amorphous chromium heterojunction thin layer covered on carbon cloth fiber, the nickel-based compound component is nickel disulfide or nickel sulfide or nickel diselenide or nickel phosphide or nickel nitride or nickel oxide, and the amorphous chromium component is chromium or molybdenum or tungsten.
[0006] The technical solution adopted by the method for preparing a nickel-based compound-amorphous chromium heterojunction self-supporting electrode provided by the present invention comprises the following steps:
[0007] (1) firstly introduce active groups on the surface of carbon cloth fiber, then wash with deionized water until the cleaning solution becomes neutral and then dry;
[0008] (2) using a nickel-chromium plating solution, a nickel-molybdenum plating solution, or a nickel-tungsten plating solution as an electrolyte, and using an electrodeposition method to cover a layer of nickel-chromium, nickel-molybdenum, or nickel-tungsten thin layer having amorphous characteristics on the surface of the dried carbon cloth fiber to obtain an amorphous nickel-chromium group metal / carbon cloth;
[0009] (3) placing the amorphous nickel-chromium metal / carbon cloth downstream of a quartz boat, placing sublimated sulfur or selenium powder or sodium hypophosphite upstream of the quartz boat, and then placing the quartz boat in a tube furnace, heating and keeping the temperature in nitrogen or argon, so as to convert the amorphous nickel on the surface of the carbon cloth into nickel disulfide or nickel sulfide or nickel diselenide or nickel phosphide nanocrystals, while chromium or molybdenum or tungsten still exists in an amorphous form;
[0010] Alternatively: the amorphous nickel-chromium metal / carbon cloth is placed in a quartz boat, the quartz boat is placed in a tube furnace, the temperature is increased and kept in ammonia or air, the amorphous nickel on the surface of the carbon cloth is converted into nickel nitride or nickel oxide nanocrystals, and the chromium, molybdenum or tungsten still exists in an amorphous form.
[0011] Preferably, the formula of the nickel-chromium plating solution described in step (2) is: 1g NiSO4·6H2O, 1g NiCl2·6H2O, 9.6g CrCl3·6H2O, 7.7g C6H8O7, 10.7g Na3C6H5O7, 6.2g H3BO3, 0.02g CH3(CH2) 11OSO3Na and 100mL deionized water; the formula of the nickel-molybdenum plating solution is: 3g Na2MoO4·2H2O, 6g NiSO4·6H2O, 2mL NH3·H2O, 8g Na3C6H5O7·2H2O, 2g NiCl·6H2O and 100mL deionized water; the formula of the nickel-tungsten plating solution is 2.6gNiSO4·6H2O, 0.48g NiCl2·6H2O, 6.6~19.8g Na2WO4·2H2O, 12.9g Na3C6H5O7, 3.1g H3BO3 and 100mL deionized water.
[0012] The technical solution adopted by the application of a nickel-based compound-amorphous chromium-based heterojunction self-supporting electrode provided by the present invention is: the nickel-based compound-amorphous chromium-based heterojunction self-supporting electrode is applied to a hydrogen evolution reaction electrocatalyst.
[0013] Compared with the prior art, the present invention has the following significant advantages and beneficial effects:
[0014] 1. Compared with existing crystalline materials, the amorphous state in the nickel-based compound-amorphous chromium heterojunction self-supporting electrode provided by the present invention has the advantages of easy reconstruction and adjustable denaturation. If one of the components of the heterojunction is amorphous, it can hybridize with different crystal planes of the crystalline component without being restricted by lattice mismatch, and the hybridization method is more flexible; in addition, the amorphous component is often dense and corrosion-resistant, which makes the material have higher electrocatalytic stability.
[0015] 2. The present invention proposes a simple and efficient electrodeposition-annealing conversion method to obtain a series of nickel-based compound-amorphous chromium family heterojunction self-supporting electrodes (including nickel disulfide-amorphous chromium / carbon cloth, nickel disulfide-amorphous molybdenum / carbon cloth, nickel sulfide-amorphous tungsten, nickel diselenide-amorphous chromium / carbon cloth, nickel diselenide-amorphous molybdenum / carbon cloth, nickel diselenide-amorphous tungsten / carbon cloth, nickel phosphide-amorphous chromium / carbon cloth, nickel phosphide-amorphous molybdenum / carbon cloth, nickel phosphide-amorphous tungsten / carbon cloth Nickel-amorphous tungsten / carbon cloth, nickel nitride-amorphous chromium / carbon cloth, nickel nitride-amorphous molybdenum / carbon cloth, nickel nitride-amorphous tungsten / carbon cloth, nickel oxide-amorphous chromium / carbon cloth, nickel oxide-amorphous molybdenum / carbon cloth, nickel oxide-amorphous tungsten / carbon cloth). Since the nickel-chromium group metals obtained by electrodeposition are in an amorphous form, annealing treatment in different atmospheres occurs in situ transformation from bottom to top, so the size of the formed nickel-based compound nanocrystals is very small.
[0016] 3. The present invention makes full use of the difference in crystallization transformation temperature between nickel and chromium group metals. By performing a simple annealing treatment at an appropriate temperature, a crystalline-amorphous heterojunction can be obtained from the amorphous coating. Compared with the traditional method of preparing a crystalline-amorphous heterojunction, it is simpler, more efficient and has universal applicability.
[0017] 4. Compared with traditional nickel-based heterogeneous materials, the material prepared by the present invention greatly increases the catalytic active sites, improves the HER catalytic efficiency and durability in the electrolyte, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is the SEM image of Ni-Mo / CC-700 in Example 1;
[0019] Figure 2 TEM image and selected area electron diffraction pattern of the Ni-Mo / CC-700 surface thin layer in Example 1, wherein a is a TEM image and b is a selected area electron diffraction pattern;
[0020] Figure 3 is the XRD spectrum of Ni-Mo / CC-700 in Example 1;
[0021] Figure 4 1 mol L Ni-Mo / CC-700 in N2 saturated solution in Example 1 -1 HER polarization curve in KOH electrolyte;
[0022] Figure 5 is the SEM image of Ni3N-a-Mo / CC-700 in Example 1;
[0023] Figure 6 This is a high-magnification TEM image of the surface thin layer of Ni3N-a-Mo / CC-700 in Example 1;
[0024] Figure 7 This is the selected area electron diffraction pattern of the Ni3N-a-Mo / CC-700 surface thin layer in Example 1;
[0025] Figure 8 is the XRD spectrum of Ni3N-a-Mo / CC-700 in Example 1;
[0026] Fig. 9 The XPS spectra of Ni3N-a-Mo / CC-700 in Example 1, wherein Figure a is the full XPS spectrum of Ni3N-a-Mo / CC-700, Figure b is the Ni 2p high-resolution spectrum, Figure c is the Mo 3d high-resolution spectrum, and Figure d is the N1s high-resolution spectrum;
[0027] Fig.10 1 mol L Ni3N-a-Mo / CC-700 in N2 saturated solution in Example 1 -1 HER polarization curve in KOH electrolyte;
[0028] Fig.11This is a curve showing the change of current over time when Ni3N-a-Mo / CC-700 is tested at a constant potential of -0.07V vs. RHE in Example 1;
[0029] Fig.12 is the SEM image of Ni-Mo / CC-300 in Example 2;
[0030] Fig.13 1 mol L Ni-Mo / CC-300 in N2 saturated solution in Example 2 -1 HER polarization curve in KOH electrolyte;
[0031] Fig.14 is the SEM image of Ni-Mo / CC-1100 in Example 3;
[0032] Fig.15 1 mol L Ni-Mo / CC-1100 in N2 saturated solution in Example 3 -1 HER polarization curve in KOH electrolyte;
[0033] Fig.16 NiS in Example 4 x -SEM image of a-Mo / CC;
[0034] Fig.17 NiS in Example 4 x -XRD spectrum of a-Mo / CC;
[0035] Fig.18 NiS in Example 4 x -a-Mo / CC in N2 saturated 1 mol L -1 HER polarization curve in KOH electrolyte;
[0036] Fig.19 is the SEM image of NiSe2-a-Mo / CC in Example 5;
[0037] Fig. 20 is the XRD spectrum of NiSe2-a-Mo / CC in Example 5;
[0038] Fig.21 1 mol L NiSe2-a-Mo / CC in N2 saturated solution in Example 5 -1 HER polarization curve in KOH electrolyte;
[0039] Fig. 22 is the SEM image of Ni2P-a-Mo / CC in Example 6;
[0040] Fig.23is the XRD spectrum of Ni2P-a-Mo / CC in Example 6;
[0041] Fig.24 1 mol L Ni2P-a-Mo / CC in N2 saturated solution in Example 6 -1 HER polarization curve in KOH electrolyte;
[0042] Fig.25 is the SEM image of NiO-a-Mo / CC in Example 7;
[0043] Fig.26 is the XRD spectrum of NiO-a-Mo / CC in Example 7;
[0044] Fig. 27 1 mol L NiO-a-Mo / CC in N2 saturated solution in Example 7 -1 HER polarization curve in KOH electrolyte;
[0045] Fig.28 : The SEM images of Ni-W / CC-0.4 in Example 8, wherein Figure a is a low-magnification SEM image, and Figure b is a high-magnification SEM image;
[0046] Fig.29 TEM image and selected area electron diffraction pattern of the surface thin layer of Ni-W / CC-0.4 in Example 8, wherein Figure a is a TEM image and Figure b is a selected area electron diffraction pattern;
[0047] Fig.30 is the XRD spectrum of Ni-W / CC-0.4 in Example 8;
[0048] Fig.31 1 mol L Ni-W / CC-0.4 in N2 saturated solution in Example 8 -1 HER polarization curve in KOH electrolyte;
[0049] Fig.32 The SEM images of Ni3N-aW / CC-0.4 in Example 8, wherein Figure a is a low-magnification SEM image and Figure b is a high-magnification SEM image;
[0050] Fig.33 TEM image and selected area electron diffraction pattern of the surface thin layer of Ni3N-aW / CC-0.4 in Example 8, wherein Figure a is a TEM image and Figure b is a selected area electron diffraction pattern;
[0051] Fig.34 is the XRD spectrum of Ni3N-aW / CC-0.4 in Example 8;
[0052] Fig.35The XPS spectra of Ni3N-aW / CC-0.4 in Example 8, wherein Figure a is the full XPS spectrum of Ni3N-aW / CC-0.4, Figure b is the Ni 2p high-resolution spectrum, Figure c is the W 4f high-resolution spectrum, and Figure d is the N1s high-resolution spectrum;
[0053] Fig.36 1 mol L Ni3N-aW / CC-0.4 in N2 saturated solution in Example 8 -1 HER polarization curve in KOH electrolyte;
[0054] Fig.37 This is a curve showing the change of current over time when Ni3N-aW / CC-0.4 is tested at a constant potential of -0.07V vs. RHE in Example 8;
[0055] Fig.38 1 mol L Ni-W / CC-0.2 in N2 saturated solution in Example 9 -1 HER polarization curve in KOH electrolyte;
[0056] Fig.39 1 mol L Ni-W / CC-0.6 in N2 saturated solution in Example 10 -1 HER polarization curve in KOH electrolyte;
[0057] Fig.40 NiS in Example 11 x -SEM image of aW / CC;
[0058] Fig.41 NiS in Example 11 x -XRD spectrum of aW / CC;
[0059] Fig.42 NiS in Example 11 x -aW / CC in N2 saturated 1 mol L -1 HER polarization curve in KOH electrolyte;
[0060] Fig.43 is the SEM image of NiSe2-aW / CC in Example 12;
[0061] Fig.44 is the XRD spectrum of NiSe2-aW / CC in Example 12;
[0062] Fig.45 1 mol L NiSe2-aW / CC in N2 saturated solution in Example 12 -1 HER polarization curve in KOH electrolyte;
[0063] Fig.46 is the SEM image of Ni2P-aW / CC in Example 13;
[0064] Fig.47 is the XRD spectrum of Ni2P-aW / CC in Example 13;
[0065] Fig.48 1 mol L Ni2P-aW / CC in N2 saturated solution in Example 13 -1 HER polarization curve in KOH electrolyte;
[0066] Fig.49 is the SEM image of NiO-aW / CC in Example 14;
[0067] Fig.50 is the XRD spectrum of NiO-aW / CC in Example 14;
[0068] Fig.51 1 mol L NiO-aW / CC in N2 saturated solution in Example 14 -1 HER polarization curve in KOH electrolyte;
[0069] Fig.52 is the SEM image of Ni-Cr / CC in Example 15;
[0070] Fig.53 is the XRD spectrum of Ni3N-a-Cr / CC in Example 15;
[0071] Fig.54 1 mol L Ni3N-a-Cr / CC in N2 saturated solution in Example 15 -1 HER polarization curve in KOH electrolyte. DETAILED DESCRIPTION
[0072] The nickel-based compound-amorphous chromium heterojunction self-supporting electrode provided by the present invention is composed of a nickel-based compound nanocrystal-amorphous chromium heterojunction thin layer covered on a carbon cloth fiber, and the thickness of the thin layer is 0.2 to 1 micron; wherein the nickel-based compound component is nickel disulfide or nickel sulfide or nickel diselenide or nickel phosphide or nickel nitride or nickel oxide, and the nanocrystal size is 5-10 nanometers; the amorphous chromium component is chromium or molybdenum or tungsten.
[0073] The method for preparing the above-mentioned nickel-based compound-amorphous chromium family heterojunction self-supporting electrode is to first cover a layer of amorphous nickel-chromium or nickel-molybdenum or nickel-tungsten thin layer on the surface of carbon cloth fiber by electrodeposition method; then heat treat under different atmospheres to convert amorphous nickel into different nickel-based compound nanocrystals, while the chromium family elements still exist in amorphous form, thereby obtaining different nickel-based compound-amorphous chromium family heterostructures, specifically:
[0074] (1) Preparation of amorphous nickel-chromium thin layer on carbon cloth fiber
[0075] The carbon cloth is immersed in a nitric acid or sulfuric acid or a sulfuric acid and nitric acid mixed solution with a mass fraction of 10% to 15% to introduce active groups on the fiber surface to improve the hydrophilicity; it is then washed with deionized water until the washing solution is neutral, and then dried for use; an electrodeposition method is adopted, in which a nickel-chromium plating solution, a nickel-molybdenum plating solution or a nickel-tungsten plating solution is used as an electrolyte to cover a layer of nickel-chromium or nickel-molybdenum or nickel-tungsten thin layer with amorphous characteristics on the surface of the carbon cloth fiber to obtain an amorphous nickel-chromium group metal / carbon cloth.
[0076] (2) Preparation of nickel-based compound-amorphous chromium heterojunction thin layer on carbon cloth fiber
[0077] The amorphous nickel-chromium group metal / carbon cloth obtained in step (1) is placed downstream of the quartz boat, and sublimated sulfur or selenium powder or sodium hypophosphite is placed upstream, and the ratio of the mass of the sublimated sulfur or selenium powder or sodium hypophosphite to the area of the amorphous nickel-chromium group metal / carbon cloth is 0.05-0.1 g cm -2 ; Place the quartz boat in a tube furnace, heat it to 450-500°C in nitrogen or argon, and keep it warm for 1-3 hours to convert the amorphous nickel on the surface of the carbon cloth into nickel disulfide or nickel sulfide or nickel diselenide or nickel phosphide nanocrystals, while the difficult-to-crystallize chromium, molybdenum or tungsten still exists in an amorphous form.
[0078] Alternatively: placing the amorphous nickel-chromium metal / carbon cloth obtained in step (1) in a quartz boat; placing the quartz boat in a tube furnace, heating it to 450-500° C. in ammonia or air, and keeping it warm for 1-3 hours, so as to convert the amorphous nickel on the surface of the carbon cloth into nickel nitride or nickel oxide nanocrystals, while the difficult-to-crystallize chromium, molybdenum or tungsten still exists in an amorphous form.
[0079] Preferably, the electrodeposition method in step (1) refers to a constant potential deposition method or a cyclic voltammetric deposition method; wherein the deposition potential of the constant potential deposition is -1.0 to 1.5 V vs. Hg / HgO, and the deposition time is 300 to 1100 s; the potential range of the cyclic voltammetric deposition is -1.2 to -1.6 V vs. Hg / HgO, and the deposition time is 60 to 100 min.
[0080] Preferably, the nickel-chromium plating solution in step (1) is formulated as follows: 1 g NiSO4·6H2O, 1 g NiCl2·6H2O, 9.6 g CrCl3·6H2O, 7.7 g C6H8O7, 10.7 g Na3C6H5O7, 6.2 g H3BO3, 0.02 g CH3(CH2) 11OSO3Na and 100mL deionized water. ; Nickel-molybdenum plating solution formula is: 3g Na2MoO4·2H2O, 6g NiSO4·6H2O, 2mL NH3·H2O, 8gNa3C6H5O7·2H2O, 2g NiCl·6H2O and 100mL deionized water; nickel-tungsten plating solution formula is 2.6g NiSO4·6H2O, 0.48g NiCl2·6H2O, 6.6-19.8g Na2WO4·2H2O, 12.9g Na3C6H5O7, 3.1g H3BO3 and 100mL deionized water.
[0081] The application direction of the nickel-based compound-amorphous chromium heterojunction self-supporting electrode prepared by the above method is: electrocatalytic hydrogen evolution reaction, applied to hydrogen evolution reaction electrocatalyst, which can improve HER catalytic efficiency and durability in electrolyte.
[0082] In order to better understand the essence of the present invention, the present invention is further described below in combination with 15 examples: Example 1: Preparation, Characterization and Performance Testing of Nickel Nitride-Amorphous Molybdenum / Carbon Cloth (Ni3N-a-Mo / CC-700)
[0083] (1) Preparation, characterization and testing of amorphous nickel-molybdenum / carbon cloth (Ni-Mo / CC-700)
[0084] The carbon cloth was cut into 2 cm*1 cm rectangles and soaked in a mixed solution of 10% nitric acid and 10% sulfuric acid (volume ratio of nitric acid to sulfuric acid was 3:1) for 12 h. It was then washed with deionized water until the washing solution was neutral and dried at 40 °C for 8 h. The Ni-Mo / CC precursor was prepared by constant potential deposition. During the synthesis, the pretreated carbon cloth was used as the working electrode, Hg / HgO electrode (1 mol L -1 KOH solution) as the reference electrode and the carbon rod as the counter electrode. The electrolyte consisted of 3g Na2MoO4·2H2O, 6g NiSO4·6H2O, 2mL NH3·H2O, 8gNa3C6H5O7·2H2O, 2gNiCl·6H2O and 100mL deionized water. The electrodeposition was performed at a potential of -1.5V vs.Hg / HgO for 700s by constant potential method. After the deposition, the working electrode was washed with deionized water and dried in an oven at 40°C for 8h. According to the electrodeposition time, the sample was labeled as Ni-Mo / CC-700.
[0085] Figure 1 This is the SEM image of Ni-Mo / CC-700, showing that the surface of the carbon cloth fiber is evenly covered with a nickel-molybdenum coating; Figure 2Figure a is a TEM image, and figure b is a selected area electron diffraction result. No lattice fringes or crystal diffraction patterns were found, proving that the surface coating is indeed amorphous. Figure 3 The XRD spectrum shows that only two mantou peaks of the carbon cloth substrate are observed, and no other crystal diffraction peaks are observed; Figure 4 HER polarization curve of Ni-Mo / CC-700 at 10 mA cm -2 The overpotential at this current density is 132 mV.
[0086] (2) Preparation, characterization and performance testing of nickel nitride-amorphous molybdenum / carbon cloth (Ni3N-a-Mo / CC-700)
[0087] The Ni-Mo / CC-700 obtained in step (1) is placed in a quartz boat, which is placed in a tube furnace, heated to 500°C in ammonia, and kept warm for 2 hours to convert the amorphous nickel on the surface of the carbon cloth into nickel nitride nanocrystals, while the difficult-to-crystallize molybdenum still exists in an amorphous form, thereby obtaining Ni3N-a-Mo / CC-700.
[0088] Figure 5 This is a SEM image, which shows that the coating still evenly covers the surface of the carbon cloth fiber after nitridation treatment; Figure 6 This is a high-magnification TEM image, where the crystalline and amorphous regions are clearly visible. The size of the crystalline region is 5-10 nm, and the composition is Ni3N, while the amorphous region is amorphous Mo (a-Mo); Figure 7 The selected area electron diffraction further proved that the crystal structure of the crystalline part corresponds to the Ni3N phase; Figure 8 is the XRD spectrum, and the signal is in good agreement with the standard signal of Ni3N (PDF#89-5144); Fig. 9 Figure a is the full XPS spectrum of the Ni3N-a-Mo / CC-700 catalyst, which confirms the presence of Ni, Mo, C, N and O elements, among which the O element can be attributed to surface oxidation after exposure to air. Fig. 9 Figure b is a Ni 2p fine spectrum, which can fit the Ni 2p of different valence states. 3 / 2 , Ni 2p 1 / 2 and the corresponding satellite peaks; Fig. 9 Figure c is the fine spectrum of Mo 3d, which can be fitted to get Mo 3+ (229.29eV and 232.69eV), Mo 5+ (230.29.3eV and 233.99eV) and Mo 6+ The different oxidation states (232.09 eV and 235.49 eV) are due to surface oxidation. Fig. 9Figure d in the figure is the N1 s fine spectrum. The peak at 399.39 eV corresponds to the NH group. At 395.29 eV and 397.59 eV, the fitted peaks of N1 s are close to the Mo-N bond and Ni-N bond, respectively. Fig.10 This is the HER polarization curve of Ni3N-a-Mo / CC-700. Only 70mV overpotential is required to obtain 10mAcm -2 The current density of 2.5 Å indicates its excellent electrocatalytic hydrogen evolution performance. Fig.11 This is the time-current curve under 70mV overpotential. It can be seen that the current of the catalytic electrode has almost no decay after 20h of continuous operation, proving its excellent stability.
[0089] Example 2: Preparation, Characterization and Performance Testing of Nickel Nitride-Amorphous Molybdenum / Carbon Cloth (Ni3N-a-Mo / CC-300)
[0090] All experimental procedures and parameters of this embodiment are the same as those of embodiment 1, with the only difference being that in step (1), deposition at a potential of -1.5 V vs. Hg / HgO for 700 s by constant potential method is changed to deposition at a potential of -1.5 V vs. Hg / HgO for 300 s. Fig.12 This is the SEM image of the precursor Ni-Mo / CC-300. From the cracked position of the coating, it can be seen that the thickness of the amorphous Ni-Mo thin layer is about 0.2 to 0.5 microns; Fig.13 HER polarization curve, 10mAcm -2 The overpotential at 256 mV is obtained. After annealing and conversion in ammonia, the HER performance of Ni3N-a-Mo / CC-300 is also lower than that of Ni3N-a-Mo / CC-700, because the deposition time is too short, the thickness of the thin layer is too small, and the active component is insufficient.
[0091] Example 3: Preparation, Characterization and Performance Testing of Nickel Nitride-Amorphous Molybdenum / Carbon Cloth (Ni3N-a-Mo / CC-1100)
[0092] All experimental procedures and parameters in this embodiment are the same as those in Embodiment 1, with the only difference being that in step (1), deposition at a potential of -1.5 V vs. Hg / HgO for 700 s by constant potential method is changed to deposition at a potential of -1.5 V for 1100 s. Fig.14 This is the SEM image of the precursor Ni-Mo / CC-1100. From the cracked position of the coating, it can be seen that the thickness of the amorphous Ni-Mo thin layer is about 0.5 to 1 micron. Fig.15 HER polarization curve, 10 mA cm -2The overpotential at 210 mV is 210 mV. After annealing and conversion in ammonia, the HER performance of Ni3N-a-Mo / CC-1100 is also lower than that of Ni3N-a-Mo / CC-700, because the deposition time is too long, the thin layer is too thick, and the conductivity is reduced.
[0093] Example 4: Nickel sulfide-amorphous molybdenum / carbon cloth (NiS x -a-Mo / CC) preparation, characterization and performance testing:
[0094] All experimental processes and parameters in this embodiment are the same as those in Embodiment 1, with the only difference being that the step (2) of "placing Ni-Mo / CC-700 in a quartz boat, placing the quartz boat in a tube furnace, heating the temperature to 500° C. in ammonia, and converting the amorphous nickel on the surface of the carbon cloth into nickel nitride nanocrystals" is changed to "placing Ni-Mo / CC-700 downstream of the quartz boat and placing 0.1 g of sublimated sulfur upstream; placing the quartz boat in a tube furnace, heating the temperature to 500° C. in argon, and keeping the temperature for 2 h to convert the amorphous nickel on the surface of the carbon cloth into nickel sulfide," while molybdenum still exists in an amorphous form. Fig.16 For NiS x -SEM image of a-Mo / CC, it can be seen that the thin layer still evenly covers the surface of carbon cloth fiber after vulcanization; Fig.17 The XRD spectrum shows that the diffraction peaks of NiS and NiS2 are clearly visible, indicating that amorphous nickel is converted into nickel sulfide nanocrystals, and no diffraction peaks of Mo are seen, indicating that Mo still exists in amorphous form; Fig.18 For NiS x HER polarization curve of a-Mo / CC, 10 mA cm -2 The overpotential is 123 mV, which shows good HER catalytic activity.
[0095] Example 5: Preparation, characterization and performance testing of nickel diselenide-amorphous molybdenum / carbon cloth (NiSe2-a-Mo / CC):
[0096] All experimental processes and parameters in this embodiment are the same as those in Embodiment 1, with the only difference being that the step (2) of "placing Ni-Mo / CC-700 in a quartz boat, placing the quartz boat in a tube furnace, heating the temperature to 500°C in ammonia, and converting the amorphous nickel on the surface of the carbon cloth into nickel nitride nanocrystals" is changed to "placing Ni-Mo / CC-700 downstream of the quartz boat and placing 0.1 g of selenium powder upstream; placing the quartz boat in a tube furnace, heating the temperature to 500°C in argon, and keeping the temperature for 2 h to convert the amorphous nickel on the surface of the carbon cloth into nickel diselenide," while molybdenum still exists in an amorphous form. Fig.19 This is the SEM image of NiSe2-a-Mo / CC. It can be seen that the thin layer still evenly covers the surface of the carbon cloth fiber after selenization. Fig. 20The XRD spectrum shows that amorphous Ni is transformed into NiSe2 nanocrystals. No diffraction peak of Mo is observed, indicating that Mo still exists in amorphous form. Fig.21 HER polarization curve of NiSe2-a-Mo / CC, 10mAcm -2 The overpotential is 139 mV, which shows good HER catalytic activity.
[0097] Example 6: Preparation, Characterization and Performance Testing of Nickel Phosphide-Amorphous Molybdenum / Carbon Cloth (Ni2P-a-Mo / CC)
[0098] All experimental processes and parameters in this embodiment are the same as those in Embodiment 1, with the only difference being that the step (2) of "placing Ni-Mo / CC-700 in a quartz boat, placing the quartz boat in a tube furnace, heating the temperature to 500° C. in ammonia, and converting the amorphous nickel on the surface of the carbon cloth into nickel nitride nanocrystals" is changed to "placing Ni-Mo / CC-700 downstream of the quartz boat and placing 0.1 g of sodium hypophosphite upstream; placing the quartz boat in a tube furnace, heating the temperature to 500° C. in argon, and keeping the temperature for 2 h, and converting the amorphous nickel on the surface of the carbon cloth into nickel phosphide," while the molybdenum still exists in an amorphous form. Fig. 22 This is the SEM image of Ni2P-a-Mo / CC. It can be seen that the thin layer still evenly covers the surface of the carbon cloth fiber after phosphating. Fig.23 The XRD spectrum shows that amorphous Ni is transformed into Ni2P nanocrystals. No diffraction peak of Mo is observed, indicating that Mo still exists in amorphous form. Fig.24 HER polarization curve of Ni2P-a-Mo / CC, 10mAcm -2 The overpotential is 160 mV, which shows good HER catalytic activity.
[0099] Example 7: Preparation, characterization and performance testing of nickel oxide-amorphous molybdenum / carbon cloth (NiO-a-Mo / CC):
[0100] All experimental processes and parameters in this embodiment are the same as those in Embodiment 1, with the only difference being that the temperature in step (2) is raised to 500°C in ammonia gas, and then raised to 500°C in air, and kept warm for 2 hours, so that the amorphous nickel on the surface of the carbon cloth is converted into nickel oxide, while the molybdenum still exists in an amorphous form. Fig.25 This is the SEM image of NiO-a-Mo / CC. It can be seen that the surface of the thin layer becomes rough and grows a spike-like structure after oxidation; Fig.26 is the XRD spectrum, which proves that amorphous Ni is oxidized into NiO nanocrystals, while Mo still exists in amorphous form; Fig. 27 HER polarization curve of NiO-a-Mo / CC, 10mAcm -2 The overpotential is 228 mV, and the HER catalytic activity is poor.
[0101] Example 8: Preparation, Characterization and Performance Testing of Nickel Nitride-Amorphous Tungsten / Carbon Cloth (Ni3N-a-Mo / CC-0.4)
[0102] (1) Preparation, characterization and testing of amorphous nickel-tungsten / carbon cloth (Ni-W / CC-0.4)
[0103] The carbon cloth was cut into 2 cm*1 cm rectangles and soaked in a mixed solution of 10% nitric acid and 10% sulfuric acid (volume ratio of nitric acid to sulfuric acid was 3:1) for 12 h. It was then washed with deionized water until the washing solution was neutral and dried at 40 °C for 8 h. The Ni-W / CC precursor was prepared by cyclic voltammetry deposition. During the synthesis, the pretreated carbon cloth was used as the working electrode, Hg / HgO electrode (1 mol L -1 KOH solution) as the reference electrode and the carbon rod as the counter electrode. The electrolyte was prepared from 2.6g NiSO4·6H2O, 0.48g NiCl2·6H2O, 13.2g Na2WO4·2H2O, 12.9g Na3C6H5O7, 3.1g H3BO3 and 100mL deionized water. Cyclic voltammetry was used to measure the potential of Hg / HgO at 50mV s -1 The deposition was carried out at a scan rate of 60 min. After the deposition, the working electrode was washed with deionized water and dried in an oven at 40 °C for 8 h. -1 ), and the sample was labeled Ni-W / CC-0.4.
[0104] Fig.28 Figure a is the SEM image of Ni-W / CC-0.4. Fig.28 Figure b is a further enlarged SEM image, showing that the Ni-W coating evenly covers the surface of the carbon cloth fiber; Fig.29 Figure a is a TEM image of a thin layer. Fig.29 Figure b is the corresponding selected area electron diffraction pattern, proving that the Ni-W thin layer obtained by electrodeposition is amorphous; Fig.30 This is the XRD spectrum, which only shows the signal of the carbon cloth substrate, and no other crystal diffraction peaks are seen; Fig.31 HER polarization curve of Ni-W / CC-0.4, 10mAcm -2 The overpotential is 127 mV, which shows that the precursor has shown good HER catalytic activity.
[0105] (2) Preparation, characterization and performance testing of nickel nitride-amorphous tungsten / carbon cloth (Ni3N-aW / CC-0.4)
[0106] The Ni-W / CC-0.4 obtained in step (1) is placed in a quartz boat, which is placed in a tube furnace, heated to 500°C in ammonia, and kept warm for 2 hours to convert the amorphous nickel on the surface of the carbon cloth into nickel nitride nanocrystals while still existing in an amorphous form, thereby obtaining Ni3N-aW / CC-0.4.
[0107] Fig.32 Figure a in 32 and Figure b in 32 are low-magnification and high-magnification SEM images of the sample, respectively, and it can be seen that the thin layer still evenly covers the surface of the carbon cloth fiber after nitridation; Fig.33 Figure a in the middle is a TEM image of a thin layer, which directly confirms the existence of a crystalline-amorphous structure. The lattice fringes in the crystalline region correspond to Ni3N. Fig.33 Figure b is the selected area electron diffraction pattern, which further confirms the existence of Ni3N; Fig.34 This is the XRD spectrum. Except for the signal of carbon cloth, other diffraction peaks are consistent with the standard card of Ni3N phase; Fig.35 Figure a is the full XPS spectrum of Ni3N-aW / CC-0.4. Fig.35 Figure b is a Ni 2p fine spectrum, which can be fitted to Ni2p with different valence states. 1 / 2 、Ni2p 3 / 2 and the corresponding satellite peaks. Fig.35 Figure c in the figure is the fine spectrum of W 4f, which can be fitted to W 6+ The oxidized states of the materials are (36.88 and 39.6 eV), among which the two pairs of peaks of WO bonds (37.6 eV) and (35.4 eV) are located at the bottom, which is because the surface oxidation of the material is inevitable when it is exposed to air. Fig.35 Figure d in the middle is the fine spectrum of N1s. The peak at 399.39 eV corresponds to the NH group. The fitted peaks of N1s at 395.29 eV and 398 eV are close to the WN bond and Ni-N bond, respectively. Fig.36 HER polarization curve of Ni3N-aW / CC-0.4, 10 mA cm -2 The overpotential is 70 mV, showing excellent HER catalytic activity; Fig.37 This is the time-current curve of Ni3N-aW / CC-0.4 at an overpotential of 70 mV. It can be seen that the current of the catalytic electrode has almost no decay after continuous operation for 20 hours, proving its excellent stability.
[0108] Example 9: Preparation, Characterization and Performance Testing of Nickel Nitride-Amorphous Tungsten / Carbon Cloth (Ni3N-aW / CC-0.2)
[0109] All experimental procedures and parameters of this embodiment are the same as those of embodiment 8, with the only difference being that the electrolyte used for electrodeposition in step (1) is changed from 13.2 g Na2WO4·2H2O to 6.6 g Na2WO4·2H2O, corresponding to a concentration of 0.2 mol L -1 . Fig.38 HER polarization curve of precursor Ni-W / CC-0.2, 10 mA cm -2 The overpotential at 186 mV is 186 mV. After annealing in ammonia, the HER performance of Ni3N-aW / CC-0.2 is also lower than that of Ni3N-aW / CC-0.4. This is because the W content is too low and the synergistic effect of the prepared crystalline-amorphous heterojunction is not optimal.
[0110] Example 10: Preparation, Characterization and Performance Testing of Nickel Nitride-Amorphous Tungsten / Carbon Cloth (Ni3N-aW / CC-0.6)
[0111] All experimental procedures and parameters in this example are the same as those in Example 8, with the only difference being that the electrolyte used for electrodeposition in step (1) is changed from 13.2 g Na2WO4·2H2O to 19.8 g Na2WO4·2H2O, corresponding to a concentration of 0.6 mol L -1 . Fig.39 HER polarization curve of precursor Ni-W / CC-0.6, 10 mA cm -2 The overpotential at 144 mV. After annealing in ammonia, the HER performance of Ni3N-aW / CC-0.6 is also lower than that of Ni3N-aW / CC-0.4. This is because the W content is too high and the synergistic effect of the prepared crystalline-amorphous heterojunction is not optimal.
[0112] Example 11: Nickel sulfide-amorphous tungsten / carbon cloth (NiS x -aW / CC) preparation, characterization and performance testing
[0113] All experimental processes and parameters in this embodiment are the same as those in Embodiment 8, with the only difference being that in step (2), Ni-W / CC-0.4 is placed in a quartz boat, which is then placed in a tube furnace and heated to 500° C. in ammonia, while Ni-W / CC-0.4 is placed downstream of the quartz boat and 0.1 g of sublimated sulfur is placed upstream; the quartz boat is placed in a tube furnace, heated to 500° C. in argon, and kept warm for 2 h, thereby converting the amorphous nickel on the surface of the carbon cloth into nickel sulfide, while tungsten still exists in an amorphous form. Fig.40 This is the SEM image of NiS-aW / CC, which shows that the thin layer is still uniformly covered after sulfurization; Fig.41The XRD spectrum of NiS-aW / CC shows that the diffraction peaks of NiS and NiS2 are clearly visible, indicating that amorphous nickel is converted into nickel sulfide nanocrystals. No diffraction peaks of W are seen, indicating that W still exists in amorphous form. Fig.42 For NiS x HER polarization curve of -aW / CC, 10mA cm -2 The overpotential is 130 mV, which shows good HER catalytic activity.
[0114] Example 12: Preparation, Characterization and Performance Testing of Nickel Diselenide-Amorphous Tungsten / Carbon Cloth (NiSe2-aW / CC)
[0115] All experimental processes and parameters in this embodiment are the same as those in Embodiment 8, with the only difference being that in step (2), Ni-W / CC-0.4 is placed in a quartz boat, which is then placed in a tube furnace and heated to 500° C. in ammonia, while Ni-W / CC-0.4 is placed downstream of the quartz boat and 0.1 g of selenium powder is placed upstream; the quartz boat is placed in a tube furnace, heated to 500° C. in argon, and kept warm for 2 h to convert the amorphous nickel on the surface of the carbon cloth into nickel diselenide, while tungsten still exists in an amorphous form. Fig.43 This is the SEM image of NiSe2-aW / CC. It can be seen that the thin layer still evenly covers the surface of the carbon cloth fiber after selenization. Fig.44 The XRD spectrum shows that amorphous Ni is transformed into NiSe2 nanocrystals. No W diffraction peak is observed, indicating that W still exists in amorphous form. Fig.45 HER polarization curve of NiSe2-aW / CC, 10mAcm -2 The overpotential is 165 mV, which shows good HER catalytic activity.
[0116] Example 13: Preparation, Characterization and Performance Testing of Nickel Phosphide-Amorphous Tungsten Carbon Cloth (Ni2P-aW / CC)
[0117] All experimental processes and parameters in this embodiment are the same as those in Embodiment 8, with the only difference being that in step (2), Ni-W / CC-0.4 is placed in a quartz boat, which is then placed in a tube furnace and heated to 500° C. in ammonia, while Ni-W / CC-0.4 is placed downstream of the quartz boat and 0.1 g of sodium hypophosphite is placed upstream; the quartz boat is placed in a tube furnace, heated to 500° C. in argon, and kept warm for 2 h, thereby converting the amorphous nickel on the surface of the carbon cloth into nickel phosphide, while tungsten still exists in an amorphous form. Fig.46 This is the SEM image of Ni2P-aW / CC. It can be seen that the thin layer still evenly covers the surface of the carbon cloth fiber after phosphating. Fig.47 The XRD spectrum shows that amorphous Ni is transformed into Ni2P nanocrystals. No W diffraction peak is observed, indicating that W still exists in amorphous form. Fig.48 HER polarization curve of Ni2P-a-Mo / CC, 10mAcm -2 The overpotential is 185 mV, which shows good HER catalytic activity.
[0118] Example 14: Preparation, Characterization and Performance Testing of Nickel Oxide-Amorphous Tungsten / Carbon Cloth (NiO-aW / CC)
[0119] All experimental processes and parameters in this embodiment are the same as those in Embodiment 8, with the only difference being that the temperature in air is increased to 500°C instead of 500°C in ammonia in step (2), and then kept at this temperature for 2 hours to convert the amorphous nickel on the surface of the carbon cloth into nickel oxide, while tungsten still exists in an amorphous form. Fig.49 This is the SEM image of NiO-aW / CC. It can be seen that the surface of the thin layer becomes rough and grows a spike-like structure after oxidation; Fig.50 is the XRD spectrum, which proves that amorphous Ni is oxidized into NiO nanocrystals, while W still exists in amorphous form; Fig.51 HER polarization curve of NiO-aW / CC, 10mAcm -2 The overpotential is 329 mV, and the HER catalytic activity is poor.
[0120] Example 15: Preparation, Characterization and Performance Testing of Nickel Nitride-Amorphous Chromium / Carbon Cloth (Ni3N-a-Cr / CC)
[0121] (1) Preparation, characterization and testing of amorphous nickel-chromium / carbon cloth (Ni-Cr / CC)
[0122] The carbon cloth was cut into 2 cm*1 cm rectangles and soaked in a mixed solution of 10% nitric acid and 10% sulfuric acid (volume ratio of nitric acid to sulfuric acid was 3:1) for 12 h. It was then washed with deionized water until the washing solution was neutral and dried at 40 °C for 8 h. The Ni-Cr / CC precursor was prepared by constant potential deposition. During the synthesis, the pretreated carbon cloth was used as the working electrode, Hg / HgO electrode (1 mol L -1 KOH solution) as the reference electrode and carbon rod as the counter electrode. The electrolyte consists of 1g NiSO4·6H2O, 1g NiCl2·6H2O, 9.6g CrCl3·6H2O, 7.7g C6H8O7, 10.7g Na3C6H5O7, 6.2g H3BO3, 0.02g CH3(CH2) 11 OSO3Na and 100mL deionized water were prepared. The deposition was carried out by constant potential deposition at -1.5V vs.Hg / HgO for 1000s. After the deposition, the working electrode was washed with deionized water and dried in an oven at 40°C for 8h. Fig.52This is the SEM image of the obtained Ni-Cr / CC, which shows that the coating is evenly covered on the surface of the carbon cloth fiber.
[0123] (2) Preparation, characterization and performance testing of nickel nitride-amorphous chromium / carbon cloth (Ni3N-a-Cr / CC)
[0124] The Ni-Cr / CC obtained in step (1) is placed in a quartz boat, which is placed in a tube furnace, heated to 500°C in ammonia, and kept warm for 2 hours to convert the amorphous nickel on the surface of the carbon cloth into nickel nitride nanocrystals, while chromium still exists in an amorphous form, thereby obtaining Ni3N-a-Cr / CC-. Fig.53 The XRD spectrum of the obtained Ni3N-a-Cr / CC, except for the signal of carbon cloth, other diffraction peaks are consistent with the standard card of Ni3N phase, proving that the amorphous Ni in the coating is converted into Ni3N nanocrystals, while no diffraction peaks of W and its compounds are found in the XRD spectrum, indicating that W still exists in amorphous form; Fig.54 HER polarization curve, 10mAcm -2 The overpotential is 71 mV, showing excellent HER electrocatalytic activity.
Claims
1. A nickel-based compound-amorphous chromium heterojunction self-supporting electrode, characterized in that: It is composed of a nickel-based compound nanocrystalline-amorphous chromium heterojunction thin layer covered on carbon cloth fiber, wherein the nickel-based compound component is nickel disulfide or nickel sulfide or nickel diselenide or nickel phosphide or nickel nitride or nickel oxide, and the amorphous chromium component is chromium or molybdenum or tungsten.
2. The nickel-based compound-amorphous chromium heterojunction self-supporting electrode according to claim 1, characterized in that: The thickness of the thin layer is 0.2-1 micrometer, and the size of the nanocrystal is 5-10 nanometers.
3. A method for preparing the nickel-based compound-amorphous chromium heterojunction self-supporting electrode according to claim 1, characterized in that The following steps are involved: (1) firstly introduce active groups on the surface of carbon cloth fiber, then wash with deionized water until the cleaning solution becomes neutral and then dry; (2) using a nickel-chromium plating solution, a nickel-molybdenum plating solution, or a nickel-tungsten plating solution as an electrolyte, and using an electrodeposition method to cover a layer of nickel-chromium, nickel-molybdenum, or nickel-tungsten thin layer having amorphous characteristics on the surface of the dried carbon cloth fiber to obtain an amorphous nickel-chromium group metal / carbon cloth; (3) placing the amorphous nickel-chromium metal / carbon cloth downstream of a quartz boat, placing sublimated sulfur or selenium powder or sodium hypophosphite upstream of the quartz boat, and then placing the quartz boat in a tube furnace, heating and keeping the temperature in nitrogen or argon, so as to convert the amorphous nickel on the surface of the carbon cloth into nickel disulfide or nickel sulfide or nickel diselenide or nickel phosphide nanocrystals, while chromium or molybdenum or tungsten still exists in an amorphous form; Alternatively: the amorphous nickel-chromium metal / carbon cloth is placed in a quartz boat, the quartz boat is placed in a tube furnace, the temperature is increased and kept in ammonia or air, the amorphous nickel on the surface of the carbon cloth is converted into nickel nitride or nickel oxide nanocrystals, and the chromium, molybdenum or tungsten still exists in an amorphous form.
4. The preparation method according to claim 3, characterized in that: The electrodeposition method described in step (2) is a constant potential deposition method or a cyclic voltammetric deposition method. The deposition potential of the constant potential deposition is -1.0 to 1.5 V vs. Hg / HgO, and the deposition time is 300 to 1100 s; the potential range of the cyclic voltammetric deposition is -1.2 to -1.6 V vs. Hg / HgO, and the deposition time is 60 to 100 min.
5. The preparation method according to claim 3, characterized in that: The formula of the nickel-chromium plating solution described in step (2) is: 1gNiSO4·6H2O, 1gNiCl2·6H2O, 9.6gCrCl3·6H2O, 7.7gC6H8O7, 10.7gNa3C6H5O7, 6.2gH3BO3, 0.02gCH3(CH2) 11 OSO3Na and 100mL deionized water; The formula of the nickel-molybdenum plating solution is: 3g Na2MoO4·2H2O, 6g NiSO4·6H2O, 2mL NH3·H2O, 8g Na3C6H5O7·2H2O, 2g NiCl·6H2O and 100mL deionized water; The formula of the nickel-tungsten plating solution is 2.6g NiSO4·6H2O, 0.48g NiCl2·6H2O, 6.6-19.8g Na2WO4·2H2O, 12.9g Na3C6H5O7, 3.1g H3BO3 and 100mL deionized water.
6. The preparation method according to any one of claims 3 to 5, characterized in that: In step (1), the carbon cloth is immersed in a nitric acid or sulfuric acid or a mixed solution of sulfuric acid and nitric acid with a mass fraction of 10% to 15% to introduce active groups on the fiber surface.
7. The preparation method according to any one of claims 3 to 5, characterized in that: In step (3), the heating temperature is 450-500° C. and the insulation time is 1-3 hours.
8. The preparation method according to any one of claims 3 to 5, characterized in that: In step (3), the ratio of the mass of the sublimated sulfur or selenium powder or sodium hypophosphite to the area of the amorphous nickel-chromium group metal / carbon cloth is 0.05-0.1 g / cm -2 .
9. An application of the nickel-based compound-amorphous chromium heterojunction self-supporting electrode according to claim 1, characterized in that: Applied to hydrogen evolution reaction electrocatalyst.
Citation Information
Patent Citations
Electrodeposition method for preparing nickel oxide nanosheet supported nickel-molybdenum oxide quantum dots
CN111118539A
Preparation method of nickel tungsten phosphide-nickel tungsten oxide with heterostructure
CN112978815A
N and P co-doped NF@NiMoO4 hollow nanowire composite material and preparation method and application thereof
CN114059082A
Molybdenum-doped nickel sulfide / nickel phosphide self-supporting heterojunction electrode and preparation method thereof
CN115863064A
Nickel-based electrocatalyst supported by porous nickel, preparation method of nickel-based electrocatalyst and application of nickel-based electrocatalyst in hydrogen production by electrolysis of water
CN116065184A
Cited By
NiMo-based crystalline / amorphous heterostructure composite material as well as preparation method and application thereof
CN119753734A