Preparation method and application of after-washing water repellency self-recovery water repellent

By copolymerizing nanotitanium dioxide with acrylate monomers, a fluorine-free hydrophobic agent was prepared. It used its photothermal conversion ability to restore the water-repellent properties of the fabric under natural drying conditions, and solved the deterioration of the water-repellent properties of the hydrophobic fabric after washing. The problem has achieved environmentally friendly and efficient hydrophobic effects.

CN119020990AActive Publication Date: 2024-11-26QINGDAO UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410934887.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-26
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The existing hydrophobic fabrics have deteriorated water-repellent properties under natural drying conditions after washing and natural drying, and common water-repellents have problems of bioaccumulativeness, toxicity and high cost.

Method used

Copolymerization of nanotitanium dioxide and acrylate monomers is used to prepare fluorine-free hydrophobic agents by modifying nanotitanium dioxide and cationic surfactant, and the water-repellent properties of the fabric are restored under natural drying conditions using the photothermal conversion ability of nanotitanium dioxide.

Benefits of technology

It realizes the recovery of efficient water repellent performance under natural drying conditions without drying, avoids environmental pollution and bioaccumulated toxicity, applies environmental protection requirements, and improves the water resistance and UV resistance of fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004940995350000091
    Figure BDA0004940995350000091
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a water repellent with self-recovery water repellency after washing, and belongs to the technical field of environment-friendly polymers. Unsaturated double bonds contained on the surface of modified titanium dioxide and acrylate monomers used for synthesis of the water repellent are subjected to free radical polymerization, titanium dioxide and a main framework of the water repellent are connected through chemical groups, titanium dioxide particles and water repellent macromolecules stably exist in water repellent emulsion, the water repellent is high in film forming fastness, and the water repellent has a good water repellent effect. Due to the photo-thermal conversion capability of the nano titanium dioxide and the roughness contribution to the fabric surface, the finished fabric has high static water contact angle, high hydrostatic pressure resistance, high spraying resistance grade and other water repellency, the fabric does not need to be dried after being washed, and the spraying resistance grade can be effectively recovered by conventional natural airing; meanwhile, the ultraviolet shielding performance of the nano titanium dioxide endows the fabric finished by the prepared water repellent with an anti-ultraviolet function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a water repellent agent with self-recovering water repellency after washing, belonging to the technical field of environmentally friendly polymers. Background Art

[0002] As consumers' demand for functional textiles gradually increases, various functional textiles have received extensive attention and development. Hydrophobic fabrics are widely used due to their excellent water-repellent, anti-fouling, and self-cleaning properties. However, water-repellent fabrics generally have the problem that the water-repellent effect decreases after natural drying after washing, while the effect recovers after high-temperature drying (≥55°C). The temperature of the fabric surface cannot reach a high temperature when it is dried naturally, resulting in a decrease in consumers' satisfaction with water-repellent textiles, which are mainly dried naturally.

[0003] Fabrics have a long history of water repellency, and commonly used water repellents are mainly fluorine-containing compounds, silicones and aliphatic hydrocarbon compounds. Fluorine-containing water repellents can give fabrics excellent water repellency, but during the synthesis and use process, fluorine-containing water repellents have certain bioaccumulation and toxicity, so there is an ecological pollution problem; at the same time, they are expensive, resulting in high production and use costs. Silicone water repellents can give fabrics better water repellency and softness, but their disadvantages are that they increase pilling and seam separation on the surface of the fabric. Long-chain aliphatic hydrocarbon water repellents are mainly acrylate compounds, which can give fabrics better hydrophobic properties, but the water repellency is slightly lower than that of fluorine-containing water repellents. Water repellents use the long alkane chains or fluorocarbon chains on their structural units to reduce the surface energy of the fabric and give it water repellency. The water-repellent finishing adopts the rolling baking method, and the alkane chains or fluorocarbon chains are freely stretched at high temperatures to form an effective coverage of the fabric.

[0004] Alkane chains or fluorocarbon chains are non-polar groups, which have a large difference in polarity from water (polar group). During the washing process, the alkane chains or fluorocarbon chains curl up to reduce the interfacial energy between the non-polar and polar groups. It takes energy for the curled non-polar groups to stretch again to form an effective cover on the fabric. The energy obtained by the fabric during the natural drying process is too low to support the re-stretching of its non-polar groups. Photothermal conversion materials can absorb ultraviolet rays in sunlight and convert light energy into heat energy. They can enhance the amount of heat obtained by water-repellent finished fabrics under sunlight and promote the re-stretching of curled non-polar groups during washing. Common photothermal conversion materials such as carbon-based materials, metal materials, semiconductor materials, etc. are mostly black or other dark colors, have high photothermal conversion capabilities, and can increase the material temperature in a short time, but their inherent colors will interfere with or directly cover the color of the textiles, and are not suitable for textile fields that require color. Summary of the invention

[0005] In view of the above problems, the purpose of the present invention is to provide a fluorine-free acrylic water repellent with self-recovery of hydrophobic properties under natural drying conditions after washing. Nano titanium dioxide is a white powder, and the use of an appropriate amount does not affect the existing color of the fabric. By introducing nano titanium dioxide into the molecular structure of the water repellent, fluorine-free high water repellency is achieved, and the fabric does not need to be dried after washing, and the water repellency self-recovers under natural drying conditions.

[0006] In view of the above purpose, the present invention first provides a method for preparing a water repellent having self-recovering water repellency after washing, the method comprising:

[0007] (1) preparing nano titanium dioxide with a titanium source, an organic solvent, a reaction inhibitor and deionized water, modifying the nano titanium dioxide with a modifier, removing the solvent by rotary evaporation and aging to obtain modified nano titanium dioxide;

[0008] (2) taking a cationic surfactant and a nonionic surfactant, dissolving them in deionized water, and then adding the modified nano-titanium dioxide obtained in step (1) to prepare an emulsion;

[0009] (3) mixing part of the acrylic ester monomer and part of the emulsion containing modified nano-titanium dioxide obtained in step (2), and emulsifying the mixture with an ultrasonic cell crusher to obtain a pre-emulsion A;

[0010] (4) mixing the remaining acrylic ester monomer and the remaining titanium dioxide-containing emulsion and emulsifying them with an ultrasonic cell crusher to obtain a pre-emulsion B;

[0011] (5) Under nitrogen protection, the pre-emulsion B and the aqueous solution of the initiator are slowly added to the pre-emulsion A, and after the reaction is kept warm, the material is cooled and discharged to obtain a water-repellent self-recovering water-repellent agent.

[0012] The present invention utilizes cationic surfactants to increase the adsorption of water repellent polymers by fabrics during water repellent finishing; uses acrylate monomers to avoid the problem of fluorine-containing groups polluting the environment; utilizes the reaction of epoxy groups of acrylate monomers with fabrics and water repellent groups to enhance the anchoring of water repellent polymers on fabrics, thereby solving the problem of fabric water resistance; and increases the surface energy of fabrics during natural drying through the photothermal conversion capability of nano titanium dioxide components, thereby promoting the reorientation of non-polar groups that curl during washing, thereby restoring a highly efficient water repellent effect.

[0013] In one embodiment of the present invention, the titanium source in step (1) includes at least one of tetrabutyl titanate, tetraethyl titanate, and tetraisopropyl titanate; the organic solvent includes at least one of ethanol, propanol, or isopropanol; the reaction inhibitor includes one or more of glacial acetic acid, nitric acid, or hydrochloric acid; and the modifier includes at least one of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, and dimethoxymethylvinylsilane.

[0014] In one embodiment of the present invention, the components in the preparation of nano titanium dioxide in step (1) include 5-20% titanium source, 60-80% organic solvent, 5-20% reaction inhibitor, and the rest is water in terms of mass percentage; after adding the modifier, the concentration of the modifier in the solution is 1-20 g / L.

[0015] In one embodiment of the present invention, the preparation method of the modified titanium dioxide in step (1) is to mix a titanium source, an organic solvent, a reaction inhibitor and deionized water, and stir at room temperature at 100-1000 r / min for 1-8 hours to obtain nano titanium dioxide, and then add a modifier, react at 20-60°C for 4-24 hours, and age after removing the solvent by rotary evaporation for 12-24 hours.

[0016] In one embodiment of the present invention, the cationic surfactant in step (2) is one or a mixture of octadecyltrimethylammonium chloride and hexadecyltrimethylammonium chloride; the nonionic surfactant is one or more mixtures of polyoxyethylene ether surfactants; and the mass ratio of the cationic surfactant to the nonionic surfactant is (0.2-0.8):1.

[0017] In one embodiment of the present invention, the mass ratio of the total amount of the cationic surfactant and the nonionic surfactant to the total amount of the acrylate monomer is (0.05-0.15):1; the mass ratio of the amount of the modified nano titanium dioxide to the total amount of the acrylate monomer is (0.01-0.1):1; the mass concentration of the modified nano titanium dioxide in the emulsion is 0.15-3%.

[0018] In one embodiment of the present invention, the acrylic acid ester monomer in step (3) includes any one or more of methyl acrylate, butyl acrylate, hexyl acrylate, octyl acrylate, decyl acrylate, dodecyl acrylate, tetradecyl acrylate, hexadecyl acrylate, octadecyl acrylate, methyl methacrylate, butyl methacrylate, hexyl methacrylate, octyl methacrylate, decyl methacrylate, dodecyl methacrylate, tetradecyl methacrylate, hexadecyl methacrylate, and octadecyl methacrylate.

[0019] In one embodiment of the present invention, the mass of the emulsion containing modified nano-titanium dioxide in step (3) is 50-80% of the mass of the total modified nano-titanium dioxide emulsion.

[0020] In one embodiment of the present invention, the acrylate monomer in step (3) accounts for 40-60% of the total acrylate monomer mass; the total mass of the acrylate monomer accounts for 15-30% of the total mass of the water repellent.

[0021] In one embodiment of the present invention, the initiator in step (5) includes one or more of azobisisobutyronitrile, azobisisoheptanenitrile, azobisisobutyramidine hydrochloride, potassium persulfate, ammonium persulfate, and dibenzoyl peroxide; the mass of the initiator accounts for 0.1 to 1% of the total mass percentage of the acrylate monomer; and the aqueous solution of the initiator is 10 to 100 times diluted with deionized water.

[0022] In one embodiment of the present invention, the reaction temperature in step (5) is 70-80° C. and the reaction time is 2-4 hours.

[0023] The present invention also provides a water repellent with self-recovering water repellency after washing, which is prepared according to the above preparation method.

[0024] The present invention also provides a method for treating a fabric with self-recovering water-repellent properties after washing, which method comprises first immersing the fabric in an aqueous solution of a water-repellent agent (40-100 g / L) prepared by the above method, then padding and baking, with a padding rate of 80-200%, pre-baking at 80-110°C for 3-5 minutes, and baking at 120-160°C for 1-5 minutes.

[0025] The present invention also provides a fabric with self-recovering water-repellent performance after washing, wherein the fabric comprises the above-mentioned titanium dioxide-based water-repellent agent with self-recovering water-repellent performance after washing, or is prepared by using the above-mentioned treatment method.

[0026] The present invention has the following beneficial effects:

[0027] 1. In the process of synthesizing the water repellent, the modified nano titanium dioxide is added to the water repellent, and the modified nano titanium dioxide undergoes free radical copolymerization with the acrylic ester monomer. The modified nano titanium dioxide and the acrylic ester main chain are linked by chemical bonds. The modified nano titanium dioxide and the water repellent main chain exist stably without phase separation.

[0028] 2. The present invention adopts the copolymerization reaction of modified nano titanium dioxide and acrylic monomer to prepare the water repellent. Nano titanium dioxide has good light-heat conversion performance. By adding nano titanium dioxide in the process of preparing the water repellent, the surface energy of the fabric during the natural drying process can be increased, and the non-polar groups that curl during the washing process can be reoriented to restore the efficient water repellent effect. The water repellent synthesized by the method of the present invention can give the fabric the ability to self-recover the water repellent performance under natural drying conditions without drying after washing. In addition, nano titanium dioxide is a white powder, and the use of an appropriate amount does not affect the existing color of the fabric.

[0029] 3. The present invention uses cationic and nonionic surfactants to prepare an emulsifier solution, which can make the acrylate molecules uniformly dispersed in the water phase to form a stable emulsion, thereby improving the performance of the application.

[0030] 4. The cationic fluorine-free acrylic water repellent prepared by the present invention avoids the environmental pollution and bioaccumulation toxicity problems caused by the use of fluorine-containing water repellents, and has extremely low VOC emissions, which meets environmental protection requirements.

[0031] 5. The water repellent prepared by the present invention is cationic and can be closely adsorbed with fabrics (the water phase system is negatively charged), which is conducive to the uniform film formation of water repellent macromolecules on the fabric surface. The cross-linkable groups contained in the water repellent improve the water resistance fastness of the water repellent.

[0032] 6. The present invention first uses part of acrylic acid monomer and part of modified titanium dioxide to prepare an emulsion as a reaction base liquid, and then slowly adds the emulsion prepared by the remaining substances and an aqueous solution of an initiator to prepare a water repellent. This method can prevent polymer precipitation and uneven molecular weight distribution caused by monomer explosion, and is conducive to the preparation of a stable emulsion. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with specific examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0034] Test method:

[0035] The spray resistance of the fabric's water repellency is evaluated by the water level, and the water level of the fabric after drying is tested according to "GB / T 4745-2012 Testing and evaluation of the waterproof performance of textiles - Water level test method".

[0036] The water repellency and water wetting resistance of the fabric are evaluated by the static water contact angle. The static contact angle of the fabric after water repellent finishing is measured using a contact angle meter: 5 μL of water droplets are added to five different locations on the fabric, and the static contact angle is measured.

[0037] The static water resistance of the fabric water repellency is carried out according to the AATCC-127-2013 "Water Resistance: Hydrostatic Pressure Test" standard.

[0038] Fabric washing and drying parameters: The fabric was washed according to GB / T8629-2017 “Household Washing and Drying Procedure for Textile Experiments” and then exposed to sunlight for 1 hour at 30°C in a sunlight fastness tester.

[0039] The evaluation of fabric softness is carried out in accordance with AATCC TM 202 "Evaluation of Relative Hand Feel of Textiles and Garments: Instrumental Method".

[0040] The fabric anti-ultraviolet evaluation shall be carried out in accordance with GB / T 18830-2009 “Evaluation of UV protection performance of textiles”.

[0041] Embodiment 1:

[0042] The following steps are followed to prepare a self-recovering water repellent agent for water repellency after washing and to finish the fabric:

[0043] (1) A titanium source (tetrabutyl titanate), an organic solvent (ethanol), a reaction inhibitor (glacial acetic acid) and deionized water were mixed (titanium source: organic solvent: reaction inhibitor: deionized water = 10:70:5:15, mass ratio) and stirred at 500 r / min at room temperature for 8 h to obtain nano-titanium dioxide. A modifier (γ-methacryloxypropyltrimethoxysilane) was added, and the concentration of the modifier in the solution was 10 g / L. After reacting at 40°C for 12 h, the mixture was cooled to room temperature and aged for 16 h to obtain modified nano-titanium dioxide.

[0044] (2) Cationic surfactant octadecyltrimethylammonium chloride, nonionic surfactant polyoxyethylene stearate (polyoxyethylene number is 20, the mass ratio of cationic surfactant to nonionic surfactant is 0.2:1) and modified nano-titanium dioxide are dissolved in deionized water to prepare an emulsion containing modified nano-titanium dioxide, wherein the mass concentration of modified nano-titanium dioxide is 1%, the mass ratio of the total amount of cationic surfactant and nonionic surfactant to the total amount of acrylate monomer is 0.05:1, the ratio of the amount of modified nano-titanium dioxide to the total mass of acrylate monomer is 0.05:1, and the total mass of acrylate monomer accounts for 20% of the total mass of the water repellent.

[0045] (3) Octadecyl acrylate (accounting for 40% of the total mass of acrylate monomers) was added to a part of the emulsion containing modified nano-titanium dioxide (accounting for 50% of the total mass of the emulsion), and the mixture was ultrasonically treated in an ice bath for 30 minutes in an ultrasonic cell crusher to obtain pre-emulsion A. Butyl acrylate (accounting for 30% of the total mass of acrylate monomers), methyl methacrylate (accounting for 20% of the total mass of acrylate monomers), and glycidyl acrylate (accounting for 10% of the total mass of acrylate monomers) were added to the remaining emulsion containing modified nano-titanium dioxide, and the mixture was ultrasonically treated in an ice bath for 30 minutes in an ultrasonic cell crusher to obtain pre-emulsion B.

[0046] (4) Under nitrogen protection, pre-emulsion B and initiator azobisisobutyramidine hydrochloride (accounting for 1% of the total mass of the acrylate monomer and diluted 100 times with deionized water) were simultaneously added dropwise into a reactor containing pre-emulsion A at a temperature of 75°C with mechanical stirring (300 r / min) at a dropping speed of 2 g / L. After reacting for 3 hours, the mixture was naturally cooled to room temperature to obtain a water repellent agent with self-recovering water repellency after washing.

[0047] Water repellent properties after washing self-recovery Water repellent treated fabrics:

[0048] The water repellent was used to treat cotton fabrics with 60 g / L of the above-mentioned water repellent by padding and baking finishing process. After the fabrics were impregnated, they were squeezed out with a 100% squeeze rate, pre-baked at 105°C for 3 minutes, and then baked at 160°C for 2 minutes. The relevant parameters of the treated fabrics are shown in Table 1.

[0049] Embodiment 2:

[0050] The following steps are followed to prepare a self-recovering water repellent agent for water repellency after washing and to finish the fabric:

[0051] (1) A titanium source (tetraethyl titanate), an organic solvent (propanol), a reaction inhibitor (nitric acid, 5 g / L) and deionized water were mixed (titanium source: organic solvent: reaction inhibitor: deionized water = 5:60:5:30, mass ratio) and stirred at 100 r / min at room temperature for 4 h to obtain nano-titanium dioxide. A modifier (vinyltrimethoxysilane) solution was added with a modifier concentration of 1 g / L. The mixture was reacted at 60°C for 4 h, then cooled to room temperature and aged for 24 h to obtain modified nano-titanium dioxide.

[0052] (2) Cationic surfactant hexadecyltrimethylammonium chloride, nonionic surfactant polyoxyethylene stearate (polyoxyethylene number is 40, the mass ratio of cationic surfactant to nonionic surfactant is 0.2:1) and modified nano-titanium dioxide are dissolved in deionized water to prepare an emulsion containing modified nano-titanium dioxide, wherein the mass concentration of modified nano-titanium dioxide is 0.15%, the mass ratio of the total amount of cationic surfactant and nonionic surfactant to the total amount of acrylate monomer is 0.05:1, the ratio of the amount of modified nano-titanium dioxide to the total mass of acrylate monomer is 0.01:1, and the total mass of acrylate monomer accounts for 30% of the total mass of the water repellent.

[0053] (3) Hexadecyl acrylate (accounting for 50% of the total mass of the acrylate monomer) is added to a part of the emulsion containing modified nano-titanium dioxide (accounting for 40% of the total mass of the emulsion), and the mixture is ultrasonically treated in an ice bath for 30 minutes in an ultrasonic cell crusher to obtain pre-emulsion A. Butyl acrylate (accounting for 25% of the total mass of the acrylate monomer), hexyl methacrylate (accounting for 20% of the total mass of the acrylate monomer), and glycidyl methacrylate (accounting for 5% of the total mass of the acrylate monomer) are added to the remaining emulsion containing modified nano-titanium dioxide, and the mixture is ultrasonically treated in an ice bath for 30 minutes in an ultrasonic cell crusher to obtain pre-emulsion B.

[0054] (4) Under nitrogen protection, pre-emulsion B and initiator potassium persulfate (accounting for 0.1% of the total mass of the acrylate monomer and diluted 100 times with deionized water) were simultaneously added dropwise into the reactor containing pre-emulsion A at a temperature of 70°C with mechanical stirring (500 r / min) at a dropping speed of 2 g / L. After reacting for 2 hours, the mixture was naturally cooled to room temperature to obtain a water repellent agent with self-recovering water repellency after washing.

[0055] Water repellent properties after washing self-recovery Water repellent treated fabrics:

[0056] The water repellent was used to treat cotton fabrics at 100 g / L by padding and baking finishing process. The fabrics were impregnated with 80% of the liquid, pre-baked at 80°C for 5 min, and then baked at 150°C for 3 min. The relevant parameters of the treated fabrics are shown in Table 1.

[0057] Embodiment 3:

[0058] The following steps are followed to prepare a self-recovering water repellent agent for water repellency after washing and to finish the fabric:

[0059] (1) A titanium source (tetraisopropyl titanate), an organic solvent (isopropanol), a reaction inhibitor (hydrochloric acid, 10 g / L) and deionized water were mixed (titanium source: organic solvent: reaction inhibitor: deionized water = 20:60:10:10, mass ratio) and stirred at 1000 r / min at room temperature for 5 h to obtain nano-titanium dioxide. A modifier (dimethoxymethylvinylsilane) was added to the solution with a modifier concentration of 20 g / L. The mixture was reacted at 20°C for 24 h, then cooled to room temperature and aged for 12 h to obtain modified nano-titanium dioxide.

[0060] (2) Cationic surfactant octadecyltrimethylammonium chloride, nonionic surfactant polyoxyethylene stearate (polyoxyethylene number is 60, the mass ratio of cationic surfactant to nonionic surfactant is 0.8:1) and modified nano-titanium dioxide are dissolved in deionized water to prepare an emulsion containing modified nano-titanium dioxide, wherein the mass concentration of modified nano-titanium dioxide is 3%, the mass ratio of the total amount of cationic surfactant and nonionic surfactant to the total amount of acrylate monomer is 0.15:1, the ratio of the amount of nano-titanium dioxide to the total mass of acrylate monomer is 0.1:1, and the total mass of acrylate monomer accounts for 15% of the total mass of the water repellent.

[0061] (3) Tetradecyl acrylate (accounting for 60% of the total mass of the acrylate monomer) was added to a part of the emulsion containing modified nano-titanium dioxide (accounting for 80% of the total mass of the emulsion), and the mixture was ultrasonically treated in an ice bath for 30 minutes in an ultrasonic cell crusher to obtain pre-emulsion A. Hexyl methacrylate (accounting for 12% of the total mass of the acrylate monomer), methyl acrylate (accounting for 20% of the total mass of the acrylate monomer), and glycidyl acrylate (accounting for 8% of the total mass of the acrylate monomer) were added to the remaining emulsion containing modified nano-titanium dioxide, and the mixture was ultrasonically treated in an ice bath for 30 minutes in an ultrasonic cell crusher to obtain pre-emulsion B.

[0062] (4) Under nitrogen protection, pre-emulsion B and initiator ammonium persulfate (accounting for 1% of the total mass of the acrylate monomer and diluted 100 times with deionized water) were simultaneously added dropwise into a reactor containing pre-emulsion A at a temperature of 80°C with mechanical stirring (300 r / min) at a dropping speed of 2 g / L. After reacting for 4 hours, the mixture was naturally cooled to room temperature to obtain a water repellent agent with self-recovering water repellency after washing.

[0063] Water repellent properties after washing self-recovery Water repellent treated fabrics:

[0064] The water repellent was used to treat cotton fabrics at 40 g / L by padding and baking finishing process. After the fabrics were impregnated, they were squeezed out with a 100% squeeze rate, pre-baked at 105°C for 2 minutes, and then baked at 120°C for 5 minutes. The relevant parameters of the treated fabrics are shown in Table 1.

[0065] Embodiment 4-5:

[0066] The following steps are followed to prepare a self-recovering water repellent agent for water repellency after washing and to finish the fabric:

[0067] Preparation of water repellent:

[0068] Same as Example 1.

[0069] Water repellent treated fabrics:

[0070] Only the fabric type was changed to polyester (Example 4) and nylon (Example 5), and the rest was the same as Example 1. The relevant parameters of the treated fabrics are shown in Table 1.

[0071] Comparative Example 1:

[0072] The fabric was treated according to the following steps: the fabric was impregnated with a domestic commercial fluorine-free acrylic ester water repellent aqueous solution (60 g / L) and then squeezed out at a 100% squeeze rate, pre-baked at 105°C for 3 minutes and then baked at 160°C for 2 minutes. The relevant parameters of the treated fabric are shown in Table 1.

[0073] Comparative Example 2:

[0074] Follow these steps to prepare the water repellent and finish the fabric:

[0075] Preparation of water repellent:

[0076] No modified nano titanium dioxide was added, and the rest was the same as in Example 1.

[0077] Water repellent treated fabrics:

[0078] Same as Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0079] Comparative Example 3:

[0080] Follow these steps to prepare the water repellent and finish the fabric:

[0081] Preparation of water repellent:

[0082] The ratio of the amount of nano titanium dioxide to the total mass of the acrylic ester monomers is 0.2:1, and the rest is the same as in Example 1.

[0083] Water repellent treated fabrics:

[0084] Same as Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0085] Comparative Example 4:

[0086] Follow these steps to prepare the water repellent and finish the fabric:

[0087] Preparation of water repellent:

[0088] The nano titanium dioxide was not modified, and the other parts were the same as those in Example 1.

[0089] Water repellent treated fabrics:

[0090] Same as Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0091] Comparative Example 5:

[0092] Follow these steps to prepare the water repellent and finish the fabric:

[0093] Preparation of water repellent:

[0094] The modified nano titanium dioxide is the same as in Example 1. The cationic surfactant octadecyl trimethyl ammonium chloride and the nonionic surfactant polyoxyethylene stearate (polyoxyethylene number is 20, and the mass ratio of the cationic surfactant to the nonionic surfactant is 1.5:1) and the modified nano titanium dioxide are dissolved in deionized water to prepare an emulsion containing modified nano titanium dioxide, wherein the mass concentration of the modified nano titanium dioxide is 2%, the mass ratio of the total amount of the cationic surfactant and the nonionic surfactant to the total amount of the acrylate monomer is 0.25:1, the amount of nano titanium dioxide is 0.2:1 of the total mass of the acrylate monomer, and the total mass of the acrylate monomer accounts for 10% of the total mass of the water repellent. Octadecanyl acrylate (accounting for 80% of the total mass of acrylate monomer) was added to a part of the modified nano-titanium dioxide emulsion (accounting for 40% of the total emulsion mass), and the mixture was ultrasonicated in an ice bath for 30 minutes in a cell crusher to obtain pre-emulsion A. Butyl acrylate (accounting for 5% of the total mass of acrylate monomer), methyl methacrylate (accounting for 10% of the total mass of acrylate monomer), and glycidyl acrylate (accounting for 5% of the total mass of acrylate monomer) were added to the remaining modified nano-titanium dioxide emulsion, and the mixture was ultrasonicated in an ice bath for 30 minutes in an ultrasonic cell crusher to obtain pre-emulsion B. Under nitrogen protection, pre-emulsion B and initiator azobisisobutyramidine hydrochloride (accounting for 2% of the total mass of acrylate monomer and diluted 100 times with deionized water) were simultaneously added dropwise in a reactor containing pre-emulsion A at a temperature of 60°C with mechanical stirring (300r / min), with a dropping speed of 2g / L. After reacting for 3 hours, the mixture was naturally cooled to room temperature to obtain a water repellent with self-recovery water repellency after washing.

[0095] Water repellent treated fabrics:

[0096] Same as Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0097] Comparative Example 6-7:

[0098] Follow these steps to make water repellent and finish fabrics:

[0099] Preparation of water repellent:

[0100] Same as Example 1.

[0101] Water repellent treated fabrics:

[0102] Only the amount of water repellent was changed to 20 g / L (Control Example 6) and 200 g / L (Control Example 7), and the others were the same as Example 1. The relevant parameters of the treated fabrics are shown in Table 1.

[0103] Table 1 Relevant parameters of treated fabrics

[0104]

[0105] Note: The untreated cotton fabric was completely wetted by water before washing and after washing, with a hydrostatic pressure resistance of 170 mm, a softness of 53.8, an ultraviolet protection factor UPF of 5.3, and an ultraviolet light transmittance T(UVA) of 24.6. The untreated polyester fabric was completely wetted by water before washing and after washing, with a hydrostatic pressure resistance of 210 mm, a softness of 48.8, an ultraviolet protection factor UPF of 23.3, and an ultraviolet light transmittance T(UVA) of 22.1. The untreated nylon fabric was completely wetted by water before washing and after washing, with a hydrostatic pressure resistance of 190 mm, a softness of 66.8, an ultraviolet protection factor UPF of 10.2, and an ultraviolet light transmittance T(UVA) of 23.2.

[0106] The static water contact angle of fabrics treated with washable water repellent changes little after washing, but there are differences in the fabric spray resistance level under different drying methods (according to the detection characterization method, the highest fabric water repellent level is 5). There is a common problem that the spray resistance level of fabrics decreases when naturally dried after washing, that is, the amount of water adhesion residue on the fabric increases.

[0107] It can be seen from Examples 1-3 in the table that the fabrics treated with the water repellent containing nano titanium dioxide in the chemical structure prepared according to the method provided by the present invention have good spray resistance after washing and natural drying, mainly because titanium dioxide can increase the surface roughness of the fabric and has light-heat conversion ability, and can effectively convert light into heat under the same sunlight irradiation, thereby promoting the recovery of the water repellent performance of the fabric; at the same time, Examples 1-3 also have good static water contact angle, hydrostatic pressure resistance, softness, spray resistance before washing and UV resistance (according to the testing standard GB / T 18830-2009, when the UPF value of the fabric is greater than 40 and the UVA transmittance is less than 5%, it can be called an "anti-ultraviolet product", and after the UPF is greater than 50, the impact on the human body can be completely ignored), and the anti-ultraviolet performance of the fabric is derived from the ultraviolet shielding ability of nano titanium dioxide.

[0108] It can be seen from Example 1 (cotton fabric), Example 4 (polyester fabric) and Example 5 (nylon fabric) in the table that the water repellent containing nano titanium dioxide in the chemical structure prepared according to the method provided by the present invention has good spray resistance after washing and natural drying, static water contact angle, hydrostatic pressure resistance, softness, spray resistance before washing and UV resistance for common textile fabrics.

[0109] By comparing Example 1 and Control Example 1, it can be seen that compared with the fabric finished with a commercial fluorine-free water repellent (without titanium dioxide) (Control Example 1), the fabric finished with a water repellent containing nano titanium dioxide in the chemical structure prepared by the method provided by the present invention (Example 1) has better spray resistance, static water contact angle, hydrostatic pressure resistance and UV resistance after natural drying after washing. The main reason is that the water repellent polymer chain prepared by the present invention is chemically linked with nano titanium dioxide, and titanium dioxide can convert solar radiation into heat energy to promote the reorientation of curled non-polar groups during washing. At the same time, titanium dioxide can increase the roughness of the fabric surface, and water droplets have a larger static water contact angle on the surface of the fabric containing it and are easy to roll off.

[0110] By comparing Example 1 and Control Example 2, it can be seen that compared with the fabric finished with the same water-repellent polymer structure but without nano-titanium dioxide product (the amount of modified titanium dioxide exceeds the parameters involved in the method provided by the present invention, the amount is 0, Control Example 2), the fabric finished with the water-repellent containing nano-titanium dioxide in the chemical structure prepared by the method provided by the present invention (Example 1) has good spray resistance, static water contact angle, hydrostatic pressure resistance and UV resistance after natural drying after washing. The main reason is that the water-repellent polymer chain prepared by the present invention is chemically linked to nano-titanium dioxide, and titanium dioxide can convert solar radiation into heat energy to promote the reorientation of curled non-polar groups during washing. At the same time, titanium dioxide can increase the roughness of the fabric surface, and water droplets have a larger static water contact angle on the surface of the fabric containing it and are easy to roll off.

[0111] Comparing Example 1 and Control Example 3, it can be seen that compared with the fabric (Control Example 3) finished with the product obtained by the modified titanium dioxide dosage exceeding the parameters involved in the method of the present invention (excessive dosage), the fabric (Example 1) prepared by the water repellent containing nano titanium dioxide in the chemical structure prepared by the method provided by the present invention has better spray resistance after washing and natural drying, static water contact angle, hydrostatic pressure resistance and softness. The main reason is that the acrylic monomer undergoes free radical polymerization on the surface of the modified titanium dioxide to form a polymer, and the excessive modified titanium dioxide causes the polymer molecular weight to decrease, the polymer size to decrease, and it cannot form an effective coverage of the fabric, which reduces the water repellency of the fabric. At the same time, the excessive modified titanium dioxide deposited on the surface of the fabric is easy to fill the void between the fibers, affecting the mutual movement between the fibers during the stress process of the fabric, which is manifested as a decrease in softness. The anti-ultraviolet performance of Control Column 3 is due to the increase in the titanium dioxide content on the surface of the fabric in Example 1, and titanium dioxide has anti-ultraviolet performance.

[0112] By comparing Example 1 and Control Example 4, it can be seen that the static water contact, hydrostatic pressure resistance, spray resistance before and after washing, and UV resistance of the fabric finished with the water repellent product prepared by directly participating in the polymer reaction without modification of nano-titanium dioxide (Control Example 4) are lower than those of the fabric finished with the water repellent containing nano-titanium dioxide in the chemical structure prepared according to the method provided by the present invention (Example 1). The reason is that the hydroxyl group on the surface of nano-titanium dioxide is ionized in the aqueous phase system to show negative charge, and electrostatic adsorption occurs with the cationic surfactant, causing the surfactant to lose its emulsification of titanium dioxide and acrylate monomers, and the stability of the synthesized product is reduced, and the water repellency of the finished fabric is reduced.

[0113] By comparing Example 1 and Control Example 5, it can be seen that the water repellent properties (static water contact, hydrostatic pressure resistance, spray resistance before and after washing) of the fabric finished with the product obtained by exceeding the parameters involved in the method provided by the present invention (Control Example 5) are lower than those of the fabric finished with the water repellent containing nano titanium dioxide in the chemical structure prepared according to the method provided by the present invention (Example 1).

[0114] Comparative Example 1 and Reference Examples 6-7 show that when the amount of water repellent prepared by the present invention to finish the fabric is too low (reference example 6), the various water repellent properties of the fabric (static water contact, hydrostatic pressure resistance, spray resistance before and after washing) and anti-ultraviolet performance are all low, because the amount of water repellent is too small, and the polymer contained in it is difficult to form an effective coverage on the fabric surface, and the hydrophilic groups of some fabrics are still retained. When the amount of water repellent prepared by the present invention to finish the fabric is too high (reference example 7), although the various water repellent properties of the fabric (static water contact, hydrostatic pressure resistance, spray resistance before and after washing) and anti-ultraviolet performance are all good, its softness (feel) decreases greatly, because the fabric surface has too many water repellent polymers and titanium dioxide particles, and the polymers are cross-linked into thick films and solid particles, filling the gaps between fabric fibers to hinder the mutual movement of fibers when the fabric is stressed.

Claims

1. A method for preparing a water repellent having self-recovering water repellency after washing, It is characterized in that The method comprises: (1) preparing nano titanium dioxide with a titanium source, an organic solvent, a reaction inhibitor and deionized water, modifying the nano titanium dioxide with a modifier, removing the solvent by rotary evaporation and aging to obtain modified nano titanium dioxide; (2) taking a cationic surfactant and a nonionic surfactant, dissolving them in deionized water, and then adding the modified nano-titanium dioxide obtained in step (1) to prepare an emulsion; (3) mixing part of the acrylic ester monomer and part of the emulsion containing modified nano-titanium dioxide obtained in step (2), and emulsifying the mixture with an ultrasonic cell crusher to obtain a pre-emulsion A; (4) mixing the remaining acrylic ester monomer and the remaining emulsion containing modified nano-titanium dioxide, and emulsifying them with an ultrasonic cell crusher to obtain a pre-emulsion B; (5) Under nitrogen protection, the pre-emulsion B and the aqueous solution of the initiator are slowly added to the pre-emulsion A, and after the reaction is kept warm, the material is cooled and discharged to obtain a water-repellent self-recovering water-repellent agent.

2. The preparation method according to claim 1, It is characterized in that In the step (1), the titanium source comprises one or more of tetrabutyl titanate, tetraethyl titanate, and tetraisopropyl titanate; the organic solvent comprises one or more of ethanol, propanol, and isopropanol; the reaction inhibitor comprises one or more of glacial acetic acid, nitric acid, or hydrochloric acid; the modifier comprises one or more of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, and dimethoxymethylvinylsilane; when preparing nano titanium dioxide, the components, by mass percentage, comprise 5-20% of the titanium source, 60-80% of the organic solvent, 5-20% of the reaction inhibitor, and the remainder is water; after the modifier is added, the concentration of the modifier in the solution is 1-20 g / L.

3. The preparation method according to claim 1 or 2, It is characterized in that The preparation method of the modified titanium dioxide is as follows: a titanium source, an organic solvent, a reaction inhibitor and deionized water are mixed, and then stirred at 100-1000 r / min for 1-8 hours at room temperature to obtain nano titanium dioxide, and then a modifier is added, and the mixture is reacted at 20-60° C. for 4-24 hours; the aging time is 12-24 hours.

4. The method according to claim 1, It is characterized in that In the step (2), the cationic surfactant is one or a mixture of octadecyltrimethylammonium chloride and hexadecyltrimethylammonium chloride; the nonionic surfactant is a mixture of one or more polyoxyethylene ether surfactants; the mass ratio of the cationic surfactant to the nonionic surfactant is (0.2-0.8):1; the mass ratio of the total amount of the cationic surfactant and the nonionic surfactant to the total amount of the acrylate monomer is (0.05-0.15):1; the mass ratio of the amount of the modified nano titanium dioxide to the total amount of the acrylate monomer is (0.01-0.1):1; the mass concentration of the modified nano titanium dioxide in the emulsion is 0.15-3%.

5. The method according to claim 1, It is characterized in that The acrylic acid ester monomer in step (3) includes any one or more of methyl acrylate, butyl acrylate, hexyl acrylate, octyl acrylate, decyl acrylate, dodecyl acrylate, tetradecyl acrylate, hexadecyl acrylate, octadecyl acrylate, methyl methacrylate, butyl methacrylate, hexyl methacrylate, octyl methacrylate, decyl methacrylate, dodecyl methacrylate, tetradecyl methacrylate, hexadecyl methacrylate, and octadecyl methacrylate.

6. The method according to claim 1, It is characterized in that The mass of the modified nano titanium dioxide emulsion in step (3) is 50-80% of the mass of the total modified nano titanium dioxide emulsion; the mass of the acrylic ester monomer is 40-60% of the mass of the total acrylic ester monomer; the total mass of the acrylic ester monomer accounts for 15-30% of the total mass of the water repellent.

7. The method according to claim 1, It is characterized in that In the step (5), the initiator comprises one or more of azobisisobutyronitrile, azobisisoheptylnitrile, azobisisobutyramidine hydrochloride, potassium persulfate, ammonium persulfate, and dibenzoyl peroxide; the mass of the initiator accounts for 0.1-1% of the total mass percentage of the acrylate monomer; the reaction temperature is 70-80° C., and the reaction time is 2-4 hours.

8. A water-repellent agent having self-recovering water-repellency after washing prepared by the method according to any one of claims 1 to 7.

9. A method for hydrophobic treatment of fabrics, It is characterized in that The method comprises the following steps: firstly immersing the fabric in the aqueous solution of the water repellent according to claim 8, and then rolling and baking the fabric, wherein the rolling rate is 80-200%, the fabric is pre-baked at 80-110° C. for 3-5 minutes, and the fabric is baked at 120-160° C. for 1-5 minutes, wherein the concentration of the water repellent in the aqueous solution of the water repellent is 40-100 g / L.

10. A hydrophobic fabric, It is characterized in that The fabric comprises the water repellent having self-recovering water repellency after washing as claimed in claim 8, or is prepared by the hydrophobic treatment method as claimed in claim 9.

Citation Information

Patent Citations

  • Method for synthesis of organic-inorganic composite hydrophobic / oleophobic surface treatment agent

    CN102352000A

  • Superhydrophobic surface coating material containing nano titanium dioxide and preparation method thereof

    CN108314949A

  • Polymethyl methacrylate / titanium dioxide nano-composite material and preparation method thereof

    CN111675784A

  • Water-resistant high-elasticity textile fabric and preparation method thereof

    CN111979772A

  • Preparation method and application of cationic fluoride-free acrylate water repellent

    CN116971177A